High-performance cast aluminum alloy and preparation method and application thereof
By adding specific elements and process to the aluminum alloy, the θ-Al2Cu and Mn6Cu4Al29 phases are formed, which solves the problem of insufficient refining eutectic silicon effect of existing aluminum alloys, significantly improves the tensile strength and yield strength, and is suitable for automotive zero Lightweight material for parts.
Patent Information
- Application Number
- CN202411201263.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
The existing high-performance low-carbon aluminum alloys have insufficient effect in refining eutectic silicon, which affects the improvement of alloy performance, and the grains are coarse during the heat treatment aging process, affecting the mechanical properties.
The use includes 4.2 to 9.3% Si, 3.0 to 5.2% Cu, 0.1 to 0.6% Mg, 0.3 to 1.2% Mn, 0.03 to 0.3% V, 0.08 to 0.15% Ti, 0.01 to 0.05% Mo, 0.01 to 0.03% Sr, is used. The aluminum alloy with 0.05-0.15% RE and Fe≤0.7% is formed by a specific melting, degassing, solid solution and aging treatment process to form the θ-Al2Cu and Mn6Cu4Al29 phases, thereby improving the tensile strength and yield strength of the alloy.
It significantly improves the tensile strength, yield strength and elongation of aluminum alloy, enhances the thermal physical properties and flow properties, and is suitable for lightweight materials of automotive parts.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloys, and in particular relates to a high-performance cast aluminum alloy and a preparation method and application thereof. Background Art
[0002] In the fields of aviation, aerospace, and automobiles, reducing weight to save materials and reduce carbon emissions is a long-term goal pursued by people and one of the development trends of modern advanced manufacturing technology. Lightweighting can be achieved by using light metals or by using higher strength materials. High-strength and tough aluminum alloys combine these two directions of lightweight development. With the rapid development of aerospace and new energy vehicle fields, the demand for high-performance cast aluminum alloy products is also increasing. High-performance cast aluminum alloys have received widespread attention due to their excellent comprehensive mechanical properties. The use of this type of alloy is of great significance for reducing the weight of the entire machine, improving the performance of the entire machine, and saving raw materials and energy. For example, the aluminum alloy scroll disk of the automobile air-conditioning compressor replaces the forged scroll disk product.
[0003] Commonly used cast aluminum alloys in the field of industrial applications include Al-Si binary alloy system, Al-Mg alloy system, Al-Si-Mg alloy system, Al-Si-Cu alloy system, etc. Cast aluminum alloys have good plasticity and toughness, and have a high heat treatment effect. Most of them are formed by gravity casting, pressure casting, squeeze casting and other special casting methods. They have high production efficiency, low manufacturing cost and can be mass-produced.
[0004] CN114231800B discloses a high-performance low-carbon aluminum alloy and a preparation method thereof, which relies on trace amounts of Ti and La elements to refine eutectic silicon. The eutectic silicon is relatively coarse and the refinement effect is insufficient, which affects the improvement of alloy performance. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a high-performance cast aluminum alloy and a preparation method and application thereof, wherein the alloy has high tensile strength, yield strength and elongation.
[0006] The present invention provides a high-performance cast aluminum alloy, which comprises the following components by mass fraction:
[0007] 4.2-9.3% Si, 3.0-5.2% Cu, 0.1-0.6% Mg, 0.3-1.2% Mn, 0.03-0.3% V, 0.08-0.15% Ti, 0.01-0.05% Mo, 0.01-0.03% Sr, 0.05-0.15% RE, Fe≤0.7% and the balance aluminum;
[0008] Among them, Mn (wt%) = 1.22Fe (wt%) + 0.25.
[0009] Preferably, the main strengthening phases of the high performance cast aluminum alloy are θ-Al2Cu phase and Mn6Cu4Al 29 Mutually.
[0010] Preferably, the RE rare earth elements are Ce and La.
[0011] The present invention provides a method for preparing the high-performance cast aluminum alloy described in the above technical solution, comprising the following steps:
[0012] a) melting crystalline silicon, pure aluminum ingot, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, rare earth, cathode copper and aluminum-titanium master alloy to obtain an aluminum melt;
[0013] b) mixing the aluminum melt and a refining agent, and degassing;
[0014] c) continuing to add pure magnesium ingots and aluminum-strontium master alloys, and continuously degassing to obtain aluminum liquid;
[0015] d) pouring the molten aluminum, and performing solid solution strengthening and aging treatment after demoulding to obtain a cast aluminum alloy.
[0016] 5. The preparation method according to claim 4, characterized in that the melting comprises:
[0017] After loading, keep the temperature at 550-600°C for 60-80 minutes, then increase the temperature to 780-810°C and keep it for 1-2 hours.
[0018] Preferably, the aluminum melt is mixed with a refining agent at 740-780°C;
[0019] The degassing conditions include: rotor speed of 425-482 rpm, compressed air flow rate of 0.6-0.8 m 3 / h, the degassing time is 120~160s.
[0020] Preferably, step c) comprises:
[0021] The conditions for continuous degassing after adding pure magnesium ingot include: rotor speed of 370-415 rpm, compressed air flow rate of 0.4-0.6 m 3 / h, continue degassing for 180-260s, keep warm for 0.5-1h;
[0022] Cool down to 720-740℃, add aluminum-strontium master alloy, continue degassing for 180-260s, rotor speed is 515-550rpm, compressed air flow rate is 0.8-1.2m 3 / h.
[0023] Preferably, the pouring temperature is 700-750°C.
[0024] Preferably, the solution treatment includes primary solution treatment and secondary solution treatment;
[0025] The temperature of the first-stage solution treatment is 465±10°C, and the holding time is 1 to 2 hours;
[0026] The temperature of the secondary solution treatment is 505±10°C, and the holding time is 6 to 8 hours;
[0027] The temperature of the aging strengthening is 170±10° C., and the insulation time is 7 to 9 hours.
[0028] The present invention provides an application of the high-performance cast aluminum alloy described in the above technical solution or the high-performance cast aluminum alloy prepared by the preparation method described in the above technical solution in lightweight materials for automobile parts.
[0029] The present invention provides a high-performance cast aluminum alloy, which includes the following components by mass fraction: 4.2-9.3% Si, 3.0-5.2% Cu, 0.1-0.6% Mg, 0.3-1.2% Mn, 0.03-0.3% V, 0.08-0.15% Ti, 0.01-0.05% Mo, 0.01-0.03% Sr, 0.05-0.15% RE, Fe≤0.7% and the balance aluminum; Mn (wt%) = 1.22Fe (wt%) + 0.25. The alloy contains Si, Cu, Mn and rare earth elements, and the alloy structure is mainly composed of α-(Al) + θ-Al2Cu + Mn6Cu4Al 29 phase + eutectic silicon, etc., with a large number of dispersed θ-Al2Cu phases and Mn6Cu4Al 29 The phase distorts the crystal lattice of the α-(Al) solid solution and closes the slip planes between grains, which plays a role in solid solution strengthening and dispersion hardening, thereby improving the elongation, tensile strength and yield strength of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the metallographic structure diagram of the aluminum alloy 100× prepared in Example 1 of the present invention;
[0031] Figure 2 The metallographic structure diagram of the aluminum alloy 200× prepared in Example 1 of the present invention (etched);
[0032] Figure 3 This is a 200× microstructure diagram of the aluminum alloy prepared in Example 1 of the present invention;
[0033] Figure 4 This is a 3000× microstructure diagram of the aluminum alloy prepared in Example 1 of the present invention; DETAILED DESCRIPTION
[0034] The present invention provides a high-performance cast aluminum alloy, which comprises the following components by mass fraction:
[0035] 4.2-9.3% Si, 3.0-5.2% Cu, 0.1-0.6% Mg, 0.3-1.2% Mn, 0.03-0.3% V, 0.08-0.15% Ti, 0.01-0.05% Mo, 0.01-0.03% Sr, 0.05-0.15% RE, Fe≤0.7% and the balance aluminum;
[0036] Among them, Mn (wt%) = 1.22Fe (wt%) + 0.25.
[0037] The aluminum alloy provided by the present invention includes 4.2% to 9.3% Si by mass fraction, and the specific content includes 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, 6.1%, 6.2%, 6.3%, 6.4 %, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7.0%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, 8.0%, 8.1%, 8.2%, 8.3%, 8.4%, 8.5%, 8.6%, 8.7%, 8.8%, 8.9%, 9.0%, 9.1%, 9.2%, or 9.3%. In the present invention, the Si element mainly plays the role of modifying the eutectic Si phase to improve the mechanical properties and toughness of the alloy.
[0038] The aluminum alloy provided by the present invention includes 3.0-5.2% Cu by mass fraction; the specific content includes 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 6.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, or 5.2%. In the present invention, Cu is an extremely important main alloying element in the aluminum alloy; the addition of copper in the present invention will make it solid-dissolve in the aluminum matrix in the alloy or form a granular compound strengthening phase θ-Al2Cu phase. According to the binary eutectic temperature (548°C) of the aluminum-copper alloy, it is about 5.65%, and the Al-Cu-Si ternary system alloy, the addition of Si content greatly reduces the solid solution temperature of the alloy.
[0039] The strengthening effect of Cu added to the aluminum alloy provided by the present invention is based on the interaction between V and Cu. The addition of V element leads to the formation of Al3V phase, which not only promotes the formation of fine equiaxed crystal cast structure, but also inhibits the coarse growth of θ-Al2Cu grains during heat treatment aging, thereby improving the mechanical properties.
[0040] The aluminum alloy provided by the present invention includes 0.1-0.6% Mg by mass fraction; the specific content includes 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, or 0.6%.
[0041] The aluminum alloy provided by the present invention includes 0.3-1.2% Mn by mass fraction, preferably 0.8-1.2%; the specific content includes 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, or 1.2%. The Mn element is added as the main element in the alloy of the present invention, and manganese and copper form Mn6Cu4Al 29 phase, has high thermal stability, while manganese dissolved in α-(Al) can reduce the atomic diffusion rate, reduce the aging process, improve heat resistance, strengthen the alloy matrix and grain boundaries, and limit the growth of θ-Al2Cu phase grains during solution treatment, improving corrosion resistance; when w(Mn) in the alloy is greater than 0.8%, insoluble primary phase Mn6Cu4Al is likely to appear in the organization 29 phase, which plays a reinforcing role in the second phase.
[0042] The aluminum alloy provided by the present invention includes 0.03-0.3% V by mass fraction; the specific content includes 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.017%, 0.018%, 0.019%, 0.2%, 0.21%, 0.22%, 0.23.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, or 0.3%. The addition of V element leads to the formation of Al3V phase, which not only promotes the formation of fine equiaxed crystal cast structure, but also inhibits the coarse growth of θ-Al2Cu grains during heat treatment aging, thereby improving mechanical properties.
[0043] The aluminum alloy provided by the present invention includes 0.08-0.15% Ti by mass fraction; the specific content includes 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15%. The Ti element in the present invention can refine the alloy structure, improve the mechanical properties, and also reduce the tendency of hot cracking and the tendency of pinhole formation.
[0044] The aluminum alloy provided by the present invention includes 0.01-0.05% Mo by mass fraction; the specific content includes 0.01%, 0.02%, 0.03%, 0.04% or 0.05%. In the present invention, Mo forms fine Al(Fe, Mo)Si compounds in the Al matrix, which are mainly located in the dendrite region, significantly reducing the harmful effects of iron, improving heat resistance and reducing the tendency to form pinholes, and improving density. Mo plays an aging strengthening role, accelerates artificial aging, that is, accelerates the formation of θ-Al2Cu, and improves tensile strength and yield strength.
[0045] The aluminum alloy provided by the present invention includes 0.01-0.03% Sr by mass fraction, and the specific content includes 0.01%, 0.015%, 0.02%, 0.025%, or 0.03%. The Sr mainly plays the role of modifying the eutectic Si phase to improve the mechanical properties and toughness of the alloy.
[0046] The aluminum alloy provided by the present invention includes 0.05-0.15% rare earth elements by mass fraction; the specific content includes 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, or 0.15%. The rare earth elements in the present invention preferably include Ce and La; in a specific embodiment, the rare earth elements are provided by cerium-rich rare earth materials, wherein Ce≥55wt% and La≥25wt%. The rare earth elements play a role in modifying the eutectic Si phase, making the needle-like eutectic Si into fibrous, pinning dislocations at the grain boundaries, hindering grain boundary sliding, and improving high-temperature strength. Rare earth can also react with impurity elements in the melt to form stable compounds, which are precipitated at the bottom of the melt to purify the melt.
[0047] The aluminum alloy provided by the present invention includes Fe≤0.7% by mass, and the specific content is 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, or 0.1%. The contents of Mn and Fe in the present invention satisfy the relationship: Mn (wt%) = 1.22Fe (wt%) + 0.25.
[0048] The aluminum alloy provided by the present invention includes the remainder aluminum by mass fraction. In a specific embodiment, industrial high-purity aluminum Al99.70 or Al99.60 is used.
[0049] The main strengthening phases of the high performance cast aluminum alloy provided by the present invention are θ-Al2Cu phase and Mn6Cu4Al 29 Phase, these two phases can distort the crystal lattice of α-(Al) solid solution and close the slip plane between grains, play the role of solid solution strengthening and dispersion hardening, improve the tensile strength and yield strength of the alloy, and have excellent elongation. At the same time, the aluminum alloy also has good thermal physical properties and flow properties.
[0050] In a specific embodiment of the present invention, the high performance cast aluminum alloy comprises the following components by mass fraction:
[0051] 4% Si, 0.5% Mg, 4.5% Cu, 0.13% Ti, 0.13% RE, 1.104% Mn, 0.25% V, 0.05% Mo, 0.015% Sr, 0.7% Fe and balance Al;
[0052] or 6.5% Si, 0.3% Mg, 5.1% Cu, 0.13% Ti, 0.13% RE, 0.494% Mn, 0.25% V, 0.05% Mo, 0.015% Sr, 0.2% Fe and the balance Al;
[0053] or 9% Si, 0.1% Mg, 3.2% Cu, 0.08% Ti, 0.05% RE, 0.86% Mn, 0.15% V, 0.03% Mo, 0.011% Sr, 0.5% Fe and the balance Al;
[0054] or 8% Si, 0.2% Mg, 3.6% Cu, 0.15% Ti, 0.15% RE, 0.616% Mn, 0.3% V, 0.02% Mo, 0.018% Sr, 0.3% Fe and the balance Al;
[0055] or 5% Si, 0.4% Mg, 4.2% Cu, 0.09% Ti, 0.1% RE, 0.372% Mn, 0.2% V, 0.04% Mo, 0.023% Sr, 0.1% Fe and the balance Al;
[0056] Or 7% Si, 0.6% Mg, 4.8% Cu, 0.12% Ti, 0.09% RE, 0.982% Mn, 0.1% V, 0.02% Mo, 0.017% Sr, 0.6% Fe and the balance Al.
[0057] The present invention provides a method for preparing the high-performance cast aluminum alloy described in the above technical solution, comprising the following steps:
[0058] a) melting crystalline silicon, pure aluminum ingot, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, rare earth, cathode copper and aluminum-titanium master alloy to obtain an aluminum melt;
[0059] b) mixing the aluminum melt and a refining agent, and degassing;
[0060] c) continuing to add pure magnesium ingots and aluminum-strontium master alloys, and continuously degassing to obtain aluminum liquid;
[0061] d) pouring the molten aluminum, and performing solid solution strengthening and aging treatment after demoulding to obtain a cast aluminum alloy.
[0062] The present invention melts crystalline silicon, pure aluminum ingot, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metal manganese, rare earth, cathode copper and aluminum-titanium master alloy to obtain aluminum melt. The charging order of the present invention in preparing the pre-melt is preferably crystalline silicon→pure aluminum ingot→aluminum-molybdenum master alloy→aluminum-vanadium master alloy→aluminum-titanium master alloy→cerium-rich rare earth→metal manganese→cathode copper; the present invention tries to make each added material compact without leaving obvious gaps.
[0063] The melting in the present invention comprises:
[0064] After loading, keep the temperature at 550-600°C for 60-80 minutes, then increase the temperature to 780-810°C and keep it for 1-2 hours.
[0065] After obtaining the aluminum melt, the present invention mixes the aluminum melt with a refining agent and degasses. The present invention cools the aluminum melt to 740-780°C and then mixes it with a refining agent, starts the degasser, and the rotor and baffle automatically sink to automatically enter the rotary degassing stage. The degassing conditions include: the rotor speed is 425-482rpm, the compressed air flow rate is 0.6-0.8m 3 / h, the degassing time is 120~160s.
[0066] Pure magnesium ingots and aluminum-strontium master alloys are continuously added, and degassing is continued to obtain aluminum liquid. Specifically, pure magnesium ingots are continuously added and degassing is continued. The conditions for continuous degassing include: a rotor speed of 370 to 415 rpm, a compressed air flow rate of 0.4 to 0.6 m 3 / h, continue degassing for 180-260s, and keep warm for 0.5-1h; after degassing, the rotor rises, and the rotor vents are immediately cleared with a tool, and the slag on the liquid surface is turned over with a slag spoon, and then the slag on the surface of the aluminum liquid is cleaned, and the heat is kept for 0.5-1h.
[0067] Cool down to 720-740℃, add aluminum-strontium master alloy, continue degassing for 180-260s, rotor speed is 515-550rpm, compressed air flow rate is 0.8-1.2m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0068] The present invention places the sample mold on a mold frame and pours the molten aluminum; the pouring temperature is controlled at 700-750° C. The aluminum liquid is poured into the sample mold by a hand-held ladle, and the pouring is slow and continuous. After the sample mold is completely solidified, the sample mold is turned over by a clamp to demould the sample, and attention is paid to turning over the sample mold steadily and not touching or scratching the surface of the sample blank, and the surface should be smooth and flat.
[0069] After demoulding, solid solution strengthening and aging treatment are carried out to obtain a cast aluminum alloy.
[0070] The solution treatment described in the present invention includes primary solution treatment and secondary solution treatment;
[0071] The temperature of the first-stage solution treatment is 465±10°C, and the holding time is 1 to 2 hours;
[0072] The temperature of the secondary solution treatment is 505±10°C, and the holding time is 6-8h; the cooling medium is water, and the temperature of the cooling water is 50°C;
[0073] The temperature of the aging strengthening is 170±10° C., the heat preservation time is 7 to 9 hours, and the cooling method is air cooling.
[0074] The aluminum alloy provided by the present invention is mainly composed of α-(Al)+θ-Al2Cu+Mn6Cu4Al after heat treatment solid solution aging strengthening. 29 phase + eutectic silicon, etc. Among them, w (Mn) is ≥ 0.8% of the alloy, and a small amount of Mn6Cu4Al is present when the primary solution treatment temperature is 455℃~475℃ 29 The phase dissolves into the matrix and is distributed in a discontinuous network at the grain boundary to prevent melting and overburning at high temperature; when the secondary solution treatment temperature is 495℃~515℃, almost all θ-Al2Cu dissolves into α-(Al) solid solution, and a large number of dispersed θ-Al2Cu phases and Mn6Cu4Al2Cu phases appear in the alloy structure after quenching and aging. 29 The phase distorts the crystal lattice of the α-(Al) solid solution and closes the slip planes between grains, which plays a role in solid solution strengthening and dispersion hardening, thereby improving the tensile strength and yield strength of the alloy.
[0075] The present invention provides an application of the high-performance cast aluminum alloy described in the above technical solution or the high-performance cast aluminum alloy prepared by the preparation method described in the above technical solution in lightweight materials for automobile parts.
[0076] In order to further illustrate the present invention, a high performance cast aluminum alloy provided by the present invention and its preparation method and application are described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0077] Example 1
[0078] (1) Ingredients
[0079] Add according to the ingredient list of the present invention.
[0080] Table 1 Pre-melted material alloy and specifications
[0081] name Brand or specification model Industrial high purity aluminum Al99.70 or Al99.60 Crystalline Silicon Secondary Silicon Pure magnesium ingot Mg99.80 Manganese Metal JMn97 or JMn96 Cathode copper Cu-CATH-2 Cerium-rich rare earth (RE) Ce≥55wt%,La≥25wt% Aluminum Titanium Master Alloy AlTi10 Aluminum-Molybdenum Master Alloy AlMo60 Aluminum Vanadium Master Alloy AlV10 Aluminum Strontium Master Alloy AlSr10
[0082] (2) Charge melting
[0083] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 552°C for 70 minutes, then heated to 785°C for melting and kept at this temperature for 1.1 hours.
[0084] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0085] 1) When the temperature of the aluminum melt drops to 745℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 425 rpm and the compressed air flow rate is 0.6m 3 / h, after degassing for 122s;
[0086] 2) Add pure magnesium ingot, continue degassing for 182 seconds, rotor speed 371 rpm, compressed air flow 0.4m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat preservation is 0.5h;
[0087] 3) When the aluminum liquid temperature drops to 720℃, add aluminum strontium master alloy, continue degassing for 185s, rotor speed 515 rpm, compressed air flow 0.8m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0088] (4) Pouring
[0089] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 705℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle. The pouring is slow and continuous. After it is completely solidified, the sample mold is turned over with pliers to demould the sample. Pay attention to turning the sample mold smoothly and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0090] (5) Heat treatment process
[0091] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 1.
[0092] Table 2 Heat treatment process
[0093]
[0094] The types and compositions of the aluminum alloy materials prepared in Example 1 are shown in Table 3:
[0095] Table 3 Examples and Comparative Examples Composition (wt%)
[0096] element Si Mg Cu Ti RE Mn V Mo Sr Fe Al Example 1 4 0.5 4.5 0.13 0.13 1.104 0.25 0.05 0.015 0.7 bal. Example 2 6.5 0.3 5.1 0.1 0.08 0.494 0.03 0.01 0.025 0.2 bal. Example 3 9 0.1 3.2 0.08 0.05 0.86 0.15 0.03 0.011 0.5 bal. Example 4 8 0.2 3.6 0.15 0.15 0.616 0.3 0.02 0.018 0.3 bal. Example 5 5 0.4 4.2 0.09 0.1 0.372 0.2 0.04 0.023 0.1 bal. Example 6 7 0.6 4.8 0.12 0.09 0.982 0.1 0.02 0.017 0.6 bal. Comparative Example 1 4 0.5 4.5 0.13 0.13 0 0.25 0.05 0.015 0.3 bal. Comparative Example 2 6.5 0.3 5.1 0.1 0.08 0.494 0 0.01 0.025 0.2 bal. Comparative Example 3 9 0.1 3.2 0.08 0.05 0.86 0.15 0 0.011 0.5 bal. Comparative Example 4 8 0.2 3.6 0.15 0.15 0.616 0 0 0.018 0.3 bal.
[0097] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 1 of the present invention are shown in Table 4:
[0098] Table 4 Performance test results of the products of the embodiments and comparative examples
[0099]
[0100]
[0101] The test results of the thermophysical properties of the aluminum alloy material prepared in Example 1 of the present invention are shown in Table 5:
[0102] Table 5 Thermophysical properties
[0103]
[0104] The flowability test results of the aluminum alloy material prepared in Example 1 of the present invention are shown in Table 6:
[0105] Table 6 Flow properties
[0106]
[0107] Example 2
[0108] (1) Ingredients
[0109] Add according to ingredient table 1 of the present invention.
[0110] (2) Charge melting
[0111] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 565°C for 65 minutes, then heated to 790°C for melting and kept at this temperature for 1.5 hours.
[0112] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0113] 1) When the temperature of the aluminum melt drops to 750℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 435 rpm and the compressed air flow rate is 0.7m 3 / h, after degassing for 130s;
[0114] 2) Add pure magnesium ingot, continue degassing for 195s, rotor speed 380 rpm, compressed air flow 0.5m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat preservation is 0.7h;
[0115] 3) When the aluminum liquid temperature drops to 730℃, add aluminum strontium master alloy, continue degassing for 200s, rotor speed 525 rpm, compressed air flow 0.9m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0116] (4) Pouring
[0117] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 720℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle. The pouring is slow and continuous. After it is completely solidified, the sample mold is flipped with pliers to demould the sample. Pay attention to flipping the sample mold smoothly and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0118] (6) Heat treatment process
[0119] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 2.
[0120] The types and compositions of the aluminum alloy materials prepared in Example 2 are shown in Table 3.
[0121] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 2 of the present invention are shown in Table 4.
[0122] The test results of the thermal physical properties of the aluminum alloy material prepared in Example 2 of the present invention are shown in Table 5.
[0123] The flow performance test results of the aluminum alloy material prepared in Example 2 of the present invention are shown in Table 6.
[0124] Example 3
[0125] (1) Ingredients
[0126] Add according to ingredient table 1 of the present invention.
[0127] (2) Charge melting
[0128] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 570°C for 75 minutes, then heated to 795°C for melting and kept at this temperature for 1.5 hours.
[0129] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0130] 1) When the temperature of the aluminum melt drops to 760℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 440 rpm and the compressed air flow rate is 0.65m 3 / h, after degassing for 140s;
[0131] 2) Add pure magnesium ingot, continue degassing for 140s, rotor speed 395 rpm, compressed air flow 0.5m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat preservation is 0.8h;
[0132] 3) When the aluminum liquid temperature drops to 735℃, add aluminum strontium master alloy, continue degassing for 220s, rotor speed 535 rpm, compressed air flow 1.0m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0133] (4) Pouring
[0134] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 725℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle, pouring slowly and continuously. After it is completely solidified, use pliers to flip the sample mold to demould the sample. Pay attention to flipping the sample mold smoothly and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0135] (7) Heat treatment process
[0136] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 2.
[0137] The types and compositions of the aluminum alloy materials prepared in Example 3 are shown in Table 3.
[0138] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 3 of the present invention are shown in Table 4.
[0139] The test results of the thermal physical properties of the aluminum alloy material prepared in Example 3 of the present invention are shown in Table 5.
[0140] The flowability test results of the aluminum alloy material prepared in Example 3 of the present invention are shown in Table 6.
[0141] Example 4
[0142] (1) Ingredients
[0143] Add according to ingredient table 1 of the present invention.
[0144] (2) Charge melting
[0145] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 580°C for 78 minutes, then heated to 801°C for melting and kept at this temperature for 1.8 hours.
[0146] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0147] 1) When the temperature of the aluminum melt drops to 7650℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 465 rpm and the compressed air flow rate is 0.7m 3 / h, after degassing for 150s;
[0148] 2) Add pure magnesium ingot, continue degassing for 230s, rotor speed 410 rpm, compressed air flow 0.55m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat preservation is 0.8h;
[0149] 3) When the aluminum liquid temperature drops to 735℃, add aluminum strontium master alloy, continue degassing for 240s, rotor speed 535 rpm, compressed air flow 1.1m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0150] (4) Pouring
[0151] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 740℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle. The pouring is slow and continuous. After it is completely solidified, the sample mold is turned over with pliers to demould the sample. Pay attention to turning the sample mold smoothly and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0152] (8) Heat treatment process
[0153] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 2.
[0154] The types and compositions of the aluminum alloy materials prepared in Example 4 are shown in Table 3.
[0155] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 4 of the present invention are shown in Table 4.
[0156] The test results of the thermal physical properties of the aluminum alloy material prepared in Example 4 of the present invention are shown in Table 5.
[0157] The flow performance test results of the aluminum alloy material prepared in Example 4 of the present invention are shown in Table 6.
[0158] Example 5
[0159] (1) Ingredients
[0160] Add according to ingredient table 1 of the present invention.
[0161] (2) Charge melting
[0162] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 590°C for 78 minutes, then heated to 805°C for melting and kept at this temperature for 1.9 hours.
[0163] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0164] 1) When the temperature of the aluminum melt drops to 770℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 475 rpm and the compressed air flow rate is 0.75m 3 / h, after degassing for 150s;
[0165] 2) Add pure magnesium ingot, continue degassing for 245s, rotor speed 405 rpm, compressed air flow 0.55m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat preservation is 0.9h;
[0166] 3) When the aluminum liquid temperature drops to 738℃, add aluminum strontium master alloy, continue degassing for 250s, rotor speed 545 rpm, compressed air flow 1.1m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0167] (4) Pouring
[0168] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 740℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle. The pouring is slow and continuous. After it is completely solidified, the sample mold is turned over with pliers to demould the sample. Pay attention to turning the sample mold smoothly and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0169] (9) Heat treatment process
[0170] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 2.
[0171] The types and compositions of the aluminum alloy materials prepared in Example 5 are shown in Table 3.
[0172] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 5 of the present invention are shown in Table 4.
[0173] The test results of the thermal physical properties of the aluminum alloy material prepared in Example 5 of the present invention are shown in Table 5.
[0174] The flow performance test results of the aluminum alloy material prepared in Example 5 of the present invention are shown in Table 6.
[0175] Example 6
[0176] (1) Ingredients
[0177] Add according to ingredient table 1 of the present invention.
[0178] (2) Charge melting
[0179] After the melting furnace is loaded, the temperature should be slowly raised. Crystalline silicon, pure aluminum ingots, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, cerium-rich rare earth, cathode copper and aluminum-titanium master alloy should be kept at 600°C for 80 minutes, then heated to 810°C for melting and kept at this temperature for 2 hours.
[0180] (3) Adding pure magnesium ingot and aluminum strontium master alloy during degassing
[0181] 1) When the temperature of the aluminum melt drops to 780℃, add environmentally friendly refining agent and start the degasser. The rotor and baffle automatically sink and enter the stage automatically. The rotor speed is 480 rpm and the compressed air flow rate is 0.8m 3 / h, after degassing for 160s;
[0182] 2) Add pure magnesium ingot, continue degassing for 260s, rotor speed 410 rpm, compressed air flow 0.6m 3 / h, after degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned, and the heat is kept for 1h;
[0183] 3) When the aluminum liquid temperature drops to 740℃, add aluminum strontium master alloy, continue degassing for 260s, rotor speed 550 rpm, compressed air flow 1.2m 3 / h; After degassing, the rotor rises, and the rotor vents are immediately cleared with tools, and the slag on the liquid surface is turned over with a slag scoop, and then the slag on the surface of the aluminum liquid is cleaned.
[0184] (4) Pouring
[0185] The sample mold is neatly placed on the mold frame; the pouring temperature is controlled within 750℃, and the aluminum liquid is poured into the sample mold with a hand-held ladle. The pouring is slow and continuous. After it is completely solidified, the sample mold is flipped with pliers to demould the sample. Pay attention to the smooth movement of flipping the sample mold and do not touch or scratch the surface of the sample blank. The surface should be smooth and flat.
[0186] (10) Heat treatment process
[0187] The samples were subjected to casting solid solution strengthening and aging treatment, see Table 2.
[0188] The type and composition of the aluminum alloy material prepared in Example 6 are shown in Table 3.
[0189] The performance test results of the tensile strength, yield strength and elongation of the aluminum alloy prepared in Example 6 of the present invention are shown in Table 4.
[0190] The test results of the thermal physical properties of the aluminum alloy material prepared in Example 6 of the present invention are shown in Table 5.
[0191] The flow performance test results of the aluminum alloy material prepared in Example 6 of the present invention are shown in Table 6.
[0192] It can be seen from the above embodiments that the present invention provides a high-performance cast aluminum alloy, which includes the following components by mass fraction: 4.2-9.3% Si, 3.0-5.2% Cu, 0.1-0.6% Mg, 0.3-1.2% Mn, 0.03-0.3% V, 0.08-0.15% Ti, 0.01-0.05% Mo, 0.01-0.03% Sr, 0.05-0.15% RE, Fe≤0.7% and the balance aluminum; Mn (wt%) = 1.22Fe (wt%) + 0.25. The alloy contains Si, Cu, Mn and rare earth elements, and the alloy structure is mainly composed of α-(Al) + θ-Al2Cu + Mn6Cu4Al 29 phase + eutectic silicon, etc., with a large number of dispersed θ-Al2Cu phases and Mn6Cu4Al 29 The phase distorts the crystal lattice of the α-(Al) solid solution and closes the slip plane between grains, which plays a role in solid solution strengthening and dispersion hardening, and improves the tensile strength, tensile strength and yield strength of the alloy. The experimental results show that the tensile strength of aluminum alloy at room temperature is 450-470MPa, the yield strength is 435-445MPa, and the elongation is 3-6%; the tensile strength at 200℃ is 363-379MPa, the yield strength is 348-356MPa, and the elongation is 3.7-7.3%; the liquidus temperature is 642-648℃; the solidus temperature is 562-574℃; the latent heat of crystallization is 342-361KJ / kg; the material shrinkage is 0.5; the linear expansion coefficient at 20-200℃ is 21.1-22.3×10 -6 K-1 ; The relative wear rate is 0.8~1; the average flow distance at 650℃ is 551~567mm, the average flow distance at 680℃ is 705~712mm, the average flow distance at 710℃ is 882~899mm, and the average flow distance at 740℃ is 947~962mm.
[0193] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high performance cast aluminum alloy comprising the following components by mass fraction: 4.2-9.3% Si, 3.0-5.2% Cu, 0.1-0.6% Mg, 0.3-1.2% Mn, 0.03-0.3% V, 0.08-0.15% Ti, 0.01-0.05% Mo, 0.01-0.03% Sr, 0.05-0.15% RE, Fe≤0.7% and the balance aluminum; in, Mn(wt%)=1.22Fe(wt%)+0.
25.
2. The high performance cast aluminum alloy according to claim 1, It is characterized in that The main strengthening phase of the high performance cast aluminum alloy is θ-Al 2 Cu phase and Mn 6 Cu 4 Al 29 Mutually.
3. The high performance cast aluminum alloy according to claim 1, It is characterized in that RE rare earth elements are Ce and La.
4. A method for preparing the high performance cast aluminum alloy according to any one of claims 1 to 3, The following steps are involved: a) melting crystalline silicon, pure aluminum ingot, aluminum-molybdenum master alloy, aluminum-vanadium master alloy, metallic manganese, rare earth, cathode copper and aluminum-titanium master alloy to obtain an aluminum melt; b) mixing the aluminum melt and a refining agent, and degassing; c) continuing to add pure magnesium ingots and aluminum-strontium master alloys, and continuously degassing to obtain aluminum liquid; d) pouring the molten aluminum, and performing solid solution strengthening and aging treatment after demoulding to obtain a cast aluminum alloy.
5. The preparation method according to claim 4, It is characterized in that The melting includes: After loading, keep the temperature at 550-600°C for 60-80 minutes, then increase the temperature to 780-810°C and keep it for 1-2 hours.
6. The preparation method according to claim 5, It is characterized in that The aluminum melt is mixed with a refining agent at 740-780° C.; The degassing conditions include: rotor speed of 425-482 rpm, compressed air flow rate of 0.6-0.8 m 3 / h, the degassing time is 120~160s.
7. The preparation method according to claim 5, It is characterized in that Step c) comprises: The conditions for continuous degassing after adding pure magnesium ingot include: rotor speed of 370-415 rpm, compressed air flow rate of 0.4-0.6 m 3 / h, continue degassing for 180-260s, keep warm for 0.5-1h; Cool down to 720-740℃, add aluminum-strontium master alloy, continue degassing for 180-260s, rotor speed is 515-550rpm, compressed air flow rate is 0.8-1.2m 3 / h.
8. The preparation method according to claim 7, It is characterized in that The pouring temperature is 700-750°C.
9. The preparation method according to claim 7, It is characterized in that The solution treatment includes primary solution treatment and secondary solution treatment; The temperature of the first-stage solid solution treatment is 465±10°C, and the holding time is 1 to 2 hours; The temperature of the secondary solution treatment is 505±10°C, and the holding time is 6 to 8 hours; The temperature of the aging strengthening is 170±10° C., and the insulation time is 7 to 9 hours.
10. Use of the high-performance cast aluminum alloy according to any one of claims 1 to 3 or the high-performance cast aluminum alloy prepared by the preparation method according to any one of claims 4 to 9 in lightweight materials for automobile parts.