Low-yield-ratio steel plate with excellent low-temperature toughness of-150 DEG C and manufacturing method thereof
By optimizing chemical composition and heat treatment process, a low yield strength steel plate containing nickel was designed to form granular bainite and slat martensite structures, which solved the low temperature toughness and flexion of low temperature steel materials below -100°C in the existing technology The problem of difficult to take into account both the strong ratio has achieved a low-temperature steel plate with high deformation margin and safety at -150℃, which is suitable for the storage and transportation of low-temperature liquefied gas.
Patent Information
- Application Number
- CN202310624013.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
It is difficult for existing low-temperature steel materials to achieve good low-temperature toughness and low yield-strength ratio at the same time below -100℃, resulting in a lack of sufficient deformation margin and safety in low-temperature environments.
By optimizing chemical composition and heat treatment process, a low yield strength steel plate containing nickel was designed, with components of C 0.03 to 0.08%, Si 0.10 to 0.25%, Mn 0.3 to 0.8%, S≤0.005%, P≤0.006%, Ni 4.6~5.5%, Mo≤0.10%, Al≤0.05%, and 40~70% of granular bainite and 30~60% of laminated martensite tissue were formed by rolling and tempering heat treatment, and the cooling speed was controlled. and tempering temperature to obtain excellent low temperature toughness and low yield strength ratio.
The high deformation margin and safety of steel plates at -150℃ are achieved, with yield strength greater than 390MPa, tensile strength 530~710MPa, elongation greater than 20%, impact absorption energy at -150℃ is above 200J, yield strength ratio reaches Below 0.85, meets the safety needs of low-temperature liquefied gas storage and transportation.
Smart Images

Figure CN119061326A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of low-temperature steel, and in particular to a low-yield ratio steel plate with excellent low-temperature toughness at -150°C and a manufacturing method thereof. Background Art
[0002] The development of today's social economy requires more and more containers, ships, storage tanks, etc. for the storage and transportation of low-temperature liquefied gases. The temperatures of these liquefied gases are much lower than room temperature, such as liquefied ethane, which is an important raw material for the petrochemical industry, at -89°C, liquefied ethylene at -104°C, and the newly emerging liquefied carbon dioxide for carbon reduction purposes. These liquefied gas storage and transportation devices need to be made of special nickel-containing low-temperature steel, which needs to have good low-temperature toughness at the corresponding low temperature to ensure safety. In addition, due to the changes in loads during sea or land transportation, and the alternation of loading and unloading during storage, especially these changes occur in low-temperature environments, there must be a large deformation reserve and margin before fracture failure, so the upper limit of the material's yield strength ratio is limited to further enhance safety.
[0003] Chinese patent CN114855060A discloses a pipeline steel with a yield ratio of ≤0.85, whose chemical composition is carbon: 0.035-0.045, silicon: 0.10-0.20, manganese: 1.63-1.68, phosphorus ≤0.012, sulfur ≤0.0015, niobium: 0.052-0.056, titanium: 0.012-0.018, aluminum ≤0.015, nickel: 0.10-0.13, chromium: 0.15-0.20, molybdenum: 0.10-0.12, copper: 0.12-0.15. Its final rolling temperature is 770-810℃, online quenching is adopted, and the cooling rate is 25-35℃ / s, achieving a low-temperature impact toughness of -40℃ ≥210J.
[0004] Chinese patent CN114875311A discloses a steel for marine engineering with a low yield ratio of ≤0.83 and a manufacturing method thereof. The chemical composition of the steel is C: 0.06%-0.08%, Si: 0.18%-0.35%, Mn: 1.50%-1.65%, Cr: 0.1%-0.2%, Mo: 0.1%-0.15%, Ni: 0.20%-0.30%, Nb: 0.025%-0.035%, Alt: 0.02%-0.03%, Zr: 0.01%-0.015%, Cu: 0.05%-0.20%, P≤0.013%, S≤0.002%. After rolling, laminar cooling is used for cooling, the cooling rate is 10-15℃ / s, the water inlet temperature is 550-700℃, and the red-return temperature is 300-500℃. After rolling, the steel plate is subjected to quenching at 900-950℃ and tempering at 550-650℃. After heat preservation, it is cooled in a laminar flow manner. The structure of the steel is a dual-phase structure consisting of bainite and a small amount of ferrite. The low-temperature impact toughness of -40℃ is ≥400J.
[0005] Chinese patent CN109777938A adopts stainless steel with a dual-phase structure design, and the components and contents (wt%) are: C: 0.02, Cr: 25.22, Ni: 7.15, Mo: 3.94, N: 0.27, Mn: 0.63, Si: 0.48, Cu: 0.22; the rest are Fe and unavoidable impurities. Through solution heat treatment at 1020-1100℃, the relative proportion of ferrite and austenite is regulated and the austenite content is controlled at 46-50%. Although the invention adds a higher alloy, the impact absorption energy does not exceed 100J at -100℃.
[0006] At present, most nickel-containing low-temperature steels are manufactured using a quenching and tempering heat treatment process. Martensite or bainite structures are obtained through high-temperature quenching. There are fine substructure units inside, which are conducive to hindering crack propagation. Although this method is easy to obtain good low-temperature toughness, this process and organizational design can easily lead to an increase in the yield strength of the material, making the yield strength ratio high. On the other hand, a common method to obtain a low yield ratio is to use dual-phase steel, which contains two phase structures: ferrite and martensite. When loaded and deformed, the softer ferrite deforms first, while the harder martensite can ensure a higher fracture strength. The combined effect of the two achieves a low yield ratio. However, the ferrite grain size in dual-phase steel is large, and the internal substructure is lacking, which cannot resist crack cleavage propagation, and it is difficult to achieve good toughness at low temperatures below -100°C. Therefore, it is a common problem in material design and manufacturing to achieve low-temperature toughness and low yield ratio simultaneously. Summary of the invention
[0007] The object of the present invention is to provide a low yield ratio steel plate with excellent low temperature toughness at -150°C and a manufacturing method thereof. The steel plate has both excellent low temperature toughness and low yield ratio, and has a high deformation margin in a low temperature environment of not less than -150°C, thereby having high service safety; the steel plate has a yield strength greater than 390MPa, a tensile strength of 530-710MPa, an elongation greater than 20%, an impact absorption energy of more than 200J at -150°C, and a yield ratio of less than 0.85, and is suitable for the construction of cryogenic containers, ships and storage tanks.
[0008] To achieve the above object, the technical solution of the present invention is:
[0009] A low yield strength ratio steel plate with excellent low temperature toughness at -150°C, the weight percentage of its components is:
[0010] C 0.03~0.08%;
[0011] Si 0.10~0.25%;
[0012] Mn 0.3~0.8%;
[0013] S≤0.005%;
[0014] P≤0.006%;
[0015] Ni 4.6~5.5%;
[0016] The balance contains Fe and other inevitable impurities.
[0017] Preferably, the balance is Fe and other inevitable impurities.
[0018] Preferably, it further contains Mo≤0.10wt%, and / or Al≤0.05wt%.
[0019] The microstructure of the low yield ratio steel plate of the present invention is that the proportion of granular bainite is 40-70% and the proportion of lath martensite is 30-60%.
[0020] The low yield strength ratio steel plate of the present invention has a yield strength greater than 390MPa, a tensile strength of 530-710MPa, an elongation greater than 20%, an impact absorption energy of more than 200J at -150°C, and a yield strength ratio of less than 0.85.
[0021] In the composition design of the low yield ratio steel plate of the present invention:
[0022] C: Carbon is not good for low temperature toughness, but carbon atoms are interstitially dissolved in the BCC lattice to greatly improve the matrix strength. To meet the requirements of comprehensive strength and toughness, a small amount of carbon needs to be added to the steel. The control range of the C content in the present invention is 0.03-0.08%.
[0023] Si: Silicon is a ferrite stabilizing element. Adding it to steel can hinder the formation of carbides, reduce the source of low-temperature cleavage cracking in steel, and help improve low-temperature toughness. However, too high a silicon content increases the brittleness of the steel. The control range of the Si content in the present invention is 0.10-0.25%.
[0024] Mn: Manganese plays a role in solid solution strengthening and can improve the strength of the steel plate. In addition, manganese can effectively improve the hardenability of the steel plate, ensuring that the thick steel plate obtains the designed structure and achieves the target performance during quenching, but high manganese content is prone to segregation. The Mn content of the present invention is in the range of 0.3-0.8%.
[0025] S: Sulfur is a harmful residual element. It can form MnS inclusions when combined with manganese. It deforms and elongates during rolling, which is not conducive to the uniformity of mechanical properties, especially low-temperature toughness. The sulfur content is required to be less than 0.005%.
[0026] P: Phosphorus is also a harmful residual element, which has a great influence on low temperature toughness and is easily segregated on austenite grain boundaries. Therefore, the P content of the present invention is less than 0.006%.
[0027] Ni: Nickel is the most important alloy element for improving low temperature toughness. It can effectively improve the low temperature cleavage strength of the matrix and reduce the tough-to-brittle transition temperature. In addition, nickel is distributed and enriched in the reversed austenite during the heat treatment process, which can further improve the low temperature toughness. However, nickel is also an expensive alloy, and adding too much will increase the cost. The Ni content of the present invention is in the range of 4.6 to 5.5%.
[0028] Mo: Mo is an additive element. Mo can greatly improve hardenability. A small amount of addition is beneficial for thick steel plates to achieve target performance and has little effect on low-temperature toughness. Molybdenum alloys are expensive, and the Mo content of the present invention is controlled to not exceed 0.10%.
[0029] Al: It is an additive element. Aluminum is a deoxidizer in converter steelmaking. Residual aluminum combines with nitrogen in steel to form AlN particles. The dissolution temperature is very high, which can play a role in pinning grain boundaries and refining grains. In the present invention, aluminum can be added in an amount not exceeding 0.05%.
[0030] The method for manufacturing a low yield ratio steel plate having excellent low temperature toughness at -150°C of the present invention comprises the following steps:
[0031] 1) Smelting and casting
[0032] Smelting, refining outside the furnace and casting into slabs according to the above ingredients;
[0033] 2) Rolling
[0034] The slab is heated to 1000-1200℃, dephosphorized with high-pressure water, the compression ratio is ≥3 during rolling, and the final rolling temperature is 850-930℃;
[0035] 3) Quenching and tempering heat treatment
[0036] After quenching treatment, the steel plate is reheated to 780-850℃ and kept at this temperature for 0.5-3 hours. After the steel plate is kept at this temperature, it is immediately cooled by spraying water. The cooling rate is controlled at 10-50℃ / s between 780-400℃, and the temperature of the steel plate is finally reduced to room temperature.
[0037] Tempering treatment, tempering temperature 550 ~ 650 ℃, keep warm for 1 to 4 hours.
[0038] In the method for manufacturing a low yield ratio steel plate of the present invention:
[0039] The steel billet is heated to 1000-1200℃ to homogenize the austenite structure and fully dissolve the carbides in the steel. At the same time, the lower limit of the heating temperature is controlled to take into account the temperature drop of the slab during rolling and ensure that the rolling is completed at the specified temperature. The compression ratio is controlled during steel plate rolling to ensure that the compression ratio is ≥3.
[0040] Rolled steel plates need to undergo quenching and tempering heat treatment to achieve performance. The complete heat treatment process includes quenching heat treatment and tempering heat treatment. The rolled steel plate is reheated at 780-850℃ and kept warm for 0.5-3 hours to make the temperature inside and outside the steel plate consistent, forming a single uniform austenite structure. After the steel plate is kept warm, it is immediately sprayed with water for cooling, and the cooling rate of the steel plate in the range of 780-400℃ is controlled at 10-50℃ / s, and the temperature of the steel plate is finally reduced to room temperature. The steel plate is then tempered to adjust the final performance. The tempering temperature is 550-650℃, and the heat preservation is 1-4 hours to eliminate the quenching stress, promote the decomposition of the metastable structure formed by quenching, and form a stable structure.
[0041] Beneficial effects of the present invention:
[0042] The low temperature toughness of steel is closely related to the composition and process. The present invention adds more nickel elements and strictly controls the content of P and S impurity elements. Such a composition design improves the low temperature cleavage fracture strength of the matrix and increases the toughness-brittle transition temperature. After quenching and tempering heat treatment, it is ensured that the austenite is transformed at a higher cooling rate during cooling and the formation of proeutectoid ferrite is avoided, thereby ensuring that the low temperature toughness of -150°C is achieved.
[0043] Another measure adopted by the present invention is to adjust the cooling rate of the quenching process, thereby regulating the type and relative proportion of the organization formed after the austenite phase transformation, to obtain a mixed organization of 40-70% granular bainite and 30-60% lath martensite, wherein the granular bainite has a higher formation temperature and lower hardness, is easier to deform, and yields first under lower stress during the tensile process. The lath martensite has a lower formation temperature and higher hardness, and finally breaks under higher stress. The combination of the two achieves a lower yield strength ratio. In addition, both belong to shear-type phase transformation organizations, and both have relatively fine substructures, so that good low-temperature toughness can be obtained at the same time.
[0044] After the above composition and production process, the yield strength of the low yield strength ratio steel plate of the present invention is greater than 390MPa, the tensile strength is 530-710MPa, the elongation is more than 20%, the impact absorption energy of the steel plate at -150°C reaches more than 200J, and the yield strength ratio does not exceed 0.85.
[0045] Compared with the prior art, the main alloying element of the present invention is nickel, and the low-temperature toughness of the steel is ensured by adding a certain amount of nickel. However, the nickel content of Chinese patents CN114855060A and CN114875311A is relatively low, and accordingly only the low-temperature toughness of -40°C is achieved. The nickel content of Chinese patent CN109777938A is 7.15%, and more Cr and Mo elements are added. The present invention also adds other alloying elements to achieve effective strengthening and delay the austenite transformation incubation time. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the metallographic structure of Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The present invention will be further described below in conjunction with the embodiments and drawings.
[0048] The chemical composition of the embodiment of the present invention is shown in Table 1, and the balance is Fe and other inevitable impurities; the manufacturing process parameters of the embodiment are shown in Table 2, and the mechanical properties of the embodiment are shown in Table 3.
[0049] The process route of the embodiment of the present invention is: converter smelting→external refining (LF desulfurization, RH vacuum degassing)→continuous casting→heating→heating→rolling→quenching→tempering→inspection.
[0050] As can be seen from Table 3, the yield strength of the steel plates in the embodiments of the present invention exceeds 390MPa, the tensile strength is between 530 and 710MPa, the elongation exceeds 20%, and the actual level reaches more than 29%. At the same time, it has excellent low-temperature toughness and low yield strength ratio, the impact energy at -150℃ exceeds 200J, and the yield strength ratio does not exceed 0.85.
[0051] See also Figure 1 , which shows the metallographic structure of Example 1 of the present invention. As can be seen from the figure, after heat treatment, the typical microstructure of Example 1 is a mixture of granular bainite and lath martensite.
[0052] In summary, the present invention adopts a simple alloying method, through quenching and tempering heat treatment with controlled process parameters, to form a dual-phase structure and adjust its ratio, to obtain a steel plate with both low yield ratio and good low-temperature toughness, meeting the requirements of yield ratio ≤0.85 and low-temperature toughness of -150°C. The product of the present invention can be used to manufacture storage devices and transportation vehicles for low-temperature liquefied gases with a service temperature of ≥-150°C, such as liquefied ethane, ethylene, carbon dioxide, etc., and has high safety.
[0053]
[0054]
[0055]
Claims
1. A low yield strength ratio steel plate with excellent low temperature toughness at -150°C, the weight percentage of its components is: C 0.03-0.08%; Si 0.10~0.25%; Mn 0.3~0.8%; S≤0.005%; P≤0.006%; Ni 4.6~5.5%; The balance contains Fe and other inevitable impurities.
2. The low yield ratio steel plate with excellent low temperature toughness at -150°C as claimed in claim 1, characterized in that: The balance is Fe and other inevitable impurities.
3. The low yield ratio steel plate with excellent low temperature toughness at -150°C according to claim 1 or 2, characterized in that: It also contains Mo≤0.10wt%, and / or Al≤0.05wt%.
4. The low yield ratio steel plate with excellent low temperature toughness at -150°C according to claim 1, 2 or 3, characterized in that: The microstructure of the low yield ratio steel plate is 40-70% granular bainite and 30-60% lath martensite.
5. The low yield ratio steel plate with excellent low temperature toughness at -150°C as claimed in claim 1, 2, 3 or 4, characterized in that: The low yield strength ratio steel plate has a yield strength greater than 390 MPa, a tensile strength of 530-710 MPa, an elongation greater than 20%, an impact absorption energy of more than 200 J at -150°C, and a yield strength ratio of less than 0.
85.
6. The method for manufacturing a low yield ratio steel plate having excellent low temperature toughness at -150°C according to any one of claims 1 to 5, characterized in that: The steps include: 1) Smelting and casting Smelting, refining outside the furnace and casting into slabs according to the components of claim 1, 2 or 3; 2) Rolling The slab is heated to 1000-1200℃, the compression ratio is ≥3 during rolling, and the final rolling temperature is 850-930℃; 3) Quenching and tempering heat treatment After quenching treatment, the steel plate is reheated to 780-850℃ and kept at this temperature for 0.5-3 hours. After the steel plate is kept at this temperature, it is immediately cooled by spraying water. The cooling rate is controlled at 10-50℃ / s between 780-400℃, and the temperature of the steel plate is finally reduced to room temperature. Tempering treatment, tempering temperature 550 ~ 650 ℃, keep warm for 1 to 4 hours.
Citation Information
Patent Citations
High-tenacity -130 DEG C low-temperature steel and manufacturing method thereof
CN102330031A
Method for manufacturing Ni steel moderately-thick plate for low-temperature container
CN105441798A
Nickel-containing steel sheet for low temperature excellent in tensile strength and toughness and manufacturing method therefor