Chromium-free steel ball and production process thereof

By using the ratio and heat treatment process of low chromium scrap steel and rare metals to produce chromium-free steel balls, the problem of difficult separation of chromium elements and easy oxidation of surfaces in metal grinding is solved, and the wear resistance and fatigue strength of the steel balls are improved , meets the needs of the metal refining process.

CN119061328APending Publication Date: 2024-12-03ANHUI NINGGUO CHENGXIN WEAR-RESISTANT MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411488136.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the metal grinding process, the chromium element is difficult to separate, which is unfavorable to the metal refining process, and the surface of the steel ball is prone to oxidation, wear resistance and fatigue strength are insufficient.

Method used

The raw material ratio of chromium-free steel balls is adopted, including 95-99% low-chromium scrap steel, 1.2-1.5% rare metals (Mn, Mo, Ti) and 0.5-0.9% sporadic auxiliary materials (C, Si, S, P), through the medium frequency Electric furnace smelting, casting, cooling separation screening and heat treatment processes (annealing, normalizing, quenching, backtempering) produce chromium-free steel balls.

Benefits of technology

The chromium content of the steel ball is reduced, its wear resistance and fatigue strength are enhanced, surface oxidation is reduced, and the overall performance of the steel ball is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061328A_ABST
    Figure CN119061328A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel ball machining, in particular to a chromium-free steel ball and a production process thereof. The chromium-free steel ball comprises the following raw materials in parts by weight: 95-99 parts of scrap steel, the scrap steel is low-chromium steel, and the chromium content is controlled to be 0.2-0.8; 1.2-1.5 parts of rare metals and 0.5-0.9 part of sporadic auxiliary materials, wherein all the raw materials are calculated in parts by weight; according to the chromium-free steel ball production technology, in the steel ball production process, a medium-frequency electric furnace is used for smelting, a later heat treatment technology is used, and the heat treatment technology comprises the annealing technology, the normalizing technology, the quenching technology and the tempering technology; through cooperative use of the processes, the surface of the formed steel ball can be rapidly heated to the specified quenching temperature, the internal temperature of the steel ball is still kept close to the room temperature, finally, the heating temperature and the hardening layer depth in the steel ball production process are easy to control, and machining is facilitated; oxidized parts on the surfaces of the steel balls are less, and carbon lost in the formed steel balls is less; in addition, the shape deformation of the finally formed steel ball is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel ball processing, in particular to a chromium-free steel ball and a production process thereof. Background Art

[0002] When steel balls act as grinding media in the process of metal refining and grinding, they will become powder and directly mix into the ground metal minerals with the long-term use of steel balls. The chromium element in the steel balls is difficult to separate from some metals.

[0003] According to national standards, the chromium content of ordinary high-chromium balls is greater than or equal to 10, and the chromium content of low-chromium balls is 1 to 3. In addition, the chromium content of carbide-containing ductile iron grinding balls also reaches 0.2 to 1.5. This is very unfavorable for the metal refining and grinding process. Therefore, in order to reduce the impact of chromium on the refined metal itself, it is necessary to use chromium-free or extremely low-chromium grinding media, such as chromium-free steel balls. At the same time, in order to cooperate with the refining of metals, the surface of the chromium-free steel balls used is required to be not easy to oxidize and have a high carbon content, and the wear resistance and fatigue strength need to be enhanced.

[0004] In view of the problems in the above background technology, the present invention aims to provide a chrome-free steel ball and a production process thereof. Summary of the invention

[0005] The object of the present invention is to provide a chrome-free steel ball and a production process thereof to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0008] 95-99 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.2-1.5 parts of rare metals and 0.5-0.9 parts of miscellaneous auxiliary materials, all raw materials are calculated by weight;

[0009] As a further solution of the present invention: wherein, the rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3-1.0; Mo: 0.3-0.4 and Ti: 0.3-0.4; the miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8-3.8; Si: ≤0.8; S: <0.04 and P: <0.04.

[0010] The production process of the chrome-free steel ball comprises the following steps:

[0011] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0012] S2: Casting and molding the smelted raw metal;

[0013] S3: Cooling, separating and screening the cast steel balls; and

[0014] S4: performing heat treatment process on the separated and screened steel balls.

[0015] As a further solution of the present invention: the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is as follows:

[0016] S11: Weigh various raw materials quantitatively according to the raw material ratio: 95-99 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.2-1.5 parts of rare metals and 0.5-0.9 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3-1.0; Mo: 0.3-0.4 and Ti: 0.3-0.4; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8-3.8; Si: ≤0.8; S: <0.04; P: <0.04;

[0017] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals into the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste into the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later.

[0018] As a further solution of the present invention: the specific implementation method of the step of casting and molding the smelted raw metal in S2 is as follows:

[0019] S21: The metal smelted in the medium frequency furnace in step S1 is tested. After the test, all the elemental components in the smelted metal meet the design standards, it is taken out of the furnace for casting, and the casting temperature is controlled between 1600°C and 1630°C.

[0020] As a further solution of the present invention: the specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0021] S31: The steel balls cast in step S2 are separated and sorted using screening equipment. The screening is divided into two steps: first, the slag is screened and the balls are cooled using a vibrating screen, and then the metal in the screened slag is magnetically separated using a magnetic separator.

[0022] As a further solution of the present invention: the specific implementation method of the step of heat treating the separated and screened steel balls in S4 is as follows:

[0023] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls obtained to 720-760° C. and then keeping the temperature for 2-3 hours, then annealing and cooling to 580-610° C. in an annealing furnace, then taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0024] S42: normalizing the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 280-300° C. for 2-3 hours, then taking it out and cooling it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0025] S43: quenching and tempering the steel balls obtained in step S42: putting the normalized steel balls into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 260-580° C., and the steel balls are heated and heat preserved for 2-3 hours;

[0026] S44: The steel balls obtained in step S43 are subjected to a cold zone process: the heat-insulating steel balls are put into a coolant for cooling, wherein the coolant used here is oil.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The chrome-free steel balls described have the following advantages:

[0029] First, in the raw material ratio composition of chromium-free steel balls, the main raw material scrap steel is low-chromium steel, so as to reduce the chromium content of the steel balls produced later from the source; at the same time, rare metal elements such as Mn, Mo and Ti are added to the production raw materials; for example, Mn can form a solid solution with iron, strengthen ferrite and austenite, and increase the strength of the alloy without reducing its ductility; at the same time, Mn can form a solid solution with iron, strengthen ferrite and austenite, and increase the strength of the alloy without reducing its ductility; especially Mo, Mo and Fe can form a strengthening phase, improve the continuity of the grain boundary interface of steel, and improve the shear strength of the grain boundary equilibrium interface, which is also an important way to enhance the hardness and strength of steel; at the same time, Mo can improve the corrosion resistance of steel, mainly by forming a defense layer, antioxidant and rust inhibitor, effectively preventing the corrosion of steel by corrosive media such as oxygen, chlorine and sulfur;

[0030] 2. In the process of steel ball production, medium frequency electric furnace is used for smelting and subsequent heat treatment process, and the heat treatment process includes annealing, normalizing, quenching and tempering process; the medium frequency electromagnetic induction heating coil is emitted by the medium frequency electric furnace, which can cause skin effect on the formed steel ball, that is, the induction coil generates a large eddy current inside the steel ball in the opposite direction of the heating current, and the distribution of the eddy current on the cross section of the steel ball is uneven, the core is almost equal to zero, and the surface current density is extremely large; in this way, the surface of the formed steel ball can be quickly heated to the specified quenching temperature, while the internal temperature of the steel ball is still kept close to room temperature, which ultimately makes the heating temperature and the depth of the hardened layer easy to control during the production process of the steel ball, which is conducive to processing; the surface of the steel ball has less oxidation, and the formed steel ball loses less carbon; in addition, the final formed steel ball has less shape deformation. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention.

[0032] Figure 1 The present invention is a schematic diagram of a production process of a chrome-free steel ball according to an embodiment of the present invention.

[0033] Figure 2 The present invention is a schematic diagram of the steps of weighing raw materials and smelting in a production process of chromium-free steel balls according to an embodiment of the present invention.

[0034] Figure 3 This is a schematic diagram of the metal smelting and casting process steps of a chromium-free steel ball production process according to an embodiment of the present invention.

[0035] Figure 4 The present invention is a schematic diagram of the steel ball separation and screening process steps of a chromium-free steel ball production process according to an embodiment of the present invention.

[0036] Figure 5 The present invention is a schematic diagram of the heat treatment process steps of a chromium-free steel ball production process according to an embodiment of the present invention. DETAILED DESCRIPTION

[0037] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0038] Example 1

[0039] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0040] Scrap steel 95 parts Scrap steel is low-chromium steel, with chromium content controlled at 0.2-0.8, rare metals 1.2 parts and miscellaneous auxiliary materials 0.5 parts, all raw materials are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8; Si: ≤0.8; S: <0.04 and P: <0.04;

[0041] See also Figure 1-5 The production process of the above-mentioned chrome-free steel ball comprises the following steps:

[0042] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0043] S2: Casting and molding the smelted raw metal;

[0044] S3: Cooling, separating and screening the cast steel balls; and

[0045] S4: heat treatment process is performed on the separated and screened steel balls;

[0046] Among them, the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is:

[0047] S11: Weigh various raw materials quantitatively according to the raw material ratio: 95 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.2 parts of rare metals and 0.5 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8; Si: ≤0.8; S: <0.04; P: <0.04;

[0048] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals to the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste to the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later;

[0049] The specific implementation method of the step S2 of casting and molding the smelted raw metal is as follows:

[0050] S21: testing the metal smelted in the medium frequency furnace in step S1. After testing, if all the elements in the smelted metal meet the design standards, the metal is taken out of the furnace for casting, and the casting temperature is controlled between 1600°C;

[0051] The specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0052] S31: The steel balls cast in step S2 are separated and sorted using a screening device. The screening is divided into two steps:

[0053] First, the slag is screened and the balls are cooled by a vibrating screen, and then the metal in the screened slag is magnetically separated by a magnetic separator;

[0054] The specific implementation method of the process step of heat treating the separated and screened steel balls in S4 is as follows:

[0055] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls to 720° C. and then keeping the temperature for 2 hours, then annealing in an annealing furnace and cooling to 580° C. before taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0056] S42: performing a normalizing process on the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 280° C. for 2 hours, and then taking it out to cool it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0057] S43: quenching and tempering the steel balls obtained in step S42: putting the normalized steel balls into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 260° C., and the steel balls are heated and heat preserved for 2 hours;

[0058] S44: subjecting the steel balls obtained in step S43 to a cold zone process: placing the heat-insulating steel balls into a coolant for cooling, wherein the coolant used here is oil;

[0059] Example 2

[0060] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0061] Scrap steel 99 parts Scrap steel is low-chromium steel, the chromium content is controlled at 0.2-0.8, rare metals are 1.5 parts and miscellaneous auxiliary materials are 0.9 parts, all raw materials are calculated by weight; among them, rare metals include Mn, Mo and Ti, the proportion of the three raw materials is controlled at: Mn: 1.0; Mo: 0.4 and Ti: 0.4; miscellaneous auxiliary materials include C, Si, S and P, the proportion of the four raw materials is controlled at: C: 3.8; Si: ≤0.8; S: <0.04 and P: <0.04;

[0062] See also Figure 1-5 The production process of the above-mentioned chrome-free steel ball comprises the following steps:

[0063] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0064] S2: Casting and molding the smelted raw metal;

[0065] S3: Cooling, separating and screening the cast steel balls; and

[0066] S4: heat treatment process is performed on the separated and screened steel balls;

[0067] Among them, the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is:

[0068] S11: Weigh various raw materials quantitatively according to the raw material ratio: 99 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.5 parts of rare metals and 0.9 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 1.0; Mo: 0.4 and Ti: 0.4; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.8; Si: ≤0.8; S: <0.04; P: <0.04;

[0069] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals to the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste to the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later;

[0070] The specific implementation method of the step S2 of casting and molding the smelted raw metal is as follows:

[0071] S21: testing the metal smelted in the medium frequency furnace in step S1. After testing, if all the elements in the smelted metal meet the design standards, the metal is taken out of the furnace for casting, and the casting temperature is controlled between 1630°C;

[0072] The specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0073] S31: The steel balls cast in step S2 are separated and sorted using a screening device. The screening is divided into two steps:

[0074] First, the slag is screened and the balls are cooled by a vibrating screen, and then the metal in the screened slag is magnetically separated by a magnetic separator;

[0075] The specific implementation method of the process step of heat treating the separated and screened steel balls in S4 is as follows:

[0076] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls to 760° C. and then keeping the temperature for 3 hours, then annealing in an annealing furnace and cooling to 610° C. before taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0077] S42: normalizing the steel ball obtained in step S41: keep the annealed steel ball in a coolant at 300° C. for 3 hours, then take it out and cool it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0078] S43: quenching and tempering the steel ball obtained in step S42: putting the normalized steel ball into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 580° C., and the steel ball is heated and heat preserved for 3 hours;

[0079] S44: subjecting the steel balls obtained in step S43 to a cold zone process: placing the heat-insulating steel balls into a coolant for cooling, wherein the coolant used here is oil;

[0080] Example 3

[0081] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0082] Scrap steel 97 parts of scrap steel are low-chromium steel, with chromium content controlled at 0.2-0.8, rare metals 1.3 parts and miscellaneous auxiliary materials 0.7 parts, all raw materials are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.6; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.3; Si: ≤0.8; S: <0.04 and P: <0.04;

[0083] See also Figure 1-5 The production process of the above-mentioned chrome-free steel ball comprises the following steps:

[0084] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0085] S2: Casting and molding the smelted raw metal;

[0086] S3: Cooling, separating and screening the cast steel balls; and

[0087] S4: heat treatment process is performed on the separated and screened steel balls;

[0088] Among them, the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is:

[0089] S11: Weigh various raw materials quantitatively according to the raw material ratio: 97 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.3 parts of rare metals and 0.7 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.6; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.3; Si: ≤0.8; S: <0.04; P: <0.04;

[0090] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals to the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste to the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later;

[0091] The specific implementation method of the step S2 of casting and molding the smelted raw metal is as follows:

[0092] S21: testing the metal smelted in the medium frequency furnace in step S1. After testing, if all the elements in the smelted metal meet the design standards, the metal is taken out of the furnace for casting, and the casting temperature is controlled between 1615°C;

[0093] The specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0094] S31: The steel balls cast in step S2 are separated and sorted using a screening device. The screening is divided into two steps:

[0095] First, the slag is screened and the balls are cooled by a vibrating screen, and then the metal in the screened slag is magnetically separated by a magnetic separator;

[0096] The specific implementation method of the process step of heat treating the separated and screened steel balls in S4 is as follows:

[0097] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls to 740°C and then keeping the temperature for 2 hours, then annealing in an annealing furnace and cooling to 590°C before taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0098] S42: performing a normalizing process on the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 290° C. for 2 hours, and then taking it out to cool it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0099] S43: quenching and tempering the steel balls obtained in step S42: putting the normalized steel balls into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 420° C., and the steel balls are heated and heat preserved for 3 hours;

[0100] S44: subjecting the steel balls obtained in step S43 to a cold zone process: placing the heat-insulating steel balls into a coolant for cooling, wherein the coolant used here is oil;

[0101] Example 4

[0102] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0103] 96 parts of scrap steel are low-chromium steel, with chromium content controlled at 0.2-0.8, 1.3 parts of rare metals and 0.6 parts of miscellaneous auxiliary materials, all raw materials are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.4; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.0; Si: ≤0.8; S: <0.04 and P: <0.04;

[0104] See also Figure 1-5 The production process of the above-mentioned chrome-free steel ball comprises the following steps:

[0105] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0106] S2: Casting and molding the smelted raw metal;

[0107] S3: Cooling, separating and screening the cast steel balls; and

[0108] S4: heat treatment process is performed on the separated and screened steel balls;

[0109] Among them, the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is:

[0110] S11: Weigh various raw materials quantitatively according to the raw material ratio: 96 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.3 parts of rare metals and 0.6 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.4; Mo: 0.3 and Ti: 0.3; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.0; Si: ≤0.8; S: <0.04; P: <0.04;

[0111] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals to the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste to the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later;

[0112] The specific implementation method of the step S2 of casting and molding the smelted raw metal is as follows:

[0113] S21: testing the metal smelted in the medium frequency furnace in step S1. After testing, if all the elements in the smelted metal meet the design standards, the metal is taken out of the furnace for casting, and the casting temperature is controlled between 1610°C;

[0114] The specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0115] S31: The steel balls cast in step S2 are separated and sorted using a screening device. The screening is divided into two steps:

[0116] First, the slag is screened and the balls are cooled by a vibrating screen, and then the metal in the screened slag is magnetically separated by a magnetic separator;

[0117] The specific implementation method of the process step of heat treating the separated and screened steel balls in S4 is as follows:

[0118] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls to 730° C. and then keeping the temperature for 2 hours, then annealing in an annealing furnace and cooling to 590° C. before taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0119] S42: performing a normalizing process on the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 285° C. for 2 hours, and then taking it out to cool it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0120] S43: quenching and tempering the steel ball obtained in step S42: putting the normalized steel ball into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 390° C., and the steel ball is heated and heat preserved for 2 hours;

[0121] S44: subjecting the steel balls obtained in step S43 to a cold zone process: placing the heat-insulating steel balls into a coolant for cooling, wherein the coolant used here is oil;

[0122] Example 5

[0123] A chrome-free steel ball, wherein the raw material ratio of the chrome-free steel ball comprises:

[0124] Scrap steel 98 parts Scrap steel is low chromium steel, chromium content is controlled at 0.2-0.8, rare metals are 1.4 parts and miscellaneous auxiliary materials are 0.8 parts, all raw materials are calculated by weight; among them, rare metals include Mn, Mo and Ti, the proportion of the three raw materials is controlled at: Mn: 0.9; Mo: 0.4 and Ti: 0.4; miscellaneous auxiliary materials include C, Si, S and P, the proportion of the four raw materials is controlled at: C: 3.6; Si: ≤0.8; S: <0.04 and P: <0.04;

[0125] See also Figure 1-5 The production process of the above-mentioned chrome-free steel ball comprises the following steps:

[0126] S1: Weigh various raw metals according to the raw material ratio for smelting;

[0127] S2: Casting and molding the smelted raw metal;

[0128] S3: Cooling, separating and screening the cast steel balls; and

[0129] S4: heat treatment process is performed on the separated and screened steel balls;

[0130] Among them, the specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is:

[0131] S11: Weigh various raw materials quantitatively according to the raw material ratio: 98 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.4 parts of rare metals and 0.8 parts of miscellaneous auxiliary materials, all of which are calculated by weight; among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.9; Mo: 0.4 and Ti: 0.4; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 3.6; Si: ≤0.8; S: <0.04; P: <0.04;

[0132] S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals to the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste to the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later;

[0133] The specific implementation method of the step S2 of casting and molding the smelted raw metal is as follows:

[0134] S21: testing the metal smelted in the medium frequency furnace in step S1. After testing, if all the elements in the smelted metal meet the design standards, the metal is taken out of the furnace for casting, and the casting temperature is controlled between 1620°C;

[0135] The specific implementation method of the step of cooling, separating and screening the cast steel balls in S3 is as follows:

[0136] S31: The steel balls cast in step S2 are separated and sorted using a screening device. The screening is divided into two steps:

[0137] First, the slag is screened and the balls are cooled by a vibrating screen, and then the metal in the screened slag is magnetically separated by a magnetic separator;

[0138] The specific implementation method of the process step of heat treating the separated and screened steel balls in S4 is as follows:

[0139] S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls to 750°C and then keeping the temperature for 3 hours, then annealing in an annealing furnace and cooling to 600°C before taking them out of the furnace, and then cooling them to room temperature in a natural environment;

[0140] S42: performing a normalizing process on the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 295° C. for 3 hours, and then taking it out to cool it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath;

[0141] S43: quenching and tempering the steel ball obtained in step S42: putting the normalized steel ball into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; the heating temperature of the medium frequency electric furnace is controlled at 550° C., and the steel ball is heated and heat preserved for 3 hours;

[0142] S44: subjecting the steel balls obtained in step S43 to a cold zone process: placing the heat-insulating steel balls into a coolant for cooling, wherein the coolant used here is oil;

[0143] According to the raw material ratios and production processes of the above five embodiments, chromium-free steel balls were manufactured. The physical parameters of the manufactured chromium-free steel balls are shown in Table 1:

[0144] Table 1

[0145] Example\Physical parameters hardness Impact toughness Ball drop fatigue times Example 1 59.5 4.1 15850 Example 2 63.1 4.3 16124 Example 3 65.0 4.6 16835 Example 4 64.2 4.4 16465 Example 5 62.9 4.2 15945

[0146] In the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0147] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A chrome-free steel ball, characterized in that: The raw material ratio of the chrome-free steel ball comprises: 95-99 parts of scrap steel, which is low-chromium steel with a chromium content controlled at 0.2-0.8; 1.2-1.5 parts of rare metals and 0.5-0.9 parts of miscellaneous auxiliary materials. All raw materials are calculated by weight.

2. The chrome-free steel ball according to claim 1, characterized in that: Rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3-1.0; Mo: 0.3-0.4 and Ti: 0.3-0.4; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8-3.8; Si: ≤0.8; S: < 0.04 and P: < 0.

04.

3. A process for producing a chrome-free steel ball as claimed in any of claims 1 to 2, characterized in that The following steps are involved: S1: weighing various raw metals according to the raw material ratio for smelting; S2: casting and molding the smelted raw metals; S3: cooling, separating and screening the cast steel balls; and S4: heat treating the separated and screened steel balls.

4. The production process of chrome-free steel balls according to claim 3, characterized in that: The specific implementation method of the step S1 of weighing various raw metals according to the raw material ratio for smelting is as follows: S11: Weigh various raw materials quantitatively according to the raw material ratio: 95-99 parts of scrap steel, which is low-chromium steel with a chromium content of 0.2-0.8, 1.2-1.5 parts of rare metals, and 0.5-0.9 parts of miscellaneous auxiliary materials, all raw materials are calculated by weight; Among them, rare metals include Mn, Mo and Ti, and the proportion of the three raw materials is controlled at: Mn: 0.3-1.0; Mo: 0.3-0.4 and Ti: 0.3-0.4; miscellaneous auxiliary materials include C, Si, S and P, and the proportion of the four raw materials is controlled at: C: 2.8-3.8; Si: ≤0.8; S: <0.04; P <0.04; S12: Start the medium frequency electric furnace, first add the weighed scrap steel, because the scrap steel content is relatively large, adding it to the medium frequency electric furnace first can save electricity; then add the weighed rare metals into the medium frequency electric furnace, the rare metal content is low and the price is relatively high, in order to reduce the burning loss, it is better to add them later; finally, add the weighed scattered waste into the medium frequency electric furnace for smelting, which is used to improve the quality of the steel balls cast later.

5. The production process of chrome-free steel balls according to claim 4, characterized in that: S2 is a step of casting and molding the smelted raw metal. The specific implementation method is as follows: S21: The metal smelted in the medium frequency furnace in step S1 is tested. After the test, all the elemental components in the smelted metal meet the design standards, it is taken out of the furnace for casting, and the casting temperature is controlled between 1600°C and 1630°C.

6. The production process of chrome-free steel balls according to claim 5, characterized in that: S3 is a step of cooling, separating and screening the cast steel balls. The specific implementation method is as follows: S31: The steel balls cast in step S2 are separated and sorted using screening equipment. The screening is divided into two steps: first, the slag is screened and the balls are cooled using a vibrating screen, and then the metal in the screened slag is magnetically separated using a magnetic separator.

7. The production process of chrome-free steel balls according to claim 6, characterized in that: S4 is a process step for heat treating the separated and screened steel balls. The specific implementation method is as follows: S41: performing an annealing process on the steel balls obtained after screening: heating the steel balls obtained to 720-760° C. and then keeping the temperature for 2-3 hours, then annealing and cooling to 580-610° C. in an annealing furnace, then taking them out of the furnace, and then cooling them to room temperature in a natural environment; S42: normalizing the steel ball obtained in step S41: keeping the annealed steel ball in a coolant at 280-300° C. for 2-3 hours, then taking it out and cooling it in a natural environment with wind; the coolant used for normalizing is a sodium nitrate salt bath; S43: performing a quenching and tempering process on the steel ball obtained in step S42: putting the normalized steel ball into a medium frequency electric furnace for heating and heat preservation to achieve quenching and tempering operations; The heating temperature of the medium frequency electric furnace is controlled at 260-580°C, and the steel balls are heated and kept warm for 2-3 hours; and S44: The steel balls obtained in step S43 are subjected to a cold zone process: the heat-insulating steel balls are put into a coolant for cooling, wherein the coolant used here is oil.