Preparation method of high-toughness nano TiB2 reinforced aluminum-lithium-based composite material
Prefabricated ingots were prepared by dry-grinding high-energy ball milling method and vacuum arc smelting technology, combining low-vacuum-argon atmosphere and double secondary feeding system, and multi-dimensional indirect ultrasonic assisted melt solidification, the nanoparticles in aluminum-lithium-based composite materials were solved. The oxidation and agglomeration problem has achieved the preparation of nano-TiB2-reinforced aluminum-lithium-based composite materials with high strength and excellent plasticity.
Patent Information
- Application Number
- CN202411571390.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-06
AI Technical Summary
When preparing nanoceramic particles-enhanced aluminum-lithium-based composite materials, the chemical activity of Li elements leads to easy reaction with air during the smelting process, resulting in problems of oxidation and hydrogen absorption, resulting in insufficient strength and plasticity of the material, and in-situ reaction synthesis method The temperature is too high and difficult to control, resulting in agglomeration and multi-aggregation of particles, affecting the performance of the material.
The sub-mm-level TiB2/Al composite particles were prepared by dry-milling high-energy ball milling method, and precast ingots were formed by vacuum arc smelting and electromagnetic stirring. Combined with low vacuum-argon atmosphere and double secondary feeding system, nano-TiB2 particles were quickly added to In the aluminum-lithium alloy melt, multi-dimensional indirect ultrasonic assisted melt solidification technology is used to ensure uniform dispersion of nanoparticles and prevent oxidation.
It effectively suppresses the hydrogen absorption and oxidation problem of aluminum lithium alloy, improves the uniform distribution and mechanical properties of nanoparticles, achieves high strength and excellent plasticity, and solves the problem of difficult temperature control and particle size control in in-situ self-generating method. Improve the overall performance of aluminum-lithium-based composite materials.
Smart Images

Figure CN119061289A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, belonging to the technical field of metallurgy and casting of metal materials. Background Art
[0002] Nano-ceramic particle reinforced aluminum-based composites have broad application prospects due to their many advantages such as high specific strength and specific stiffness, good wear resistance, high thermal conductivity and low thermal expansion coefficient. As a new type of aerospace structural material, aluminum-lithium alloy can greatly improve the structural stability by replacing traditional commercial aluminum alloys due to its advantages such as low density, high specific strength and specific stiffness, and can reduce the weight of structural components by 10%~20% and increase the stiffness by 15%~20%. Therefore, it is of great significance and practical application value to deeply study and prepare nano-ceramic particle reinforced aluminum-lithium based composites with aluminum-lithium alloy as the matrix.
[0003] However, unlike other aluminum alloys, due to the high chemical activity of Li element, it is very easy to react with air during the smelting process of aluminum-lithium alloy, resulting in oxidation, hydrogen absorption and other problems, and these problems will become more obvious as the Li content in the alloy increases. Therefore, this makes the preparation of aluminum-lithium based composite materials extremely difficult, seriously restricting its further promotion and application. The Chinese patent with application publication number CN108998700 A discloses an ultra-lightweight, high-modulus, high-strength cast aluminum-lithium based composite material and its preparation method. In this patent, the Li content of the matrix alloy can be as high as 3.5wt.%, but the prepared T6 state in-situ self-generated TiB2 reinforced aluminum-lithium based composite material has a generally low elongation (elongation of about 2%). At the same time, the Chinese patent with application publication number CN115652149 A discloses a lightweight, high-strength aluminum-lithium based composite material containing TiB2 reinforced phase particles and its preparation method. The extruded rod is obtained by homogenization annealing and hot extrusion process, and then the desired material is obtained by solid solution and aging treatment, but the elongation of the composite material is only about 4%.
[0004] Although ceramic particle reinforced aluminum-lithium based composites can be prepared by in-situ reaction synthesis, unfortunately, the reaction temperature of in-situ TiB2 particle generation is too high (greater than 800ºC), the process is difficult to control, and TiB2 particles are usually submicron-sized, which will cause severe air absorption and oxidation, and the particles are severely agglomerated and mostly gathered at the grain boundaries, resulting in poor strengthening and toughening effects of the prepared composite materials, especially poor plasticity. For the above reasons, it is necessary to provide a preparation method with higher operability, which can effectively inhibit the serious problems of hydrogen absorption and oxidation caused by long-term contact with air of aluminum-lithium alloys while completing the rapid addition of nanoparticles, and ensure that the nanoparticles are evenly distributed in the alloy. Summary of the invention
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: to provide a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, comprising the following steps: S1, preparing a prefabricated ingot of nano-TiB2 / Al composite particles; The nano-TiB2 / Al composite particle prefabricated ingot is firstly prepared by mixing nano-TiB2 particles with micron aluminum powder by dry grinding high-energy ball milling to produce sub-millimeter TiB2 / Al composite particles, and then placing the composite particles in a water-cooled concave copper mold for vacuum arc melting, applying electromagnetic stirring after the composite particles are completely melted, and then cooling the mold to obtain a prefabricated ingot, and preparing sub-millimeter TiB2 / Al composite particles with high TiB2 content by dry grinding high-energy ball milling from nano-TiB2 particles and micron aluminum powder to improve the spontaneous agglomeration characteristics of the original nano-particles, which can play a good pre-dispersion role in the subsequent distribution of TiB2 particles, and at the same time avoid the oxidation and pollution problems caused by the nano-TiB2 particles being exposed to the air, and solve the problem of the particles being blown away by the arc due to the small particle size during the subsequent high vacuum arc melting; S2, placing the raw materials of the aluminum-lithium based composite material in a low vacuum stirring pit type melting furnace for smelting to melt the raw materials to form a melt; S3, after the raw material of the aluminum-lithium-based composite material is completely melted, a feeding system is used to first add pure Li particles and a commercial covering agent dedicated to aluminum-lithium alloy into the molten raw material of the aluminum-lithium-based composite material, and an argon atmosphere is introduced for protection; S4, then using another feeding system to add the prefabricated ingot of nano-TiB2 / Al composite particles to the molten aluminum-lithium-based composite material raw material, stirring the molten aluminum-lithium-based composite material raw material to release the nano-TiB2 particles in the prefabricated ingot into the molten aluminum-lithium-based composite material raw material, stirring to promote the dispersion of nano-particles and melt homogeneity, and obtain an aluminum-lithium alloy melt containing nano-particles; S5. Pour the aluminum-lithium alloy melt containing the nanoparticles into the mold through a liquid leakage device, perform ultrasonic vibration, and evacuate the mold cavity to maintain a preset vacuum degree. After cooling, open the mold to obtain the nanoparticle-reinforced cast aluminum-lithium alloy.
[0006] The TiB2 / Al prefabricated ingot obtained by the present invention can be directly and quickly added to the aluminum-lithium alloy melt, solving the problem that nanoparticles are difficult to add to the aluminum liquid. Under the dual protection of low vacuum-argon atmosphere and flux, combined with short-time mechanical stirring, it can effectively promote the uniform dispersion of nanoparticles while avoiding the problem of serious hydrogen oxidation of the aluminum-lithium alloy melt due to the long mechanical stirring time in the traditional external addition method, and effectively improve the wettability of the reinforcing particles and the aluminum matrix, which is beneficial to improving the mechanical properties of the composite material.
[0007] The present invention optimizes the order of adding raw materials and temperature control during the smelting process, especially for the addition of pure Li particles and TiB2 / Al intermediate alloy ingots, using a double secondary feeding system, one feeding system first adds pure Li particles and a commercial covering agent dedicated to aluminum-lithium alloys, and then uses another feeding system to add a prefabricated ingot of nano-TiB2 / Al composite particles to the molten aluminum-lithium based composite material raw materials, thereby reducing the loss of pure Li and reducing the damage to material properties due to phenomena such as hydrogen absorption and oxidation.
[0008] Compared with the traditional high vacuum or non-vacuum direct cooling solidification method, the multi-dimensional indirect ultrasonic assisted melt solidification technology provided by the present invention can not only greatly reduce the shrinkage and shrinkage defects in the melt, but also effectively refine the organization and improve the component segregation problem, thereby improving the quality and performance of the casting. In addition, compared with the high vacuum melting and casting method, the method of the present invention is more operable and has lower cost, and the quality of the casting is higher than that of the non-vacuum melting and casting method. In addition, the method of the present invention has no special restrictions on the composition of the cast aluminum-lithium alloy, and can even be promoted and applied to the melting and casting of metal materials such as high-quality aluminum-lithium alloys and other aluminum-based composite materials. At the same time, the ultrasonic time in the method of the present invention is as short as 30~120s, and the number and action position of the horn can be selected according to the shape of the casting, which greatly improves production efficiency.
[0009] The present invention introduces nano-TiB2 particles into the aluminum-lithium alloy by liquid addition of prefabricated ingots. Different from the existing in-situ autogenous method for preparing aluminum-lithium-based composite materials, it can avoid problems such as air absorption, severe oxidation, and difficulty in controlling particle size and content caused by excessively high reaction temperatures. In addition, the aluminum-lithium-based composite material prepared by the present invention has both excellent strength and plasticity, and truly realizes the organic combination of the advantages of a lightweight and high-strength aluminum-lithium alloy matrix and high-performance ceramic particles.
[0010] The preparation method of the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material of the present invention is more operable. While completing the rapid addition of nanoparticles, it can effectively inhibit the serious problems of hydrogen absorption and oxidation of aluminum-lithium alloys caused by long-term contact with air, and ensure that the nanoparticles are evenly distributed in the alloy.
[0011] Preferably, in step S1, the particle size of the selected nano-TiB2 particles is 20-100 nm, the nano-TiB2 particles account for 5-40% of the total mass of the composite particles, the ball mill speed is 200-300 rpm, and the particle size of the TiB2 / Al composite particles is 0.1 mm-1 mm.
[0012] Preferably, in step S1, when vacuum arc melting is adopted, the arc current is 16-20A, an electromagnetic stirrer is used for stirring, and the electromagnetic stirring speed is 100-200rpm.
[0013] Preferably, the smelting in step (2) is repeated multiple times to make the TiB2 particles evenly dispersed in the melt.
[0014] Preferably, in step S2, the smelting temperature is 700-750°C, and during the smelting process, the melting furnace is evacuated and argon gas is used for gas washing, and the vacuum degree formed in the melting furnace is less than or equal to 5Pa.
[0015] In step S3, the Li particles are cylinders with a diameter greater than 3 mm. The surface of the Li particle raw material has a layer of protective kerosene, and a suitable amount of commercial aluminum-lithium alloy covering agent can be adhered. Before adding the Li particles, the melt temperature is reduced to 660-680°C to avoid serious overburning and hydrogen absorption oxidation of the Li element due to excessive temperature, and then the temperature is raised to 700-720°C.
[0016] In step S4, the content of nano-TiB2 particles in the aluminum-lithium alloy melt after the precast ingot is added is 0~5wt.%, the stirring speed is 0~500rpm, the stirring time is 5~10min, the stirring temperature is 700~720℃, and the stirring head of the electromagnetic stirrer is placed 10mm above the bottom of the crucible to avoid obvious fluctuations on the surface of the aluminum liquid and damage the protective layer of the covering agent, thereby promoting uniform dispersion of the nano-particles and effectively improving the problem of hydrogen absorption and oxidation.
[0017] In step S5, the pouring temperature of the aluminum-lithium alloy melt containing nanoparticles is 670-690°C, the ultrasonic power of the ultrasonic vibration is 0-8.4 kW, the ultrasonic time is 30-120s, the cavity of the mold includes but is not limited to round ingots, square ingots and other specific shapes, and the vacuum degree is less than or equal to 5Pa.
[0018] The beneficial effects of the present invention are: (1) The present invention adopts high-energy ball milling to prepare TiB2 / Al composite particles with a high mass fraction of sub-millimeter level or above, which not only improves the spontaneous agglomeration characteristics of the original nanoparticles, avoids the oxidation and pollution problems caused by the nano TiB2 particles exposed to the air, but also solves the problem of the particles being blown away by the arc due to their small particle size during subsequent high vacuum arc melting; (2) The present invention adopts high vacuum arc melting to melt the sub-millimeter TiB2 / Al composite particles produced by high-energy ball milling into a prefabricated ingot, and applies electromagnetic stirring during the melting process to promote the uniform distribution of nano-TiB2 particles in the prefabricated ingot, which plays a good pre-dispersion role in the subsequent distribution of TiB2 particles in the aluminum-lithium based composite material; (3) The TiB2 / Al precast ingot obtained by the present invention can be directly and quickly added to the aluminum-lithium alloy melt, solving the problem that nanoparticles are difficult to add to the aluminum liquid, especially the addition of particles to the aluminum-lithium alloy liquid is more difficult. Under the dual protection of low vacuum-argon atmosphere and flux, combined with short-time mechanical stirring, it can effectively promote the uniform dispersion of nanoparticles while avoiding the problem of serious hydrogen oxidation in the aluminum-lithium alloy melt caused by the long mechanical stirring time in the traditional external addition method, and effectively improve the wettability of the reinforcing particles and the aluminum matrix, which is beneficial to improving the mechanical properties of the composite material; (4) The present invention optimizes the order of adding raw materials and temperature control during the smelting process, especially for the addition of pure Li particles and TiB2 / Al master alloy ingots, using a secondary feeding system to add materials, thereby reducing the loss of pure Li and reducing the damage to material properties caused by hydrogen absorption and oxidation; (5) Compared with the traditional high vacuum or non-vacuum direct cooling solidification method, the multi-dimensional indirect ultrasonic assisted melt solidification technology provided by the present invention can not only significantly reduce shrinkage defects in the melt, but also effectively refine the structure and improve the problem of component segregation, thereby improving the quality and performance of the casting. In addition, compared with the high vacuum melting and casting method, the new method is more operable and has lower cost, while the quality of castings is higher than that of non-vacuum melting and casting methods. Moreover, the new method has no special restrictions on the composition of cast aluminum-lithium alloys, and can even be promoted and applied to the melting and casting of high-quality aluminum-lithium alloys, other aluminum-based composite materials and other metal materials. At the same time, the ultrasonic time in the new method is as short as 30~120s, and the number and action position of the amplitude rod can be selected according to the shape of the casting, which greatly improves production efficiency; (6) The present invention introduces nano-TiB2 particles into the aluminum-lithium alloy by liquid external addition, which is different from the existing in-situ self-generation method for preparing aluminum-lithium based composite materials. It can avoid problems such as gas absorption and severe oxidation caused by excessive reaction temperature and difficulty in controlling particle size and content. In addition, the aluminum-lithium based composite material prepared by the present invention has both excellent strength and plasticity, and truly realizes the organic combination of the advantages of lightweight and high-strength aluminum-lithium alloy matrix and high-performance ceramic particles. (7) The present invention utilizes dry high-energy ball milling to mix nano-TiB2 particles with micron aluminum powder to produce sub-millimeter TiB2 / Al composite particles, and then produces a prefabricated ingot of the TiB2 / Al composite particles. Compared with a structure such as a thin strip, more TiB2 particles can be added to the prefabricated ingot, so that more nano-TiB2 particles in the prefabricated ingot can be released into the molten aluminum-lithium-based composite material raw material, so that the TiB2 particle content in the aluminum-lithium-based composite material raw material is higher, thereby improving the performance of the composite material; (8) The present invention pours the aluminum-lithium alloy melt containing nanoparticles into a mold through a leakage device, performs ultrasonic vibration, and evacuates the mold cavity to maintain a preset vacuum degree. After cooling, the mold is opened to obtain the nanoparticle-reinforced cast aluminum-lithium alloy. The aluminum-lithium alloy melt is directly leaked and molded without pressurizing it. Large-scale die-casting equipment is not required, the processing technology is simpler, the processing cost is lower, and the performance of the obtained composite material can still be comparable to that of the composite material obtained by pressure molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which: Figure 1 It is a process flow chart of the preparation method of the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material of the present invention; Figure 2 It is a microscopic characterization diagram of a sample in an embodiment of a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material of the present invention. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] A method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material comprises the following steps: Example 1: Reference Figure 1 The casting in this embodiment is a square ingot, and the alloy composition of the ingot is as follows: 2.5% Li, 1.5% Cu, 0.2% Sc, 0.5% TiB2, and the balance is Al. The content of nanoparticles in the nano-TiB2 / Al prefabricated ingot is 10wt.%.
[0022] The present invention provides a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, and the specific manufacturing method is: S101: TiB2 particles with an average particle size of 100 nm and pure aluminum powder with an average particle size of 50 μm were weighed according to a ratio of 10% TiB2 particle mass content, and mixed evenly in a ball mill at a rotation speed of 200 rpm to form submillimeter TiB2 / Al composite particles. The composite particles were melted into multiple prefabricated ingots with a diameter of 10 mm in a high vacuum arc melting furnace, the arc current was 16 A, and the electromagnetic stirring speed was 100 rpm; S102: placing other alloy raw materials except pure Li particles and TiB2 / Al prefabricated ingots in a low vacuum stirring pit melting furnace for smelting at a smelting temperature of 700-750°C, evacuating the furnace in time during the smelting process and using argon gas for washing, and the vacuum degree in the furnace is less than or equal to 5Pa; S103: After the alloy raw materials are completely melted, pure Li particles with an appropriate amount of commercial covering agent for aluminum-lithium alloy on the surface are added by one of the dual secondary feeding systems. Before adding the Li particles, the melt temperature is reduced to 660-680°C to prevent the Li element from being severely overburned and absorbing hydrogen oxidation due to excessive temperature. Then the temperature is raised to 700-720°C; S104: adding TiB2 / Al precast ingot by another secondary feeding system, and then applying mechanical stirring (electromagnetic stirring) to the melt to accelerate the release of nano-TiB2 particles in the precast ingot, and promote the dispersion of nano-particles and the homogeneity of the melt, to obtain an aluminum-lithium alloy composite melt containing nano-particles, the stirring temperature is 700° C., the stirring speed is 300 rpm, and the stirring time is 5 min; S105: The TiB2 / Al-2.5Li-1.5Cu composite melt is quickly poured into the mold through a liquid leakage device, and ultrasonic vibration is turned on to assist the melt solidification. Multiple sets of indirect ultrasonic amplitude rods in the ultrasonic vibration device act on the outer wall of the mold to form a multi-dimensional ultrasonic component, and the ultrasonic effect is better. The melt pouring temperature is 670-690°C, the indirect ultrasonic power is 2.8kW, and the ultrasonic time is 60s. The vacuum degree of the mold cavity during the entire pouring process is less than or equal to 5Pa. After cooling, the mold is opened to obtain a square casting of nanoparticle-reinforced aluminum-lithium based composite materials. The microstructure of the casting sample is shown in FIG. Figure 2 As shown; Embodiment 2: The casting in this embodiment is a round ingot, and the alloy composition of the ingot is as follows by mass percentage: 0.6% Li, 4.5% Cu, 5% TiB2, and the balance is Al. The content of nanoparticles in the nano-TiB2 / Al prefabricated ingot is 40wt.%.
[0023] like Figure 1 As shown, the present invention provides a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, and the specific manufacturing method is: S101: TiB2 particles with an average particle size of 100 nm and pure aluminum powder with an average particle size of 50 μm were weighed according to a ratio of 20% TiB2 particle mass content, and mixed evenly in a ball mill at a rotation speed of 300 rpm to form submillimeter TiB2 / Al composite particles. The composite particles were melted into multiple prefabricated ingots with a diameter of 10 mm in a high vacuum arc melting furnace, the arc current was 20 A, and the electromagnetic stirring speed was 200 rpm; S102: placing the raw materials other than pure Li particles and TiB2 / Al prefabricated ingots in a low vacuum stirring pit melting furnace for melting at a melting temperature of 700-750°C, evacuating the furnace in time during the melting process and using argon gas for washing, and the vacuum degree in the furnace is less than or equal to 5Pa; S103: After the alloy raw materials are completely melted, pure Li particles with an appropriate amount of commercial covering agent for aluminum-lithium alloy on the surface are added by one of the dual secondary feeding systems. Before adding the Li particles, the melt temperature is reduced to 660-680°C to prevent the Li element from being severely overburned and absorbing hydrogen oxidation due to excessive temperature. Then the temperature is raised to 700-720°C; S104: adding the TiB2 / Al precast ingot by another secondary feeding system, and then applying mechanical stirring (electromagnetic stirring) to the melt to accelerate the release of nano-TiB2 particles in the precast ingot into the melt, and promote the dispersion of nano-particles and the homogeneity of the melt, to obtain an aluminum-lithium alloy composite melt containing nano-particles, the stirring temperature is 700° C., the stirring speed is 500 rpm, and the stirring time is 10 min; S105: The TiB2 / Al-0.3Li-4.5Cu composite melt is quickly poured into the mold through a liquid leakage device, and ultrasonic vibration is turned on to assist the melt solidification. Multiple sets of indirect ultrasonic amplitude rods in the ultrasonic vibration device act on the outer wall of the mold to form a multi-dimensional ultrasonic component with better ultrasonic effect. The melt pouring temperature is 670~690℃, the indirect ultrasonic power is 8.4kW, and the ultrasonic time is 120s. During the whole process, the vacuum degree of the mold cavity is less than or equal to 5Pa. After cooling, the mold is opened to obtain a circular casting of nanoparticle reinforced aluminum-lithium based composite materials.
[0024] Example 3: The casting in this example is a Z-shaped ingot, and the ingot alloy composition is as follows by mass percentage: 2% Li, 2% Cu, 0.5% Mg, 0.2% Zr, 0.15% Ag, 1% TiB2, and the balance is Al. The content of nanoparticles in the nano-TiB2 / Al prefabricated ingot is 20wt.%.
[0025] The present invention provides a method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, and the specific manufacturing method is: S101: TiB2 particles with an average particle size of 100 nm and pure aluminum powder with an average particle size of 50 μm were weighed according to a ratio of 20% TiB2 particle content, and mixed evenly in a ball mill at a rotation speed of 250 rpm to form submillimeter TiB2 / Al composite particles. The composite particles were melted into multiple prefabricated ingots with a diameter of 10 mm in a high vacuum arc melting furnace, the arc current was 18 A, and the electromagnetic stirring speed was 150 rpm; S102: placing the raw materials other than pure Li particles and TiB2 / Al prefabricated ingots in a low vacuum stirring pit melting furnace for melting at a melting temperature of 700-750°C, evacuating the furnace in time during the melting process and using argon gas for washing, and the vacuum degree in the furnace is less than or equal to 5Pa; S103: After the alloy raw materials are completely melted, pure Li particles with an appropriate amount of commercial covering agent for aluminum-lithium alloy on the surface are added by one of the dual secondary feeding systems. Before adding the Li particles, the melt temperature is reduced to 660-680°C to prevent the Li element from being severely overburned and absorbing hydrogen oxidation due to excessive temperature. Then the temperature is raised to 700-720°C; S104: adding TiB2 / Al precast ingot by another secondary feeding system, and then applying mechanical stirring (electromagnetic stirring) to the melt to accelerate the release of nano-TiB2 particles in the precast ingot, and promote the dispersion of nano-particles and the homogeneity of the melt, to obtain an aluminum-lithium alloy melt containing nano-particles, the stirring temperature is 700° C., the stirring speed is 400 rpm, and the stirring time is 8 min; S105: The TiB2 / Al-2Li-2Cu composite melt is quickly poured into the mold through a liquid leakage device, and ultrasonic vibration is turned on to assist the melt solidification. Multiple sets of indirect ultrasonic amplitude transformers in the ultrasonic vibration device act on the outer wall of the mold to form a multi-dimensional ultrasonic component with better ultrasonic effect. The melt pouring temperature is 670-690°C, the indirect ultrasonic power is 5.6kW, and the ultrasonic time is 90s. The vacuum degree of the mold cavity during the entire pouring process is less than or equal to 5Pa. After cooling, the mold is opened to obtain a Z-shaped casting of nanoparticle-reinforced aluminum-lithium based composite materials.
[0026] Table 1 shows the composition of the cast aluminum-lithium alloy materials prepared in different embodiments and the test results of the tensile mechanical properties (tensile strength, yield strength and elongation) of the cast aluminum-lithium alloy materials. The results show that the nanoparticle-containing cast aluminum-lithium alloy provided by the present invention has high strength and good toughness, and its cast comprehensive mechanical properties are higher than those of the existing particle-reinforced cast aluminum-lithium alloy composite materials, especially the elongation.
[0027] Table 1:
[0028] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material, using a die-casting machine to die-cast the aluminum alloy material poured in a mold, characterized in that: The steps include: S1, preparing a prefabricated ingot of nano-TiB2 / Al composite particles; The nano-TiB2 / Al composite particle prefabricated ingot is prepared by first mixing nano-TiB2 particles with micron aluminum powder using a dry high-energy ball milling method to produce sub-millimeter TiB2 / Al composite particles, and then placing the composite particles in a water-cooled concave copper mold for vacuum arc melting, applying electromagnetic stirring after the composite particles are completely melted, and then cooling the mold to obtain a prefabricated ingot; S2, placing the raw materials of the aluminum-lithium based composite material in a low vacuum stirring pit type melting furnace for smelting to melt the raw materials to form a melt; S3, after the raw material of the aluminum-lithium-based composite material is completely melted, firstly adding pure Li particles and a commercial covering agent dedicated to aluminum-lithium alloy into the melted raw material of the aluminum-lithium-based composite material; S4, then adding a prefabricated ingot of nano-TiB2 / Al composite particles to the molten aluminum-lithium-based composite material raw material, stirring the molten aluminum-lithium-based composite material raw material to release the nano-TiB2 particles in the prefabricated ingot into the molten aluminum-lithium-based composite material raw material, to obtain an aluminum-lithium alloy melt containing nano-particles; S5. Pour the aluminum-lithium alloy melt containing the nanoparticles into the mold through a liquid leakage device, perform ultrasonic vibration, and evacuate the mold cavity to maintain a preset vacuum degree. After cooling, open the mold to obtain the nanoparticle-reinforced cast aluminum-lithium alloy.
2. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 1, characterized in that: In step S1, the particle size of the selected nano-TiB2 particles is 20-100 nm, the nano-TiB2 particles account for 5-40% of the total mass of the composite particles, the ball mill speed is 200-300 rpm, and the particle size of the TiB2 / Al composite particles is 0.1 mm-1 mm.
3. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 2, characterized in that: In step S1, when vacuum arc melting is adopted, the arc current is 16-20A, and an electromagnetic stirrer is used for stirring, and the electromagnetic stirring speed is 100-200rpm.
4. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 3, characterized in that: The smelting in step (2) is repeated multiple times to make the TiB2 particles evenly dispersed in the melt.
5. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 4, characterized in that: In step S2, the smelting temperature is 700-750°C. During the smelting process, the melting furnace is evacuated and argon gas is used for washing. The vacuum degree formed in the melting furnace is less than or equal to 5Pa.
6. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 5, characterized in that: In step S3, the Li particles are cylinders with a diameter greater than 3 mm, and a layer of protective kerosene is provided on the surface of the Li particle raw material. Before adding the Li particles, the melt temperature is reduced to 660-680°C, and then the temperature is increased to 700-720°C.
7. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 6, characterized in that: In step S4, the content of nano-TiB2 particles in the aluminum-lithium alloy melt after the precast ingot is added is 0~5wt.%, the stirring speed is 0~500rpm, the stirring time is 5~10min, the stirring temperature is 700~720℃, and the stirring head of the electromagnetic stirrer is placed 10mm above the bottom of the crucible.
8. The method for preparing the high-strength and tough nano-TiB2 reinforced aluminum-lithium based composite material according to claim 7, characterized in that: In step S5, the pouring temperature of the aluminum-lithium alloy melt containing nanoparticles is 670-690° C., the ultrasonic power of the ultrasonic vibration is 0-8.4 kW, the ultrasonic time is 30-120 s, and the vacuum degree is less than or equal to 5 Pa.
Citation Information
Patent Citations
High-dispersive-distribution nano-titanium diboride particle reinforced aluminum matrix composite material and preparation method thereof
CN110257655A
Preparation method of micro-nanometer TiB2 particle reinforced magnesium-lithium-based composite material
CN111304506A
Preparation method of additional nano-particle reinforced cast aluminum-lithium alloy
CN114672686A
Lightweight high-strength TiB2-reinforced-phase-particle-containing aluminum-lithium-based composite material and preparation method thereof
CN115652149A
Cited By
High-dispersion TiB2 / A356 composite material and preparation method thereof
CN121046678A
Heat treatment method for high-performance ultralight cast aluminum alloy
CN122406130A