Preparation method of high-speed steel roller with high accident resistance

By using raw materials such as pig iron to prepare the roll outer alloy and performing incubation and heat treatment, an accident-resistant graphite phase is formed, which solves the problem of insufficient wear resistance and accident-resistant properties of high-speed steel rolls in hot-rolled strips and steel rolling lines. Significantly improves the performance and use effect of the roll.

CN119061312APending Publication Date: 2024-12-03SINOSTEEL XINGTAI MACHINERY & MILL ROLL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410956687.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing high-speed steel rolling rolls have problems of insufficient wear resistance and accident resistance in hot-rolled strips and steel rolling lines, especially in terms of tail-flip sticking steel and roll surface cracks.

Method used

The roll outer alloy is prepared by raw materials such as pig iron, nickel iron, ferrous vanadium, ferrochromium, and ferromolybdenum. Through incubation and heat treatment technology, a graphite phase with high wear resistance and accident resistance is formed, which improves the roll's thermal crack resistance and resistance. Accidentality.

Benefits of technology

It significantly improves the wear resistance and accident resistance of the rolling roll, solves the problems of hot cracks and block drops in the rolling surface of hot-rolled plate and steel rolling lines, and improves the rolling line efficiency and finished product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061312A_ABST
    Figure CN119061312A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-speed steel roller with high accident resistance, which belongs to the field of roller preparation, and comprises the following steps: taking alloy and other materials as raw materials, so that the alloy components of the outer layer of the roller comprise 2.3-6.0% of C, 1.0-6.0% of Si, 0.3-1.0% of Mn, less than or equal to 0.10% of P, less than or equal to 0.1% of S, 1.0-8.0% of Cr, 2.0-5.0% of Ni, 0.5-6.0% of Mo, 0.5-6.0% of V, 0.5-3.0% of W, 0.5-2.0% of Nb and the balance of Fe; discharging after the components reach the standard, and performing inoculation treatment in the discharging process; pouring by adopting an integral or centrifugal composite mode, and after pouring is finished, carrying out cold box opening at the mold temperature of less than or equal to 60 DEG C; rough machining is conducted on the casting blank after box opening, and heat treatment is conducted after rough machining is completed; and after heat treatment is finished, performing subsequent processing until a finished product is obtained. The prepared roller can meet the requirements of high wear resistance and high accident resistance of a rolling line.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of roller preparation, in particular to a method for preparing a high-speed steel roller with high accident resistance. Background Art

[0002] With the rapid development of hot-rolled strip and section steel rolling lines, the performance requirements for rolls (rings) are getting higher and higher. The emergence and continuous development of high-speed steel rolls on the entire line have complied with the application requirements of rolls in the hot rolling field. However, the finishing mill frame is affected by the special working conditions and the further improvement of the rolling line efficiency is affected. The hot-rolled strip finished product frame has tail swinging and steel sticking, and conventional high-speed steel materials cannot be used. The section steel rolling line uses conventional high-speed steel and has the problem of roll surface cracks. Therefore, there is an urgent need for a highly wear-resistant and highly accident-resistant material with good wear resistance, thermal cracking resistance and accident resistance to adapt to special working conditions. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a high-speed steel roller with high accident resistance. The outer layer of the roller forms a highly wear-resistant material with a graphite phase, which has high wear resistance, high accident resistance and thermal cracking resistance, which not only meets the requirements of high wear resistance and high accident resistance of the rolling line, but also meets the plate surface quality.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0005] A method for preparing a high-speed steel roll with high accident resistance comprises the following steps:

[0006] Step A, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, so that the alloy composition and range of the outer layer of the roller are: C2.3-6.0%, Si1.0-6.0%, Mn0.3-1.0%, P≤0.10%, S≤0.1%, Cr1.0-8.0%, Ni2.0-5.0%, Mo0.5.0-6.0%, V0.5-6.0%, W0.5-3.0%, Nb0.5-2.0%, and the balance is Fe;

[0007] Step B, after the ingredients in step A meet the standards, the product is taken out of the furnace, and inoculation treatment is performed during the process;

[0008] Step C, casting is performed by integral or centrifugal compound method, and after casting, the mold temperature is ≤60°C and the box is opened cold;

[0009] Step D, rough processing is performed on the ingot after unpacking, and heat treatment is performed after the rough processing is completed;

[0010] Step E: After the heat treatment is completed, subsequent processing is performed until the finished product is obtained.

[0011] A further improvement of the technical solution of the present invention is that in step A and step B, the melting temperature of the molten steel of the outer layer of the rolling mill is 1400-1700°C, and it is taken out of the furnace when it is heated to a temperature of 1500-1800°C by power supply, and poured when the temperature drops to 1320-1410°C, and inoculation treatment is performed during the process of taking out of the furnace and pouring.

[0012] A further improvement of the technical solution of the present invention is that in step A, the proportion of scrap steel and scrap rollers in the raw materials is ≤10%, wherein Cr+Mo+V+W+Nb≥7%.

[0013] A further improvement of the technical solution of the present invention is that in step A, the high temperature insulation time of the raw materials needs to be ≥20 minutes.

[0014] A further improvement of the technical solution of the present invention is that in step B, the amount of Si added after the inoculant is added during the inoculation treatment accounts for more than 30% of the total Si content.

[0015] A further improvement of the technical solution of the present invention is that in step B, during the inoculation treatment, the inoculation during the discharge process requires that the inoculant be added to 1 / 5-5 / 4 of the amount of molten steel discharged.

[0016] A further improvement of the technical solution of the present invention is that in step B, during the inoculation process, the inoculant is any two of SiFe, SiBa, and FeMn.

[0017] A further improvement of the technical solution of the present invention is that the amount of the inoculant added is 2%-2.4% of the weight of the molten steel.

[0018] A further improvement of the technical solution of the present invention is that: in step C, when centrifugal casting is adopted, the casting needs to be placed in a sealed space for cooling after the casting is completed; after the overall casting is completed, carbonized rice husks are sprinkled into the riser for heat preservation.

[0019] A further improvement of the technical solution of the present invention is that in step D, the heat treatment method is high-temperature diffusion annealing, the annealing temperature is 1000-1050°C, the holding time is based on the minimum wall thickness Lmm / 50h, and after the holding is completed, the temperature is slowly reduced to 600°C at a rate of 10-20°C / h and the holding time is based on the minimum wall thickness Lmm / 100h. After the holding is completed, the temperature is increased to 1000-1100°C and held again, and the holding time is based on the minimum wall thickness Lmm / 50h. After the holding is completed, the steel is cooled by blowing, cooled to 450-500°C, and then charged into the furnace for tempering, with a tempering temperature of 400-600°C.

[0020] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:

[0021] The present invention improves the accident resistance of high-performance rollers (rings) used for hot rolling and section steel rolling lines by adding a large amount of alloy, and at the same time, uses an inoculant to produce a lubricating phase and accident-resistant graphite. The developed material with high wear resistance and good accident resistance can be applied to the steel rolling industry, especially to solve the problems of roller surface thermal cracks and block falling caused by tail swinging and steel sticking in the hot-rolled plate and strip finished product rack. At the same time, the good thermal conductivity of graphite can also solve the roller ring thermal crack problem caused by using conventional high-speed steel in the finishing rolling universal rack of the section steel rolling line. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 This is a graphite image of the roller outer layer before corrosion prepared in Example 1 of the present invention;

[0024] Figure 2 This is a diagram of the matrix structure of the roller after the outer layer is corroded according to Example 1 of the present invention. DETAILED DESCRIPTION

[0025] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or apparatus.

[0026] The present invention is further described in detail below with reference to the accompanying drawings and embodiments:

[0027] A method for preparing a high-speed steel roll with high accident resistance comprises the following steps:

[0028] Step A, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, so that the alloy composition and range of the outer layer of the roller are: C2.3-6.0%, Si1.0-6.0%, Mn0.3-1.0%, P≤0.10%, S≤0.1%, Cr1.0-8.0%, Ni2.0-5.0%, Mo0.5.0-6.0%, V0.5-6.0%, W0.5-3.0%, Nb0.5-2.0%, and the balance is Fe; the core material of the roller is conventional material and conventional smelting, casting, inoculation and other methods;

[0029] The proportion of scrap steel and scrap rollers in the raw materials is ≤10%, of which Cr+Mo+V+W+Nb is ≥7%.

[0030] The melting temperature of the outer layer of the roller is 1400-1700℃. It is heated to 1500-1800℃ and then taken out of the furnace. When the temperature drops to 1320-1410℃, it is poured. Inoculation treatment is carried out during the process of taking out of the furnace and pouring.

[0031] The high temperature insulation time of raw materials needs to be ≥20min.

[0032] Step B, after the ingredients in step A meet the standards, the product is taken out of the furnace, and inoculation treatment is performed during the process;

[0033] During the inoculation treatment, the amount of Si added after the addition of the inoculant accounts for more than 30% of the total Si content;

[0034] During the inoculation treatment, the inoculation during the furnace discharge process requires that the inoculant be added between 1 / 5-5 / 4 of the amount of molten steel discharged;

[0035] During the inoculation process, the inoculant is any two of SiFe, SiBa, and FeMn;

[0036] The amount of inoculant added is 2%-2.4% of the weight of the molten steel.

[0037] Step C, casting is performed by integral or centrifugal compound method, and after casting, the mold temperature is ≤60°C and the box is opened cold;

[0038] When centrifugal casting is adopted, it needs to be placed in a sealed space for cooling after the casting is completed; after the overall casting is completed, carbonized rice husks are sprinkled into the riser for insulation.

[0039] Step D, rough processing is performed on the ingot after unpacking, and heat treatment is performed after the rough processing is completed;

[0040] The heat treatment method is high-temperature diffusion annealing, the annealing temperature is 1000-1050℃, the holding time is based on the minimum wall thickness Lmm / 50h, after the holding is completed, the temperature is slowly reduced to 600℃ at a rate of 10-20℃ / h, and the holding time is based on the minimum wall thickness Lmm / 100h. After the holding is completed, the temperature is increased to 1000-1100℃ and held again, and the holding time is based on the minimum wall thickness Lmm / 50h. After the holding is completed, it is cooled by blowing, cooled to 450-500℃ and charged into the furnace for tempering, and the tempering temperature is 400-600℃.

[0041] Step E: After the heat treatment is completed, subsequent processing is performed until the finished product is obtained.

[0042] Example 1

[0043] A method for preparing a high-speed steel rolling roll with high accident resistance, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, adopting an industrial frequency furnace for smelting, and reaching a designed composition range: the outer layer molten iron contains C2.3%, Si6.0%, Mn0.3%, P0.03%, S0.06%, Cr1.0%, Ni3.23%, Mo1.69%, V0.5%, W3.0%, Nb2.0%, and the balance is Fe; the core molten iron contains C4.96%, Si1.5%, Mn0.13%, P0.05%, S0.04%, Cr0.13%, Ni0.1%, Mo0.1%, and the balance is Fe. The outer layer is melted at a temperature of 1501°C, and after the components are leveled, it is kept warm for 30 minutes, and the temperature is raised to 1600°C and taken out of the furnace. The pre-baked red-hot ladle is taken out of the furnace, and the temperature is reduced to 1450°C for centrifugal pouring. 1% SiFe+1% SiBa inoculant is added when it is taken out of the furnace. The core molten steel is melted at a temperature of 1320°C and taken out of the furnace. The pouring temperature is 1250°C. 1% rare earth magnesium is added to the bottom of the ladle when the core is taken out of the furnace. 0.5% SiFe and 0.5% SiBa spheroidizer and inoculant are added during the pouring process. The spheroidizer is added after being put into an aluminum barrel and sealed; the box is opened cold 73 hours after the pouring is completed, and roughing and heat treatment are completed after cold opening until the finished product.

[0044] Example 2

[0045] A method for preparing a high-speed steel rolling roll with high accident resistance, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, adopting an industrial frequency furnace for smelting, and reaching a designed composition range: the outer layer molten iron has C6.0%, Si1.3%, Mn1.0%, P0.02%, S0.04%, Cr3.21%, Ni3.8%, Mo1.51%, V2.16%, W0.85%, Nb0.5, and the balance is Fe; the core molten iron has C4.63%, Si1.35%, Mn0.11%, P0.05%, S0.04%, Cr0.14%, Ni0.21%, Mo0.15%, and the balance is Fe. The outer layer is melted at a temperature of 1506°C, and the components are kept warm for 25 minutes after being leveled. The temperature is raised to 1610°C and taken out of the furnace. The pre-baked red-hot ladle is turned over and taken out of the furnace. The temperature is reduced to 1440°C for centrifugal pouring. 1.1% SiFe+1.3% FeMn inoculant is added when taking out of the furnace. The core molten steel is melted at a temperature of 1330°C and taken out of the furnace. The pouring temperature is 1260°C. 1.2% rare earth magnesium is added to the bottom of the ladle when the core is taken out of the furnace. 0.55% SiFe and 0.55% SiBa spheroidizer and inoculant are added during the pouring process. The spheroidizer is added after being sealed in an aluminum barrel. The box is opened cold for 80 hours after pouring. After the box is opened cold, roughing and heat treatment are completed until the finished product.

[0046] Example 3

[0047] A method for preparing a high-speed steel roller with high accident resistance, using pig iron, nickel iron, vanadium iron, chromium iron, molybdenum iron and niobium iron as raw materials, adopting industrial frequency furnace smelting to reach the designed composition range: outer layer molten iron C4.9%, Si1.0%, Mn0.51%, P0.02%, S0.04%, Cr3.21%, Ni5.0%, Mo1.5%, V1.5%, W0.85%, Nb0.5, and the balance is Fe. Melting at a temperature of 1506℃, keeping the temperature for 29 minutes after the components are leveled, heating to 1630℃ and taking out of the furnace, using the pre-baked red hot state to turn the bag out of the furnace, and lowering the temperature to 1470℃ for integral casting, adding 1.2% SiFe+0.9% FeMn inoculant when taking out of the furnace; the core material of the roller, the smelting, casting, inoculation and other methods are the same as those in Example 1; cold unpacking for 85 hours after the casting is completed, and roughing and heat treatment are completed after cold unpacking until the finished product.

[0048] Example 4

[0049] A method for preparing a high-speed steel roller with high accident resistance, using pig iron, nickel iron, vanadium iron, chromium iron, molybdenum iron and niobium iron as raw materials, adopting industrial frequency furnace smelting to reach the designed composition range: outer layer molten iron C4.85%, Si6.0%, Mn0.53%, P0.03%, S0.02%, Cr8.0%, Ni3.15%, Mo0.5%, V6.0%, W0.5%, Nb0.5, and the balance is Fe. Melting at a temperature of 1501°C, keeping the temperature for 22 minutes after the components are leveled, heating to 1610°C and taking out of the furnace, using the pre-baked red hot state to turn the bag out of the furnace, and the temperature is reduced to 1420°C for integral casting, and adding 0.8% SiFe+1.6% FeMn inoculant when taking out of the furnace; the core material of the roller, the smelting, casting, inoculation and other methods are the same as those in Example 1; cold unpacking for 80 hours after the casting is completed, and roughing and heat treatment are completed after cold unpacking until the finished product.

[0050] Example 5

[0051] A method for preparing a high-speed steel rolling mill roll with high accident resistance, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, adopting an industrial frequency furnace for smelting to reach a designed composition range: the outer layer of molten iron has C4.52%, Si1.83%, Mn0.51%, P0.04%, S0.03%, Cr3.25%, Ni3.16%, Mo1.57%, V2.11%, W0.85%, Nb0.5, and the balance is Fe. The material is melted at 1502°C, kept warm for 25 minutes after the components are evened out, and then the temperature is raised to 1650°C for taking out of the furnace. The material is taken out of the furnace in a red-hot state after being baked in advance, and the temperature is lowered to 1430°C for integral pouring. When taking out of the furnace, 0.9% SiFe + 1.2% FeMn inoculant is added. The core material of the roll is melted, poured, and inoculated in the same manner as in Example 1. The material is opened cold for 70 hours after pouring, and roughing and heat treatment are completed after cold opening until the finished product is obtained.

[0052] Example 6

[0053] A method for preparing a high-speed steel roller with high accident resistance, using pig iron, nickel iron, vanadium iron, chromium iron, molybdenum iron and niobium iron as raw materials, adopting industrial frequency furnace smelting to reach the designed composition range: outer layer molten iron C4.75%, Si1.96%, Mn0.41%, P0.03%, S0.02%, Cr2.15%, Ni2.0%, Mo6.0%, V2.15%, W0.84%, Nb0.51, and the balance is Fe. Melting at a temperature of 1501°C, keeping the temperature for 21 minutes after the components are leveled, heating to 1640°C and taking out of the furnace, using the pre-baked red hot state to turn the bag out of the furnace, and the temperature is reduced to 1420°C for integral casting, and 0.8% SiFe+1.3% FeMn inoculant is added when taking out of the furnace; the core material of the roller, the smelting, casting, inoculation and other methods are the same as those in Example 1; cold opening after pouring for 71 hours, and roughing and heat treatment are completed after cold opening until the finished product.

[0054] Example 7

[0055] A method for preparing a high-speed steel roller with high accident resistance, using pig iron, nickel iron, vanadium iron, chromium iron, molybdenum iron and niobium iron as raw materials, adopting industrial frequency furnace smelting to reach the designed composition range: outer layer molten iron C1.51%, Si1.96%, Mn0.41%, P0.03%, S0.02%, Cr2.15%, Ni2.0%, Mo6.0%, V2.15%, W0.84%, Nb0.51, and the balance is Fe. Melting at a temperature of 1501°C, keeping the temperature for 21 minutes after the components are leveled, heating to 1640°C and taking out of the furnace, using the pre-baked red hot state to turn the bag out of the furnace, the temperature is reduced to 1420°C for integral casting, and 0.8% SiFe+1.3% FeMn inoculant is added when taking out of the furnace; the core material of the roller, the smelting, casting, inoculation and other methods are the same as those in Example 1; cold opening after pouring for 71 hours, and roughing and heat treatment are completed after cold opening until the finished product.

[0056] The roller products prepared in Examples 1 to 7 were taken for sample tensile mechanical property testing, and the performance testing was carried out in accordance with the national standard GB / T228. The test results are shown in Table 1.

[0057] Table 1 Example product performance test results

[0058]

[0059] The graphite image of the roller outer layer before corrosion prepared in Example 1 is as follows: Figure 1 As shown, the black phase is graphite (graphite is Figure 1 The black dots in the figure), the matrix structure diagram of the roll after the outer layer corrosion prepared in Example 1 is as follows Figure 2As shown, the white phase is carbide, which is dispersed, the matrix is ​​gray, the structure is martensite + carbide, and the matrix has good resistance to thermal cracking.

[0060] It can be seen from the data in Table 1 that Example 7 has a low carbide content and fails to effectively precipitate graphite under high alloy conditions, resulting in the failure resistance and surface quality being inferior to those of Examples 1-6.

[0061] The rollers prepared in Examples 1-6 were subjected to test rolling in the rear section of hot rolling, especially in the finished product stand, and the machine wear was reduced by more than 50%, and the millimeter rolling amount was increased to more than twice that of the high nickel-chromium working rollers; at the same time, in the test rolling on the universal stand of the steel rolling line, the steel passing amount reached 1.5 times that of semi-steel, solving the problem of steel sticking to the bottom of the universal roller ring groove.

[0062] According to the performance test results, the high accident resistance and high wear resistance roll prepared by the present invention is applied to the roll rings of hot rolling and section steel rolling lines to good effect.

[0063] In addition, the upper and lower limits and interval values ​​of the process parameters (such as component content, time, temperature, ratio, dosage, etc.) of the present invention can all achieve the present invention, and the embodiments are not listed one by one here.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a high-speed steel roll with high accident resistance, characterized in that: The following steps are involved: Step A, using pig iron, ferronickel, ferrovanadium, ferrochrome, ferromolybdenum and ferroniobium as raw materials, so that the alloy composition and range of the outer layer of the roller are: C2.3-6.0%, Si1.0-6.0%, Mn0.3-1.0%, P≤0.10%, S≤0.10%, Cr1.0-8.0%, Ni2.0-5.0%, Mo0.5.0-6.0%, V0.5-6.0%, W0.5-3.0%, Nb0.5-2.0%, and the balance is Fe; Step B, after the ingredients in step A meet the standards, the product is taken out of the furnace, and inoculation treatment is performed during the process; Step C, casting is performed by integral or centrifugal compound method, and after casting, the mold temperature is ≤60°C and the box is opened cold; Step D, rough processing is performed on the ingot after unpacking, and heat treatment is performed after the rough processing is completed; Step E: After the heat treatment is completed, subsequent processing is performed until the finished product is obtained.

2. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step A and step B, the melting temperature of the molten steel of the outer layer of the roller is 1400-1700°C, and the steel is taken out of the furnace when it is heated to 1500-1800°C by electricity, and poured when the temperature drops to 1320-1410°C. Inoculation treatment is performed during the process of taking out of the furnace and pouring.

3. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step A, the proportion of scrap steel and scrap rollers in the raw materials is ≤10%, wherein Cr+Mo+V+W+Nb≥7%.

4. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step A, the raw materials must be kept at high temperature for ≥ 20 min.

5. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step B, the amount of Si added after the inoculant is added during the inoculation treatment accounts for more than 30% of the total Si content.

6. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step B, during the inoculation treatment, the inoculation during the outflow process requires that the inoculant be added in the flow between 1 / 5-5 / 4 of the amount of molten steel out of the furnace.

7. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step B, during the inoculation process, the inoculant is any two of SiFe, SiBa, and FeMn.

8. The method for preparing a high-speed steel roll with high accident resistance according to claim 7, characterized in that: The amount of inoculant added is 2%-2.4% of the weight of the molten steel.

9. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step C, when centrifugal casting is adopted, the casting needs to be placed in a sealed space for cooling after the casting is completed; after the overall casting is completed, carbonized rice husks are sprinkled into the riser for heat preservation.

10. The method for preparing a high-speed steel roll with high accident resistance according to claim 1, characterized in that: In step D, the heat treatment method is high-temperature diffusion annealing, the annealing temperature is 1000-1050°C, the holding time is based on the minimum wall thickness Lmm / 50h, after the holding is completed, the temperature is slowly reduced to 600°C at a rate of 10-20°C / h and the holding time is based on the minimum wall thickness Lmm / 100h, after the holding is completed, the temperature is increased to 1000-1100°C and held again, the holding time is based on the minimum wall thickness Lmm / 50h, after the holding is completed, the air is blown to cool, cooled to 450-500°C and charged into the furnace for tempering, and the tempering temperature is 400-600°C.

Citation Information

Cited By

  • Preparation method of wear-resistant high-speed steel plate strip roller

    CN120984854A