Steel for thin-gauge battery shell as well as preparation method and application of steel
The battery shell steel processed through specific components and processes solves the problems of sand holes and ear making during stamping, and improves molding performance and mold service life.
Patent Information
- Application Number
- CN202411170139.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing thin-specification steel for battery shells cannot achieve both sand holes and ear-free during stamping, and the high strength leads to poor molding performance and large mold wear.
Continuous casting billets with specific components are treated with smelting, hot rolling, cold rolling, annealing and water quenching to control carbon content and annealing temperature. Combined with specific cold rolling processes and annealing treatment, they can reduce the pressure-in defects of iron oxide sheets and mixed crystal defects. , reduce sand holes and ear-making phenomena, and improve molding performance.
It realizes a battery shell steel without sand holes and ears, with moderate strength and good molding performance, reducing mold wear and suitable for multi-pass stamping.
Smart Images

Figure CN119061310A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of steel preparation, and in particular relates to a thin-gauge steel for battery shells and a preparation method and application thereof. Background Art
[0002] With the development of new energy vehicles in China, especially the rapid promotion of electric buses and electric buses, the demand for power batteries is increasing. In the production process of batteries, steel battery shells play an important role in ensuring battery quality and safety. Therefore, the quality of steel battery shells is very important. The battery shell is produced by multiple stampings and has a deep forming depth. The stamped battery shell requires high strength and high surface quality to ensure battery safety, so the comprehensive performance of the steel strip is very high. At the same time, with the increase in product demand, the production efficiency of the product is improved, and the stamping speed is rapidly increased. The existing thin-gauge battery shells are usually made of low-carbon steel. However, although the existing low-carbon steel has fewer sand holes and ears, the strength is too high. After the stamping speed is rapidly increased, it will be limited, resulting in poor forming performance and large wear on the mold. Summary of the invention
[0003] Therefore, the technical problem to be solved by the present invention is to overcome the problem that the existing thin-gauge steel for battery shells cannot simultaneously achieve no pinholes and no ears, and to overcome the defects of poor forming performance and large mold wear due to excessive strength, thereby providing a thin-gauge steel for battery shells and its preparation method and application.
[0004] The present invention provides a method for preparing thin-gauge battery shell steel, comprising the following steps:
[0005] 1) Mixing raw materials, smelting and continuously casting to obtain continuous casting billets;
[0006] The continuous casting billet comprises, by mass percentage, the following components: C: 0.02-0.03%, Si: 0.01-0.03%, Mn: 0.10-0.25%, P≤0.015%, S≤0.015%, Als: 0.05-0.07%, Ti: 0.021-0.040%, and the rest are iron elements and unavoidable impurity elements;
[0007] 2) heating, hot rolling, cooling and coiling the continuous casting billet obtained in step 1) to obtain a hot rolled billet;
[0008] The relationship between the final rolling temperature of the hot rolling and the carbon content in the continuous casting billet is T=1066*2(0.4-M*100)±10°C, where T is the final rolling temperature and M is the mass percentage of carbon in the continuous casting billet;
[0009] 3) uncoiling the hot-rolled billet obtained in step 2), pickling it, and cold rolling it to obtain a cold-rolled billet;
[0010] 4) annealing the cold-rolled billet obtained in step 3) at 800-850° C., and then cooling in stages, performing aging treatment, and water quenching treatment to obtain the thin-gauge battery shell steel.
[0011] Preferably, the smelting in step 1) includes converter smelting and refining;
[0012] The converter smelting temperature is 1640-1680°C, and the converter smelting time is 40-60min;
[0013] The continuous casting speed in step 1) is 1.0-1.5 m / min;
[0014] The continuous casting billet has a thickness of 180-220 mm;
[0015] Optionally, the refining includes LF refining and RH refining;
[0016] The LF refining tapping temperature is 1600-1640°C, and the LF refining time is 35-55min;
[0017] The RH refining tapping temperature is 1570-1620° C., and the RH refining time is 8-12 minutes.
[0018] Preferably, in step 2), the continuous casting billet obtained in step 1) is heated to a temperature of 1130-1180° C. out of the furnace and then hot rolled;
[0019] The hot rolling process includes rough rolling and finish rolling;
[0020] Optionally, the pressing rate of the rough rolling is 75%-85%;
[0021] Optionally, the heating step in step 2) further includes a surface peeling treatment of the continuous casting billet.
[0022] Preferably, the hot rolled billet has a thickness of 1.8-3.0 mm;
[0023] Optionally, the cooling in step 2) is layer cooling, cooling to a temperature of 680-740° C.;
[0024] The coiling temperature in step 2) is 660-720°C;
[0025] Preferably, the pickling agent for pickling in step 3) is a hydrochloric acid aqueous solution;
[0026] Optionally, the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 10-20%;
[0027] The present invention does not specifically limit the composition form of the hydrochloric acid aqueous solution. The hydrochloric acid aqueous solution may be an unused hydrochloric acid aqueous solution, or may be a hydrochloric acid aqueous solution obtained by mixing part of the unused hydrochloric acid aqueous solution with a recycled hydrochloric acid aqueous solution that has been recycled and regenerated.
[0028] Preferably, the cold rolling reduction rate in step 3) is 75-87.5%;
[0029] The cold rolling process uses emulsion lubrication, and the saponification value of the emulsion is 180-190 mgKOH / g;
[0030] Optionally, the temperature of the emulsion during cold rolling is 45-70°C;
[0031] Further optionally, the temperature of the emulsion during cold rolling is 50-55°C;
[0032] Optionally, the rolling environment temperature of the cold rolling is 0-50° C. For example, it can be selected that the rolling environment temperature of the cold rolling is room temperature.
[0033] Optionally, the thickness of the cold rolled billet is ≤ 0.4 mm;
[0034] Optionally, after the cold rolling step in step 3) is completed, a coiling step is also included;
[0035] Optionally, the coiling temperature is 0-45°C, for example, optionally, the coiling is performed at room temperature.
[0036] Optionally, after the hot-rolled slab obtained in step 2) is uncoiled in step 3), a hot-rolled slab welding process is also included; post-processing the hot-rolled slab after welding can effectively reduce unnecessary losses of steel in the preparation process.
[0037] Preferably, the annealing time in step 4) is 60-360s;
[0038] The segmented cooling in step 4) includes slow cooling and fast cooling;
[0039] The cooling rate of the slow cooling section is 2-5°C / s, and the slow cooling section is cooled to 680-700°C;
[0040] The cooling rate of the fast cooling section is 40-60°C / s, and the fast cooling section is cooled to 380-420°C;
[0041] The aging treatment temperature in step 4) is 380-420°C, and the aging treatment time is 220-300s;
[0042] After the aging treatment in step 4) is completed, a cooling treatment is also included, and water quenching treatment is performed after cooling to 100-140°C;
[0043] Optionally, the step 4) further includes a cleaning step before the annealing step;
[0044] Optionally, the annealing step in step 4) further includes the steps of uncoiling and cleaning; optionally, the water quenching step in step 4) further includes the steps of leveling, oiling and coiling after completion of the water quenching step.
[0045] Optionally, the leveling reduction is 1.0-1.5%;
[0046] Optionally, the amount of oil applied is 300-500 mg / m 2 , oiling is double-sided oiling;
[0047] Optionally, the coiling temperature is 0-45°C, for example, optionally, the coiling is performed at room temperature.
[0048] The present invention provides a thin-gauge steel for battery shells, which is prepared by the above-mentioned method for preparing the thin-gauge steel for battery shells.
[0049] The present invention also provides an application of the thin-gauge battery shell steel described above in a battery shell.
[0050] The technical solution of the present invention has the following advantages:
[0051] 1. The preparation method of thin-gauge battery shell steel provided by the present invention comprises the following steps: 1) mixing raw materials, smelting and continuously casting to obtain a continuous casting billet; the continuous casting billet, by mass percentage, comprises the following components: C: 0.02-0.03%, Si: 0.01-0.03%, Mn: 0.10-0.25%, P≤0.015%, S≤0.015%, Als: 0.05-0.07%, Ti: 0.021-0.040%, and the rest are iron elements and unavoidable impurity elements; 2) mixing step 1) The obtained continuous casting billet is heated, hot rolled, cooled and coiled to obtain a hot rolled billet; the relationship between the final rolling temperature of the hot rolling and the carbon content in the continuous casting billet is T = 1066*2(0.4-M*100)±10°C, wherein T is the final rolling temperature, and M is the mass percentage of carbon in the continuous casting billet; 3) the hot rolled billet obtained in step 2) is uncoiled, pickled and cold rolled to obtain a cold rolled billet; 4) the cold rolled billet obtained in step 3) is annealed at 800-850°C, and then cooled in sections, aged and water quenched to obtain the thin-gauge battery shell steel. The present invention adopts a continuous casting billet with specific components to effectively reduce the sand holes and earing phenomena in steel; the present invention determines the hot rolling final rolling temperature according to the carbon content in the continuous casting billet and the relationship between the specific hot rolling final rolling temperature and the carbon content in the continuous casting billet. At this corresponding temperature, the iron oxide scale indentation defect can be effectively reduced, the sand hole generation can be reduced, and the strength of the low-carbon steel product can be controlled. At the same time, after the cold rolling billet, a specific annealing temperature of 800-850°C is selected, and then staged cooling, aging treatment, and water quenching treatment are performed, which can cooperate with the hot rolling final rolling temperature, and can jointly eliminate mixed crystal defects, improve the anisotropy of the product, and effectively reduce the generation of earing. The present invention uses continuous casting billets of specific components, controls the carbon content of the continuous casting billets and the final rolling temperature of hot rolling to satisfy a specific relationship, and cooperates with a specific cold rolling process, a specific annealing temperature and a specific treatment after annealing. When the thin-gauge battery shell steel is used to prepare the battery shell, the battery shell can be free of sand holes and earing. The steel has moderate strength (lower than the original low-carbon steel), good forming performance, and little wear on the mold, which can perfectly match the use requirements of multi-pass stamping of the battery shell steel.
[0052] 2. The preparation method of thin-gauge battery shell steel provided by the present invention, wherein the cold rolling uses emulsion lubrication, and the saponification value of the emulsion is 180-190 mgKOH / g; cold rolling can reduce the rolling force and improve the surface smoothness of the strip under the lubrication effect of the emulsion with this saponification value. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0054] Figure 1 Metallographic diagram of hot-rolled billet after hot rolling in Example 1 of the present invention;
[0055] Figure 2 Metallographic diagram of the thin-gauge battery case steel according to Example 2 of the present invention;
[0056] Figure 3 Metallographic diagram of thin-gauge battery case steel according to Example 3 of the present invention;
[0057] Figure 4 Metallographic diagram of the thin-gauge battery case steel of Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0058] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0059] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0060] Example 1
[0061] This embodiment provides a method for preparing thin-gauge battery shell steel, comprising the following steps:
[0062] 1) Mixing the raw materials, smelting and refining in a converter, wherein the converter smelting temperature is 1652° C., the converter smelting time is 51 min, the refining includes LF refining and RH refining, wherein the LF refining temperature is 1611° C., the LF refining time is 36 min, the RH refining tapping temperature is 1584° C., the RH refining time is 9 min, and then continuous casting is performed at a pulling speed of 1.2 m / min to obtain a continuous casting billet, the thickness of the continuous casting billet is 220 mm; the components of the continuous casting billet, by mass percentage, are: C: 0.026%, Si: 0.03%, Mn: 0.15%, P: 0.013%, S: 0.0019%, Als: 0.052%, Ti: 0.024%, and the rest are iron and unavoidable impurities;
[0063] 2) The continuous casting billet obtained in step 1) is subjected to surface peeling treatment and then heat treatment. The furnace temperature of the continuous casting billet after the heat treatment is 1150°C. After being discharged from the furnace, hot rolling is performed. The hot rolling final rolling temperature T=1066*2(0.4-0.026%*100)±10°C is determined according to the carbon content in the continuous casting billet, that is, the hot rolling final rolling temperature is determined to be 804°C. The hot rolling includes rough rolling and then fine rolling, wherein the reduction rate of the rough rolling is 83%. After the rolling is completed, the billet is layer-cooled and then coiled at 692°C to obtain a hot rolled billet with a thickness of 2 mm. The metallographic diagram of the hot rolled billet is as follows: Figure 1 As shown;
[0064] 3) uncoiling the hot-rolled slab obtained in step 2) and welding the hot-rolled slab, pickling it with a hydrochloric acid aqueous solution and then continuously cold rolling it at room temperature, wherein the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 18%, the cold rolling is lubricated by an emulsion, the temperature of the emulsion is 55° C., the saponification value of the emulsion is 181.75 mgKOH / g, the cold rolling reduction rate is 85%, and then coiling it at room temperature to obtain a cold-rolled slab with a thickness of 0.3 mm;
[0065] 4) The cold rolled billet obtained in step 3) is unrolled, washed with water, and annealed at a temperature of 835° C. for 75 seconds. After annealing, it is cooled in stages, first slowly cooled to 680° C. at a cooling rate of 2° C. / s, then quickly cooled to 420° C. at a cooling rate of 45° C. / s, and then aged at a temperature of 420° C. for 230 seconds. Then, it is cooled to 120° C., quenched in a water quenching tank, and then leveled and oiled on both sides at room temperature. The leveling reduction is 1.2% and the oiling amount is 400 mg / m 2 , and then coiled at room temperature to obtain the thin-gauge battery shell steel.
[0066] Example 2
[0067] This embodiment provides a method for preparing thin-gauge battery shell steel, comprising the following steps:
[0068] 1) Mixing the raw materials, smelting and refining in a converter, wherein the converter smelting temperature is 1658° C., the converter smelting time is 48 min, the refining includes LF refining and RH refining, wherein the LF refining temperature is 1620° C., the LF refining time is 36 min, the RH refining tapping temperature is 1578° C., and the RH refining time is 8 min; then continuously casting is performed at a pulling speed of 1.1 m / min to obtain a continuous casting billet, the thickness of the continuous casting billet is 220 mm; the components of the continuous casting billet, by mass percentage, are: C: 0.021%, Si: 0.02%, Mn: 0.22%, P: 0.009%, S: 0.0028%, Als: 0.066-%, Ti: 0.034%, and the rest are iron and unavoidable impurities;
[0069] 2) The continuous casting billet obtained in step 1) is subjected to surface peeling treatment and then heat treatment. The temperature of the continuous casting billet after the heat treatment is 1140° C. After being discharged from the furnace, hot rolling is performed. The hot rolling final rolling temperature T=1066*2(0.4-0.021%*100)±10° C. is determined according to the carbon content in the continuous casting billet, that is, the hot rolling final rolling temperature is determined to be 811° C. The hot rolling includes rough rolling and then finish rolling, wherein the reduction rate of the rough rolling is 79%, and after the rolling is completed, the billet is layer-cooled, and then coiled at 701° C. to obtain a hot rolled billet with a thickness of 2.5 mm;
[0070] 3) uncoiling the hot-rolled slab obtained in step 2) and welding the hot-rolled slab, pickling it with a hydrochloric acid aqueous solution and then continuously cold rolling it at room temperature, wherein the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 18%, the cold rolling is lubricated by an emulsion, the temperature of the emulsion is 53° C., the saponification value of the emulsion is 181.75 mgKOH / g, the cold rolling reduction rate is 85%, and then coiling it at room temperature to obtain a cold-rolled slab with a thickness of 0.3 mm;
[0071] 4) The cold rolled billet obtained in step 3) is unrolled, washed with water, and annealed at a temperature of 835° C. for 75 seconds. After annealing, it is cooled in stages, first slowly cooled to 700° C. at a cooling rate of 3° C. / s, then quickly cooled to 410° C. at a cooling rate of 40° C. / s, and then aged at a temperature of 410° C. for 260 seconds. Then, it is cooled to 110° C., quenched in a water quenching tank, and then leveled and oiled on both sides at room temperature. The leveling reduction is 1.5% and the oiling amount is 350 mg / m 2 Then, the thin-gauge battery shell steel is coiled at room temperature to obtain the thin-gauge battery shell steel. The metallographic image of the thin-gauge battery shell steel is as follows: Figure 2 shown.
[0072] Example 3
[0073] This embodiment provides a method for preparing thin-gauge battery shell steel, comprising the following steps:
[0074] 1) Mixing the raw materials, smelting and refining in a converter, wherein the converter smelting temperature is 1642° C., the converter smelting time is 42 min, the refining includes LF refining and RH refining, wherein the LF refining temperature is 1603° C., the LF refining time is 35 min; the RH refining tapping temperature is 1580° C., the RH refining time is 12 min, and then continuous casting is performed at a pulling speed of 1.2 m / min to obtain a continuous casting billet, the thickness of the continuous casting billet is 220 mm; the components of the continuous casting billet, by mass percentage, are: C: 0.02%, Si: 0.01%, Mn: 0.10%, P: 0.008%, S: 0.003%, Als: 0.07%, Ti: 0.040%, and the rest are iron and unavoidable impurities;
[0075] 2) The continuous casting billet obtained in step 1) is subjected to surface peeling treatment and then heat treatment. The temperature of the continuous casting billet after the heat treatment is 1140° C. After being discharged from the furnace, hot rolling is performed. The hot rolling final rolling temperature T=1066*2(0.4-0.02%*100)±10° C. is determined according to the carbon content in the continuous casting billet, that is, the hot rolling final rolling temperature is determined to be 820° C. The hot rolling includes rough rolling and then finish rolling, wherein the reduction rate of the rough rolling is 83.6%. After the rolling is completed, the billet is layer-cooled and then coiled at 680° C. to obtain a hot rolled billet with a thickness of 2 mm;
[0076] 3) uncoiling the hot-rolled slab obtained in step 2) and welding the hot-rolled slab, pickling it with a hydrochloric acid aqueous solution and then continuously cold rolling it at room temperature, wherein the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 18%, the cold rolling is lubricated by an emulsion, the temperature of the emulsion is 55° C., the saponification value of the emulsion is 190.00 mgKOH / g, the cold rolling reduction rate is 87.5%, and then coiling it at room temperature to obtain a cold-rolled slab with a thickness of 0.25 mm;
[0077] 4) The cold rolled billet obtained in step 3) is unrolled, washed with water, annealed at 800°C for 130s, cooled in stages after annealing, first slowly cooled to 700°C at a cooling rate of 3°C / s, then rapidly cooled to 410°C at a cooling rate of 55°C / s, then aged at 410°C for 300s, then cooled to 120°C, quenched in a water quenching tank, then leveled at room temperature, oiled on both sides, leveled with a reduction of 1.0%, and oiled at 500mg / m 2 Then, the thin-gauge battery shell steel is coiled at room temperature to obtain the thin-gauge battery shell steel. The metallographic image of the thin-gauge battery shell steel is as follows: Figure 3 shown.
[0078] Example 4
[0079] This embodiment provides a method for preparing thin-gauge battery shell steel, comprising the following steps:
[0080] 1) Mixing the raw materials, smelting and refining them in a converter, wherein the converter smelting temperature is 1680° C., the converter smelting time is 60 min, the refining includes LF refining and RH refining, wherein the LF refining temperature is 1640° C., the LF refining time is 55 min, the RH refining tapping temperature is 1620° C., the RH refining time is 8 min, and then continuously casting is performed at a pulling speed of 1.4 m / min to obtain a continuous casting billet, the thickness of the continuous casting billet is 220 mm; the components of the continuous casting billet, by mass percentage, are: C: 0.03%, Si: 0.03%, Mn: 0.25%, P: 0.015%, S: 0.005%, Als: 0.05%, Ti: 0.021%, and the rest are iron and unavoidable impurities;
[0081] 2) The continuous casting billet obtained in step 1) is subjected to surface peeling treatment and then heat treatment. The temperature of the continuous casting billet after the heat treatment is 1180°C. After being discharged from the furnace, hot rolling is performed. The hot rolling final rolling temperature T=1066*2(0.4-0.03%*100)±10°C is determined according to the carbon content in the continuous casting billet, that is, the hot rolling final rolling temperature is determined to be 782°C. The hot rolling includes rough rolling and then finish rolling, wherein the reduction rate of the rough rolling is 78.2%. After the rolling is completed, the billet is layer-cooled and then coiled at 720°C to obtain a hot rolled billet with a thickness of 2.5 mm;
[0082] 3) uncoiling the hot-rolled slab obtained in step 2) and welding the hot-rolled slab, pickling it with a hydrochloric acid aqueous solution and then continuously cold rolling it at room temperature, wherein the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 18%, the cold rolling is lubricated by an emulsion, the temperature of the emulsion is 55° C., the saponification value of the emulsion is 180.00 mgKOH / g, the cold rolling reduction rate is 84%, and then coiling it at room temperature to obtain a cold-rolled slab with a thickness of 0.4 mm;
[0083] 4) The cold rolled billet obtained in step 3) is unrolled, washed with water, and annealed at a temperature of 850° C. for 130 seconds. After annealing, it is cooled in stages, first slowly cooled to 680° C. at a cooling rate of 4° C. / s, then quickly cooled to 420° C. at a cooling rate of 45° C. / s, and then aged at a temperature of 420° C. for 220 seconds. Then, it is cooled to 140° C., quenched in a water quenching tank, and then leveled and oiled on both sides at room temperature. The leveling reduction is 1.5% and the oiling amount is 500 mg / m 2 , and then coiled at room temperature to obtain the thin-gauge battery shell steel.
[0084] Comparative Example 1
[0085] This comparative example provides a method for preparing thin-gauge steel for battery shells, which differs from Example 1 in that the final hot rolling temperature in step 2) is 860°C.
[0086] The obtained thin gauge battery shell steel metallographic image is as follows Figure 4 shown.
[0087] Comparative Example 2
[0088] This comparative example provides a method for preparing thin-gauge steel for battery shells, which differs from Example 1 in that the annealing temperature in step 4) is 770°C.
[0089] Comparative Example 3
[0090] This comparative example provides a method for preparing thin-gauge battery shell steel, which is different from Example 1 in that, in step 4), the cold-rolled billet obtained in step 3) is unrolled and then washed with water, annealed, the annealing temperature is 835°C, the annealing time is 75s, and after annealing, the layer is cooled to room temperature and then flattened and oiled on both sides, the flattening reduction is 1.2%, and the oiling amount is 400mg / m 2 , and the thin-gauge steel for battery shell is obtained by winding at room temperature.
[0091] Comparative Example 4
[0092] This comparative example provides a method for preparing thin-gauge steel for battery shells, which is different from Example 1 in that, compared with the continuous casting billet described in step 1), its components, by mass percentage, are: C: 0.0023%, Si: 0.012%, Mn: 0.38%, P: 0.011%, S: 0.004%, Als: 0.058%, Ti: 0.051%, and the rest are iron and unavoidable impurities.
[0093] Test Case
[0094] The thin-gauge battery shell steel obtained in Examples 1-4 and Comparative Examples 1-4 was tested. The lower yield strength, tensile strength and elongation after fracture in the forming performance were determined with reference to the standard GB / T228-2021. The test results are shown in Table 1. The higher the elongation after fracture, the better the forming performance; the thin-gauge battery shell steel obtained in Examples 1-4 and Comparative Examples 1-4 was tested for △r value. The test reference standard GB / T228-2021 was used, and the test results were expressed in absolute values as shown in Table 1. The smaller the absolute value of △r, the better, indicating that the material has uniform properties in all directions, which is more uniform during stamping deformation and is not easy to produce "ear-making" defects. When the absolute value of △r exceeds 0.3, it is more likely to produce "ear-making" defects.
[0095] The thin-gauge battery shell steel obtained in Examples 1-4 and Comparative Examples 1-4 was placed on a battery shell mold and punched into a cylindrical battery shell with a diameter of 65 cm. Under the condition of a punching speed of 100 passes / minute, 9 passes were punched to reach a punching depth of 6.5 cm. The thin-gauge battery shell steel obtained in Examples 1-4 and Comparative Examples 1-4 were used to punch 10,000 cylindrical battery shells, respectively. At the same time, the surface scratch rate, crack rate, sand hole rate and ear rate of the 10,000 cylindrical battery shells corresponding to Examples 1-4 and Comparative Examples 1-4 were counted in real time. The test results are shown in 1. The lower the crack rate, the better the forming performance and the less wear on the mold.
[0096] Table 1
[0097]
[0098]
[0099] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing thin-gauge battery shell steel, It is characterized in that The following steps are involved: 1) Mixing raw materials, smelting and continuously casting to obtain continuous casting billets; The continuous casting billet comprises, by mass percentage, the following components: C: 0.02-0.03%, Si: 0.01-0.03%, Mn: 0.10-0.25%, P≤0.015%, S≤0.015%, Als: 0.05-0.07%, Ti: 0.021-0.040%, and the rest is iron and unavoidable impurities; 2) heating, hot rolling, cooling and coiling the continuous casting billet obtained in step 1) to obtain a hot rolled billet; The relationship between the final rolling temperature of the hot rolling and the carbon content in the continuous casting billet is T=1066*2(0.4-M*100)±10°C, where T is the final rolling temperature and M is the mass percentage of carbon in the continuous casting billet; 3) uncoiling the hot-rolled billet obtained in step 2), pickling it, and cold rolling it to obtain a cold-rolled billet; 4) annealing the cold-rolled billet obtained in step 3) at 800-850° C., and then cooling in stages, performing aging treatment, and water quenching treatment to obtain the thin-gauge battery shell steel.
2. The method for preparing the thin-gauge battery shell steel according to claim 1, It is characterized in that The smelting in step 1) includes converter smelting and refining; The converter smelting temperature is 1640-1680°C, and the converter smelting time is 40-60min; In step 1), the continuous casting speed is 1.0-1.5 m / min; The continuous casting billet has a thickness of 180-220 mm; Optionally, the refining includes LF refining and RH refining; The LF refining tapping temperature is 1600-1640°C, and the LF refining time is 35-55min; The RH refining tapping temperature is 1570-1620° C., and the RH refining time is 8-12 minutes.
3. A method for preparing thin-gauge battery shell steel according to claim 1 or 2, It is characterized in that In step 2), the continuous casting billet obtained in step 1) is heated to a temperature of 1130-1180° C. after being taken out of the furnace, and hot rolling is performed after being taken out of the furnace; The hot rolling process includes rough rolling and finish rolling; Optionally, the pressing rate of the rough rolling is 75%-85%; Optionally, the heating step in step 2) further includes a surface peeling treatment of the continuous casting billet.
4. A method for preparing thin-gauge battery shell steel according to any one of claims 1 to 3, It is characterized in that The thickness of the hot rolled billet in step 2) is 1.8-3.0 mm; The coiling temperature in step 2) is 660-720°C.
5. A method for preparing thin-gauge battery shell steel according to any one of claims 1 to 4, It is characterized in that The pickling agent for pickling in step 3) is a hydrochloric acid aqueous solution; Optionally, the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 10-20%.
6. A method for preparing thin-gauge battery shell steel according to any one of claims 1 to 5, It is characterized in that The cold rolling reduction rate in step 3) is 75-87.5%; The cold rolling process uses emulsion lubrication, and the saponification value of the emulsion is 180-190 mgKOH / g; Optionally, the thickness of the cold-rolled billet is ≤0.4 mm; Optionally, after the cold rolling step in step 3) is completed, a coiling step is also included.
7. A method for preparing thin-gauge battery shell steel according to any one of claims 1 to 6, It is characterized in that The annealing time in step 4) is 60-360s; The segmented cooling in step 4) includes slow cooling and fast cooling; The cooling rate of the slow cooling section is 2-5°C / s, and the slow cooling section is cooled to 680-700°C; The cooling rate of the rapid cooling section is 40-60°C / s, and the rapid cooling section cools to 380-420°C.
8. A method for preparing thin-gauge battery shell steel according to any one of claims 1 to 7, It is characterized in that The aging treatment temperature in step 4) is 380-420°C, and the aging treatment time is 220-300s; After the aging treatment in step 4) is completed, a cooling treatment is also included, and water quenching treatment is performed after cooling to 100-140°C; Optionally, the step 4) further includes a cleaning step before the annealing step; Optionally, after the water quenching step in step 4), the steps of leveling, oiling and coiling are also included.
9. A thin gauge steel for battery shells, It is characterized in that The thin-gauge battery shell steel is prepared by the preparation method of any one of claims 1 to 8.
10. Use of the thin-gauge battery shell steel according to claim 9 in a battery shell.
Citation Information
Patent Citations
High-r-value thick-specification IF automotive steel and production method thereof
CN104120337A
Production method for steel for deep drawing of battery case
CN106148803A
Pure steel belt for electric vehicle battery and preparation method of pure steel belt
CN109321842A
Cold-rolled steel sheet for battery case with tensile strength of 320 MPa and production method of cold-rolled steel sheet
CN114107833A
Low-carbon steel with high yield ratio and high ductility and toughness and preparation method thereof