Short-time high-temperature-resistant aluminum alloy for aerospace advanced aircraft component and preparation method thereof
By optimizing the composition and preparation process of Al-Cu-Mg-Ag alloy, the problem of insufficient performance of aluminum alloy under short-term high-temperature service conditions in the aerospace field is solved, and the high-temperature mechanical performance is improved and cost reduction is reduced, meeting the needs of space vehicles.
Patent Information
- Application Number
- CN202411183894.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing heat-resistant aluminum alloy materials are insufficient in short-term high-temperature service conditions in the aerospace field, and have high cost and process complexity, making it difficult to meet the demands of advanced aerospace vehicles for high temperature and low cost.
By optimizing the composition and preparation process of Al-Cu-Mg-Ag alloy, the Cu, Ag, Mg/Si ratio and H element content are controlled, and semi-continuous casting, homogenized annealing, forging, solid solution treatment, cold deformation stress removal treatment is adopted. and aging treatment, a new type of short-term high-temperature aluminum alloy for advanced aerospace aircraft components was prepared.
It significantly improves the high-temperature short-term mechanical properties and purity of the material, broadens the process window, reduces costs, improves the stability and qualification rate of mass production, and meets the high-temperature and economic requirements of spacecraft.
Smart Images

Figure CN119061300A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new alloy materials, and in particular to an aluminum alloy resistant to short-time high temperature for advanced aerospace aircraft components and a preparation method thereof. Background Art
[0002] With the continuous development of advanced aerospace aircraft technology, higher requirements are put forward for key components, including important indicators such as lightweight, high temperature resistance of 300-400℃, and low-cost batch production. Traditional heat-resistant titanium alloy materials have gradually failed to meet these emerging needs due to their high cost and difficult processing characteristics. In contrast, heat-resistant aluminum alloys have been widely used in heat-resistant parts in the fields of automobiles, aerospace, etc. due to their low density, high specific strength, and good heat resistance. At present, heat-resistant aluminum alloys and technologies for components in the aerospace field mainly focus on the long-term high temperature durability, creep properties, and performance after long-term heat exposure of the materials. For example, the technologies disclosed in patent documents such as Chinese patents CN111373861B and CN101245430A are mostly concentrated in these aspects.
[0003] With the development of advanced aerospace vehicles, the heat-resistant temperature requirements for materials are getting higher and higher, especially in the range of 300-400°C. The existing heat-resistant aluminum alloy technology is mainly aimed at the long-term service environment in the aviation field, and is not fully suitable for the short-term high-temperature service conditions in the aerospace field. In addition, in order to maintain the performance of the material, the addition of rare earth elements (Sc, Er, Y) or precious metal elements (Ag) in the existing technology leads to increased costs and complicated process, which have become obstacles to further development. Therefore, it is necessary to develop new heat-resistant aluminum alloy materials to meet the demand for higher service temperatures in the aerospace field, and have good economy and processability. Summary of the invention
[0004] The present invention is intended to provide an aluminum alloy resistant to short-time high temperature for advanced aerospace aircraft components and a preparation method thereof, aiming to achieve low cost and short-time high temperature resistance of the aluminum alloy.
[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components, characterized in that the content of each element is: Cu 5.00-5.90wt%, Ag 0.50-1.60wt%, Mg0.20-0.60wt%, Mn 0.20-0.40wt%, Ti 0.02-0.20wt%, Zr 0.10-0.20wt%, Fe 0-0.05wt%, Si 0-0.05wt%, H 0-0.1ppm, and the balance is Al.
[0006] The amount of element addition was further optimized to obtain a preferred solution: the content of each element was: Cu 5.50-5.90wt%, Ag 0.80-1.50wt%, Mg 0.25-0.40wt%, Mn 0.30-0.40wt%, Ti 0.05-0.10wt%, Zr 0.10-0.15wt%, Fe 0-0.03wt%, Si 0-0.02wt%, H 0-0.1ppm, and the balance was Al.
[0007] On the other hand, the technical solution also provides a method for preparing short-time high-temperature resistant aluminum alloys for advanced aerospace aircraft components, including semi-continuous casting to prepare ingots, homogenization annealing, surface processing and material separation, forging blanking, free forging / ring rolling / reverse extrusion hot forming intermediate products, solution treatment, cold deformation stress relief treatment and aging treatment.
[0008] Preferably, as an improvement, Mg / Si≥29, Ag / Mg=3~4 in the elements.
[0009] Preferably, as an improvement, the ratio of Cu+Ag in the elements is 6.5-7.5.
[0010] Preferably, as an improvement, the purity of Al, Mg and Ag is 99.99% and the particle size of Ag is 3-5 mm.
[0011] Preferably, as an improvement, the operation of forging blanks and forming intermediate products is to first perform 1 to 3 fires of forging blanks at 430-480°C, and then perform 2 to 8 fires of free forging at 400-480°C to produce intermediate products of aerospace components; or perform 1 to 3 fires of forging blanks at 430-480°C, and then perform 2 to 5 fires of ring rolling at 430-460°C to produce intermediate products of aerospace components; or perform 1 to 3 fires of forging blanks at 430-480°C, and then perform one back extrusion at 430-460°C to produce intermediate products of aerospace components.
[0012] The preferred scheme for the operation of forging blanks and forming intermediate products is: first perform 2 fire forging blanks at 440-460°C, and then perform 4 fires of free forging at 440-460°C to produce intermediate products of aerospace components; or first perform 2 fire forging blanks at 440-460°C, and then perform 2 fires of ring rolling at 440-460°C to produce intermediate products of aerospace components; or first perform 2 fire forging blanks at 440-460°C, and then perform one back extrusion at 440-460°C to produce intermediate products of aerospace components.
[0013] Preferably, as an improvement, the solution treatment is to subject the intermediate product to single-stage solution treatment or double-stage solution treatment and then water quenching, the single-stage solution treatment is: solution treatment at 490-530°C for 3-8h; the double-stage solution treatment is solution treatment at 490-510°C for 2-5h, and then solution treatment at 510-520°C for 3-5h.
[0014] Preferably, as an improvement, the single-stage solution treatment is solution treatment at 510-520°C for 6-7 hours and then water quenching, and the double-stage solution treatment is solution treatment at 490-500°C for 3 hours, and then further solution treatment at 510-520°C for 3 hours, and water quenching is completed within 10 seconds.
[0015] Preferably, as an improvement, within 30 minutes after the solution treatment, a ring rolling or free forging method is used to perform 0-3% stress relief deformation at room temperature.
[0016] The preferred scheme for cold deformation stress relief treatment is: within 30 minutes after solution treatment, 0-2% cold deformation is performed by ring rolling.
[0017] Preferably, as an improvement, a single-stage aging treatment is adopted during the aging treatment, the treatment temperature is 130-180° C., and the treatment time is 7-22 hours.
[0018] The preferred scheme for aging treatment is: short-time single-stage aging at 140-165°C × 6-10h.
[0019] The principles and advantages of this solution are: In this technical solution, the composition and preparation process of the alloy material are comprehensively optimized based on Al-Cu-Mg-Ag alloy in order to solve the problems existing in the application of aluminum alloys in advanced aerospace aircraft components in the prior art.
[0020] Al-Cu-Mg-Ag alloy is a new type of heat-resistant aluminum alloy structural material. Its comprehensive mechanical properties are better than those of existing conventional heat-resistant aluminum alloys, mainly due to the presence of a high thermal stability Ω phase in its microstructure. At present, in order to ensure that Al-Cu-Mg-Ag alloy has good high-temperature performance, a large amount of Cu and Ag elements are often added in the prior art, and certain requirements are made on the Ag / Mg ratio and Cu / Mg ratio. After systematically studying the Al-Cu-Mg-Ag series alloys, the inventor creatively discovered that the dominant Ω phase is sensitive to the Mg / Si ratio. To ensure good high-temperature performance and its uniformity, a high Mg / Si ratio must be strictly controlled. If the Mg / Si ratio is too small, part of the Mg solute atoms in the alloy precipitate in the form of MgSi phase, the formation of Mg-Ag clusters is inhibited, and then the precipitation of the Ω phase is hindered, and the formation of the θ′ phase is promoted, which ultimately leads to a decrease in the high-temperature mechanical properties of the alloy. In addition, the inventors found that focusing on the improvement of short-term high-temperature mechanical properties requires a higher Cu+Ag content and Ag / Mg ratio. However, too high a Cu+Ag content and too high an Ag / Mg ratio do not significantly improve short-term high-temperature mechanical properties, but instead aggravate component segregation, unstable performance and increased material costs. Because the Cu content of Al-Cu-Mg-Ag heat-resistant aluminum alloy exceeds the limit solid solubility, the alloy contains a large amount of Cu-rich excess phase ( Figure 1 and Figure 2 ), resulting in a narrow process window for material preparation, which in turn leads to difficulty in controlling the forming process, low flaw detection pass rate, long product delivery cycle and high price.
[0021] Based on this, this technical solution further determined through research that Cu+Ag=6.5~7.5, Mg / Si≥29, Ag / Mg=3~4, so as to achieve the purpose of controlling the precipitation of Ω phase and θ' phase, improving short-term high-temperature performance and its uniformity, while controlling the degree of component segregation and performance uniformity, and balancing room temperature performance and high temperature performance.
[0022] Moreover, the inventors have also found through research that the H element has a direct impact on the process performance of the excess phase during the forming process. Controlling the H element content is extremely important for the process performance, defect control, performance and uniformity of the alloy. By limiting the H content to 0-0.1ppm, the purity can be controlled, cracking can be prevented during the material forming process, and the product flaw detection pass rate and mechanical property uniformity can be improved.
[0023] In terms of preparation process, Al-Cu-Mg-Ag heat-resistant aluminum alloy is a highly alloyed alloy, and it is difficult to control component segregation and performance uniformity, especially in mass production, and it is easy to have problems with poor batch stability. The inventors have found that the performance uniformity and batch stability can be effectively improved by controlling the deformation process parameters and stress relief cold deformation treatment during the production process. Specifically, through special forging blanking and intermediate product preparation processes, the deformation amount can be guaranteed, and the mechanical properties and their uniformity can be improved; by optimizing the solid solution treatment, the uniformity of the room temperature and high temperature mechanical properties of the alloy material can be improved; through stress relief and aging treatment, it can provide a basis for the uniform precipitation of strengthening phases during the subsequent aging period, improve performance uniformity, and balance short-term high temperature mechanical properties and preparation efficiency.
[0024] During the technical research and development period, the control of the process conditions of forging and heat treatment is one of the difficulties in the research and development of this technical solution: the material structure of this technical solution is complex, and it is sensitive to the thermometer and deformation during forging. If it is not properly controlled, it will lead to the risk of unqualified organization, unqualified mechanical properties and unqualified ultrasonic flaw detection, which will eventually affect the performance of the product. If the forging temperature is higher than 480℃, the organization will be overheated or overburned, the low-melting-point intergranular material will melt, and the oxidizing gas in the furnace will penetrate into the grain boundary, oxidizing the intergranular material and destroying the connection between the grains. There will be a risk of cracking during forging, as well as unqualified organization and unqualified mechanical properties after forging, which will affect the use of the product; if the forging temperature is lower than 330℃, the forging has poor plasticity and high deformation resistance. There will also be a risk of cracking during forging, making the product unusable. Secondly, if the forging deformation is insufficient, it will cause a coarse organization and the strength of the forging will not meet the requirements, which will affect the performance of the product.
[0025] For the heat treatment process, the heat treatment temperature and holding time need to be strictly controlled. If the solution temperature is too high, overburning will occur, resulting in unqualified structure. Long holding time will lead to coarsening of grains and unqualified mechanical properties. If the solution temperature is too low or the holding time is too short, the alloy elements cannot be completely dissolved, and the final strengthening phase precipitated after aging is small, resulting in low mechanical properties. Inappropriate aging temperature and holding time will affect the number and distribution of precipitated phases, thereby affecting the mechanical properties of the product, especially the high-temperature mechanical properties, and ultimately causing the product's performance to be unqualified.
[0026] In summary, the beneficial effects of this technical solution are:
[0027] 1. Compared with the Al-Cu-Mg-Ag heat-resistant aluminum alloy in the prior art, which lacks strict control over purity and other properties, the present invention strictly controls the contents of Fe, Si, Mg / Si and H, so that the obtained aluminum alloy materials and products have higher purity, and the quality and batch stability are effectively controlled.
[0028] 2. The present invention emphasizes high temperature short-time mechanical properties, and controls alloy elements, gas content and purity, especially the mechanical properties data within 30 minutes, which has significant advantages over the prior art. The chemical composition control and preparation method of the alloy disclosed in this technical solution are tested by experiments: 300℃ high and tangential tensile strength>300MPa, elongation>9%, 350℃ high and tangential tensile strength>150MPa, elongation>10%.
[0029] 3. The intrinsic characteristics of Al-Cu-Mg-Ag heat-resistant aluminum alloy determine that its hot working process window is narrow and its process performance is poorer than other 2-series aluminum alloys. The present invention broadens the process window and significantly improves the process performance by controlling the main alloy elements, impurity elements and gas elements.
[0030] 4. Al-Cu-Mg-Ag heat-resistant aluminum alloy contains a large amount of Cu-rich excess phase ( Figure 1 and Figure 2 ), which easily produces microscopic defects in the material preparation process, and further leads to a low flaw detection pass rate. The present invention significantly improves the flaw detection pass rate by strictly controlling the H content.
[0031] 5. Al-Cu-Mg-Ag heat-resistant aluminum alloy often contains high copper and high silver, the process is difficult to control, the scrap rate is high, and the process used is mostly for long-term service performance. The process is complex, the cycle is long, and the energy consumption is high, which leads to its cost being much higher than that of ordinary aluminum alloy. Based on the technical problem to be solved, the present invention focuses on short-term high-temperature performance, optimizes from composition to process, and controls all aspects such as purity, gas content and stress relief, so that the cost of the alloy and products of the technical solution has obvious advantages over the Al-Cu-Mg-Ag heat-resistant aluminum alloy in the prior art.
[0032] 6. In summary, the present invention significantly improves material quality stability, process window, qualified rate, high-temperature short-time performance and other performances compared with the prior art through overall optimization of alloy materials and preparation processes. Its batch production capacity has excellent stability and meets the high requirements of aerospace vehicle structural parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the metallographic structure of the alloy after homogenization heat treatment of Example 1 of the present invention (the figure indicates the Cu-rich excess phase).
[0034] Figure 2 This is a scanned photograph of the alloy properties after heat treatment of Example 1 of the present invention (the figure indicates the Cu-rich excess phase).
[0035] Figure 3 This is a diagram showing the short-term mechanical property variation of the alloy in Example 1 of the present invention.
[0036] Figure 4 Schematic diagram of the advanced aerospace vehicle component blank in Example 4. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in combination with specific examples, but the implementation methods of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following implementation methods are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.
[0038] Program Overview:
[0039] A short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components, the content of each element is: Cu 5.00-5.90wt%, Ag 0.50-1.60wt%, Mg 0.20-0.60wt%, Mn 0.20-0.40wt%, Ti 0.02-0.20wt%, Zr 0.10-0.20wt%, Fe 0-0.05wt%, Si 0-0.05wt%, H 0-0.1ppm, and the balance is Al.
[0040] Among them, Mg / Si≥29, Ag / Mg=3~4, Cu+Ag=6.5~7.5, and the purity of Al, Mg and Ag are all 99.99%; the particle size of Ag is 3~5mm.
[0041] A method for preparing a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components comprises the following steps:
[0042] S1. Semi-continuous casting to prepare ingots. All raw materials for preparing ingots are pure metals (Al 99.99% (GB / T1196-2008), Mg99.99% (GB / T 3499-2011), IC-Ag99.99% (GB / T 4135-2016), aluminum master alloy (GB / T 27677-2011): aluminum-manganese master alloy, aluminum-copper master alloy, aluminum-zirconium master alloy, aluminum-titanium (refining agent) master alloy; in addition, considering that the melting point and specific gravity of Ag are relatively higher than those of the matrix Al element, in order to avoid segregation due to the high melting point and specific gravity, silver beads or silver particles with a particle size of 3 to 5 mm are uniformly added to the aluminum liquid during the smelting process; during smelting, pure aluminum is first melted, and the master alloy is added after the pure aluminum is completely melted. After the master alloy is melted, the temperature is lowered and pure magnesium and pure silver are added. After the pure magnesium and pure silver are completely melted, degassing and slag removal are carried out, and the aluminum-titanium master alloy refiner prepared in advance is added, and semi-continuous casting is carried out after standing.
[0043] S2, homogenization annealing: After the ingot casting is completed, double-stage homogenization annealing is carried out, and the holding time is extended during the annealing process to effectively eliminate the casting coarse dendrites and reduce the risk of cracking. Specifically, the specific process of the annealing process is: after keeping at 440-470℃ for 10-30h, keep at 500-530℃ for 30-50h, and then air cool.
[0044] S3. Surface processing and material sorting: The roughness of the blank surface processing is required to be ≤3.2, and UT ultrasonic flaw detection is internally controlled. After confirming that there are no defects, the material is powdered.
[0045] S4. Forging and forming intermediate products: first forging the blank for 1 to 3 times at 430-480°C, and then free forging for 2 to 8 times at 400-480°C to produce intermediate products for aerospace components; or ring rolling for 2 to 5 times at 430-460°C to produce intermediate products for aerospace components; or reverse extrusion for one time at 430-460°C to produce intermediate products for aerospace components.
[0046] S6. Solution treatment: The intermediate product is subjected to single-stage solution treatment or double-stage solution treatment and then water quenched. The single-stage solution treatment is: solution treatment at 490-530°C for 3-8 hours; the double-stage solution treatment is: solution treatment at 490-510°C for 2-5 hours, and then solution treatment at 510-520°C for 3-5 hours.
[0047] S7. Cold deformation stress relief treatment: Within 30 minutes after solution treatment, ring rolling or free forging method is used to perform 0-3% stress relief deformation at room temperature.
[0048] S8. Aging treatment: single-stage aging treatment is adopted, the treatment temperature is 130-180°C, and the treatment time is 7-22h.
[0049] Example 1
[0050] A short-time high-temperature resistant aluminum alloy for advanced aerospace vehicle components, the content of each element of which is: Cu 5.90wt%, Ag 0.50wt%, Mg 0.20wt%, Mn 0.25wt%, Ti 0.05wt%, Zr 0.20wt%, Fe 0.02wt%, Si0.0068wt%, H 0.08ppm, and the balance is Al.
[0051] A preparation method of a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components, comprising the following steps: obtaining an ingot by semi-continuous casting and homogenization heat treatment, opening the ingot by two-fire forging at 450°C, and then performing three-fire free forging at 470°C to manufacture an intermediate product of aerospace aircraft components; performing solid solution at 510°C for 6 hours, and then completing water quenching within 10 seconds. Subsequently, cold ring rolling is performed, with a cold deformation amount of 2%, and the time from solid solution to cold ring rolling is controlled within 30 minutes. Finally, an aging treatment is performed at 150°C for 8 hours to obtain a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components.
[0052] Example 2
[0053] A short-time high-temperature resistant aluminum alloy for advanced aerospace vehicle components, the content of each element of which is: Cu 5.10wt%, Ag 1.60wt%, Mg 0.60wt%, Mn 0.60wt%, Ti 0.20wt%, Zr 0.10wt%, Fe 0.05wt%, Si0.05wt%, H 0.1ppm, and the balance is Al.
[0054] A preparation method of a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components, comprising the following steps: obtaining an ingot by semi-continuous casting and homogenization heat treatment, opening the ingot by one-time forging at 480°C, and then manufacturing an intermediate product of aerospace aircraft components by one-time reverse extrusion at 430°C; performing solid solution treatment at 520°C for 5 hours, and then completing water quenching within 10 seconds. Subsequently, cold ring rolling is performed, with a cold deformation amount of 1%, and the time from solid solution to cold ring rolling is controlled within 30 minutes. Finally, an aging treatment is performed at 140°C for 10 hours to obtain a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components.
[0055] Example 3
[0056] A short-time high-temperature-resistant aluminum alloy for advanced aerospace vehicle components, the content of each element of which is as follows: Cu 5.90wt%, Ag 0.80wt%, Mg 0.35wt%, Mn 0.2wt%, Ti 0.07wt%, Zr 0.15wt%, Fe 0.01wt%, Si 0.008wt%, H 0.07ppm, and the balance is Al.
[0057] A preparation method of a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components, comprising the following steps: obtaining an ingot by semi-continuous casting and homogenization heat treatment, opening the ingot by two-time forging at 470°C, and then ring rolling three times at 460°C to manufacture aerospace aircraft component blanks; performing solid solution at 480°C for 3 hours, then performing solid solution at 515°C for 3 hours, and completing water quenching within 10 seconds. Subsequently, cold ring rolling is performed, with a cold deformation amount of 1%, and the time from solid solution to cold ring rolling is controlled within 30 minutes. Finally, an aging treatment is performed at 160°C for 7 hours to obtain a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components.
[0058] Example 4
[0059] A short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components, wherein the content of each element is: Cu 5.60wt%, Ag 1.10wt%, Mg 0.35wt%, Mn 0.25wt%, Ti 0.07wt%, Zr 0.10wt%, Fe 0.01wt%, Si 0.01wt%, H 0.07ppm, and the balance is Al. The rest is the same as in Example 1.
[0060] Example 5
[0061] The difference between this embodiment and embodiment 1 is that: in this embodiment, a method for preparing a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components includes the following steps: semi-continuous casting and homogenization heat treatment are used to obtain an ingot, and the ingot is opened by 1 fire forging at 430°C, and then 8 fires of free forging are performed at 400°C to manufacture an intermediate product of aerospace aircraft components; solid solution is performed at 510°C for 2 hours, and then solid solution is performed at 520°C for 5 hours, and then water quenching is completed within 10 seconds. Subsequently, cold ring rolling is performed, with a cold deformation amount of 3%, and the time from solid solution to cold ring rolling is controlled within 30 minutes. Finally, an aging treatment is performed at 150°C for 8 hours to obtain a short-time high-temperature resistant aluminum alloy for advanced aerospace aircraft components.
[0062] Comparative Example 1
[0063] The difference between the aluminum alloy of this comparative example and that of Example 4 is that the aluminum alloy comprises the following elements in percentage by weight: Cu wt 3.90%, Mg 1.10wt%, Ag 1.10wt%, Mn 0.60wt%, Zr 0.20wt%, Si 0.04wt% and the rest is Al. There is no cold deformation process.
[0064] Comparative Example 2
[0065] The difference between the aluminum alloy of this comparative example and the aluminum alloy of Example 4 is that the aluminum alloy includes the following elements in percentage by weight: Cu 6.50wt%, Mg 0.40wt%, Ag 1.70wt%, Mn 0.35wt%, Zr 0.15wt%, Ti 0.06wt%, Fe 0.03wt%, Si 0.02wt%, and the rest is Al. No cold deformation process
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 4 is that in this comparative example, Mg / Si=25, Ag / Mg=5.
[0068] Comparative Example 4
[0069] The difference between this comparative example and Example 4 is that in this comparative example, Mg / Si=30, Ag / Mg=2.
[0070] Comparative Example 5
[0071] The difference between this comparative example and Example 4 is that in this comparative example, Cu+Ag=5.
[0072] Comparative Example 6
[0073] The difference between this comparative example and Example 4 is that in this comparative example, Cu+Ag=8.
[0074] Comparative Example 7
[0075] The difference between this comparative example and Example 4 is that in this comparative example, H 0.18 ppm
[0076] Comparative Example 8
[0077] The difference between this comparative example and Example 4 is that in this comparative example, the forging temperature is 500°C.
[0078] Comparative Example 9
[0079] The difference between this comparative example and Example 4 is that in this comparative example, the forging temperature is 300°C.
[0080] Comparative Example 10
[0081] The difference between this comparative example and Example 4 is that in this comparative example, the solution treatment temperature is 530° C. and the solution treatment time is 7.5 h.
[0082] Comparative Example 11
[0083] The difference between this comparative example and Example 4 is that in this comparative example, the solution treatment time is 480° C. and the solution treatment time is 2 h.
[0084] Experimental Example 1 Metallographic structure and electron microscope scanning
[0085] The alloy material of Example 1 is subjected to homogenization heat treatment and its metallographic structure is as follows: Figure 1 As shown in the figure, the arrow points to the excess Cu-rich phase; the scanning morphology of the alloy after heat treatment is as follows Figure 2 As shown, the circle position is the Cu-rich excess phase.
[0086] Experimental Example 2 Mechanical Properties Test
[0087] The aluminum alloy prepared in Example 1 was subjected to tensile tests at different temperatures of 200°C, 300°C, 350°C and 400°C, and different holding times of 0min, 10min, 20min, 30min, 60min and 120min. The test results of different holding times are shown in FIG. Figure 3 As shown: It can be seen that under different temperature conditions, the tensile properties after 10 to 30 minutes of treatment generally do not change much. After more than 30 minutes, the performance shows an overall downward trend (normally, the high-temperature tensile test is kept warm for about 10 minutes). Considering the service time of advanced aerospace aircraft, it is more reasonable for the present invention to consider short-term high-temperature mechanical properties within 30 minutes. The test results of room temperature mechanical properties and short-term high-temperature mechanical properties at different temperatures of Example 1 are shown in Table 1.
[0088] Table 1 Mechanical properties test and flaw detection results of Example 1
[0089]
[0090]
[0091] The aluminum alloy materials prepared in Example 2 and Example 3 were subjected to mechanical property tests at different temperatures of 200°C, 300°C, 350°C and 400°C. The test results are shown in Table 2 and Table 3, respectively.
[0092] Table 2 Mechanical properties test and flaw detection results of Example 2
[0093]
[0094] Table 3 Mechanical properties test and flaw detection results of Example 3
[0095]
[0096] Experimental Example 3 Performance Comparison
[0097] Mechanical property tests and ultrasonic flaw detection were performed on Example 4 and Comparative Examples 1 to 11, and the test results are shown in Table 4.
[0098] Table 4 Mechanical properties test and flaw detection results of Example 4 and Comparative Examples 1 to 11
[0099]
[0100] From the data in Table 4, it can be seen that the cold deformation process has a certain influence on the mechanical properties and flaw detection results of aluminum alloys. To ensure good high-temperature performance and its uniformity, it is necessary to strictly control the high Mg / Si ratio. If the Mg / Si ratio is too small, part of the Mg solute atoms in the alloy will precipitate in the form of MgSi phase, and the formation of Mg-Ag clusters will be inhibited, thereby hindering the precipitation of Ω phase and promoting the formation of θ′ phase, which ultimately leads to a decrease in the high-temperature mechanical properties of the alloy. Focusing on the improvement of short-term high-temperature mechanical properties, a higher Cu+Ag content and Ag / Mg ratio are required. However, if the Cu+Ag content is too high and the Ag / Mg ratio is too high, the improvement of short-term high-temperature mechanical properties is not obvious, but it aggravates the segregation of components, unstable performance and increased material costs. Comparative Examples 8 to 9 were all scrapped during flaw detection due to temperature problems during forging, and the next step of heat treatment and mechanical property testing could not be carried out.
[0101] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components, characterized in that: The content of each element is: Cu 5.00~5.90wt%, Ag 0.50~1.60wt%, Mg 0.20~0.60wt%, Mn 0.20~0.40wt%, Ti 0.02~0.20wt%, Zr 0.10~0.20wt%, Fe 0~0.05wt%, Si 0~0.05wt%, H 0~0.1ppm, and the balance is Al.
2. The short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 1, characterized in that: Among the elements, Mg / Si≥29, Ag / Mg=3~4.
3. The short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 2, characterized in that: Among the elements, Cu+Ag=6.5~7.
5.
4. The short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 3, characterized in that: The purity of Al, Mg and Ag is 99.99% and the particle size of Ag is 3-5 mm.
5. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to any one of claims 1 to 4, characterized in that: It includes semi-continuous casting to prepare ingots, homogenization annealing, surface processing and material separation, forging blanking, free forging / ring rolling / reverse extrusion hot forming intermediate products, solution treatment, cold deformation stress relief treatment and aging treatment.
6. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 5, characterized in that: The operation of forging blank and forming intermediate products is to first perform 1 to 3 fires of forging blank at 430 to 480° C., and then perform 2 to 8 fires of free forging at 400 to 480° C. to produce intermediate products of aerospace components; or perform 1 to 3 fires of forging blank at 430 to 480° C., and then perform 2 to 5 fires of ring rolling at 430 to 460° C. to produce intermediate products of aerospace components; or perform 1 to 3 fires of forging blank at 430 to 480° C., and then perform one back extrusion at 430 to 460° C. to produce intermediate products of aerospace components.
7. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 6, characterized in that: The solution treatment is to perform single-stage solution treatment or double-stage solution treatment on the intermediate product and then water quench it. The single-stage solution treatment is: solution treatment at 490-530°C for 3-8h; the double-stage solution treatment is: solution treatment at 490-510°C for 2-5h, and then solution treatment at 510-520°C for 3-5h.
8. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 7, characterized in that: The single-stage solution treatment is to carry out solution treatment at 510-520°C for 6-7 hours and then water quench. The double-stage solution treatment is to carry out solution treatment at 490-500°C for 3 hours and then continue to carry out solution treatment at 510-520°C for 3 hours, and complete water quenching within 10 seconds.
9. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 8, characterized in that: Within 30 minutes after the solution treatment, a ring rolling or free forging method is used to perform 0-3% stress relief deformation at room temperature.
10. The method for preparing a short-time high temperature resistant aluminum alloy for advanced aerospace aircraft components according to claim 9, characterized in that: A single-stage aging treatment is adopted during aging treatment, the treatment temperature is 130-180°C, and the treatment time is 7-22h.
Citation Information
Patent Citations
High strength and high heat resistant aluminum alloy material and preparation method thereof
CN104711468A
An aluminum-copper-magnesium-silver alloy and its heat treatment method
CN111373861B
Heat-resistant and corrosion-resistant Al-Cu-Mg alloy as well as preparation method and application thereof
CN115786788A