High-strength high-ductility Cu-Ni-Si alloy plate and preparation method thereof
Through medium deformation, deep cold rolling and graded aging treatment, a fine precipitation phase is formed, which solves the problem of unsatisfactory grain regulation of Cu-Ni-Si alloy sheets, improves its strength and plasticity, and achieves efficient Cu-Ni -Si alloy sheet preparation.
Patent Information
- Application Number
- CN202411058629.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-02
AI Technical Summary
In the processing technology of traditional Cu-Ni-Si alloys, the grain size and morphology are not ideal, which affects its strength and conductivity. The deep cold rolling process leads to a decrease in material plasticity and an increase in production costs.
The deep-cold rolling process with medium deformation (70-80%) is adopted, including the first deep-cold rolling, intermediate aging treatment and the second deep-cold rolling, combined with the graded aging treatment, to form a small and evenly distributed precipitation phase. Obstruct dislocation movement and enhance material strength and plasticity.
On the basis of maintaining high strength and excellent conductivity, the plasticity and comprehensive mechanical properties of Cu-Ni-Si alloy sheets are significantly improved, reducing the internal stress concentration of the material and the aggregation of precipitation phases, and improving the forming ability and elongation of the material. .
Smart Images

Figure CN119061334A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of copper alloys, and in particular to a high-strength and high-ductility Cu-Ni-Si alloy plate and a preparation method thereof. Background Art
[0002] With the rapid development of integrated circuit technology, especially in the field of large-scale and ultra-large-scale integrated circuits, the performance requirements for lead frames are becoming increasingly stringent. Cu-Ni-Si alloy has become the preferred material for lead frame manufacturing in the field of integrated circuits due to its excellent comprehensive properties such as high strength and good conductivity.
[0003] In the traditional processing technology, the Cu-Ni-Si alloy exhibits problems of poor grain size, morphology and precipitation behavior control in the process of conventional room temperature rolling followed by conventional aging treatment, which affects the strength and conductivity of the alloy and limits its potential in high-end applications. In order to solve this problem, deep cold rolling technology has been developed for alloy processing in recent years. However, large deformation rolling (more than 90% deformation) is generally adopted, and the work hardening phenomenon is significant, which seriously reduces the plasticity of the plate. In addition, this method has a long processing process and is accompanied by high energy consumption and production costs. Summary of the invention
[0004] In view of one or more technical problems existing in the prior art, the present invention provides a high-strength and high-ductility Cu-Ni-Si alloy plate and a preparation method thereof. The preparation method of the Cu-Ni-Si alloy plate provided by the present invention can improve the plasticity of the Cu-Ni-Si alloy plate while maintaining high strength and excellent conductivity by rolling with a medium deformation amount (70-80%), thereby obtaining a Cu-Ni-Si alloy plate with excellent comprehensive performance.
[0005] In a first aspect, the present invention provides a method for preparing a high-strength and high-ductility Cu-Ni-Si alloy plate, the preparation method comprising:
[0006] The hot-rolled Cu-Ni-Si alloy is subjected to a first deep cold rolling, an intermediate aging treatment and a second deep cold rolling to obtain a deep cold rolled plate; the total deformation after the first deep cold rolling is 40-45% of the initial thickness of the hot-rolled Cu-Ni-Si alloy; the total deformation after the second deep cold rolling is 70-80% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0007] The deep cold rolled plate is subjected to graded aging treatment to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate.
[0008] Preferably, the hot-rolled Cu-Ni-Si alloy is obtained by subjecting the cast Cu-Ni-Si alloy to solution treatment and hot rolling;
[0009] Preferably, the temperature of the solution treatment is the same as the temperature of the hot rolling;
[0010] More preferably, the temperature of the solution treatment and the hot rolling is 850-950° C.; and / or the time of the solution treatment is 1-2 h.
[0011] Preferably, the total deformation after hot rolling is 70-80% of the initial thickness of the cast Cu-Ni-Si alloy;
[0012] The deformation amount of each pass during the hot rolling process is 15-25% of the initial thickness of the cast Cu-Ni-Si alloy; and / or
[0013] The holding time between each pass in the hot rolling process is 5 to 10 minutes.
[0014] Preferably, the deformation amount of each pass in the first deep cold rolling process is 5-10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
[0015] Preferably, the temperature of the intermediate aging treatment is 400-500°C, preferably 425-475°C; and / or
[0016] The intermediate aging treatment time is 60 to 120 minutes.
[0017] Preferably, the second deep cold rolling includes a first stage and a second stage, and the deformation amount of each pass in the second stage is smaller than the deformation amount of each pass in the first stage.
[0018] Preferably, the deformation amount of each pass in the first stage is 8-10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy; and / or
[0019] The deformation amount of each pass in the second stage is 3-5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
[0020] Preferably, the graded aging treatment includes a primary aging treatment and a secondary aging treatment, and the temperature of the secondary aging treatment is greater than the temperature of the primary aging treatment.
[0021] Preferably, the temperature of the primary aging treatment is 150-250°C; and / or
[0022] The temperature of the secondary aging treatment is not higher than the temperature of the intermediate aging treatment.
[0023] In a second aspect, the present invention provides a high-strength and high-ductility Cu-Ni-Si alloy plate, which is prepared by the preparation method described in the first aspect.
[0024] Compared with the prior art, the present invention has at least the following beneficial effects:
[0025] The present invention firstly performs a first deep cold rolling with a small deformation amount to introduce deformation twins, thereby achieving a preliminary improvement in the strength of the material, and at the same time can effectively reduce the proliferation of dislocations during the rolling process, reduce the internal stress concentration of the material, help maintain the plasticity of the material, enhance its forming ability in a low temperature environment, and reduce the possibility of material fracture; then an intermediate aging treatment is performed, which is beneficial to the formation of fine and evenly distributed precipitation phases in the alloy matrix while maintaining the deformation twins, can effectively hinder the movement of dislocations, and thus improve the strength of the material, and can also reduce the impact of recovery softening caused by the alloy during the precipitation process; then a second deep cold rolling is performed, and the effect of the intermediate aging treatment is utilized to promote the formation of more fine deformation twins, further improving the strength of the material, and through two-step deep cold rolling. The invention realizes the refinement of alloy grains under medium deformation (70-80%), thereby enhancing the plasticity of Cu-Ni-Si alloy sheet, and also promotes the uniform distribution of nano-precipitated phases in the alloy, and significantly improves the strength of Cu-Ni-Si alloy sheet on the basis of maintaining the electrical conductivity of Cu-Ni-Si alloy sheet; finally, through graded aging treatment, on the basis of maintaining deformation twins, the precipitation process in the alloy is precisely regulated to make the distribution of precipitation phase more uniform, effectively reduce the negative impact of dislocation on plasticity, and reduce the aggregation of precipitation phase and grain coarsening phenomenon, maintain the uniformity and stability of material microstructure, improve the uniformity of material during plastic deformation, thereby improving the elongation, and further improving the comprehensive mechanical properties of Cu-Ni-Si alloy sheet. The preparation method of Cu-Ni-Si alloy sheet provided by the invention can realize the improvement of plasticity of Cu-Ni-Si alloy sheet on the basis of maintaining high strength and excellent electrical conductivity by rolling with medium deformation (70-80%), and obtain Cu-Ni-Si alloy sheet with excellent comprehensive performance.
[0026] The preparation method of the Cu-Ni-Si alloy plate provided by the present invention can improve the plasticity of the Cu-Ni-Si alloy plate while maintaining high strength and excellent conductivity by rolling with a medium deformation amount (70-80%), thereby obtaining a Cu-Ni-Si alloy plate with excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 It is a schematic diagram of the preparation process of the high-strength and high-ductility Cu-Ni-Si alloy plate of the present invention;
[0029] Figure 2 This is a diagram showing the mechanism of improving the mechanical properties of the Cu-Ni-Si alloy plate by the preparation method of the high-strength and high-ductility Cu-Ni-Si alloy plate provided by the present invention;
[0030] Figure 3 is a metallographic structure diagram of a hot-rolled Cu-Ni-Si alloy provided in Example 1 of the present invention;
[0031] Figure 4 1 is a grain boundary distribution diagram (left) and a KAM diagram (right) of a plate after the first deep cold rolling provided in Example 1 of the present invention;
[0032] Figure 5 The grain boundary distribution diagram (left) and SEM diagram (right) of the plate after intermediate aging treatment provided in Example 1 of the present invention;
[0033] Figure 6 This is a TEM-EDS image of the high-strength and high-ductility Cu-Ni-Si alloy plate provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] In a first aspect, the present invention provides a method for preparing a high-strength and high-ductility Cu-Ni-Si alloy plate, the preparation method comprising:
[0036] The hot-rolled Cu-Ni-Si alloy is subjected to a first deep cold rolling, an intermediate aging treatment, and a second deep cold rolling to obtain a deep cold rolled plate; the total deformation after the first deep cold rolling is 40-45% (for example, it can be 40%, 41%, 42%, 43%, 44% or 45%) of the initial thickness of the hot-rolled Cu-Ni-Si alloy; the total deformation after the second deep cold rolling is 70-80% (for example, it can be 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%) of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
[0037] The deep cold rolled plate is subjected to graded aging treatment to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate.
[0038] The present invention firstly performs a first deep cold rolling with a small deformation amount to introduce deformation twins, thereby achieving a preliminary improvement in the strength of the material, and at the same time can effectively reduce the proliferation of dislocations during the rolling process, reduce the internal stress concentration of the material, help maintain the plasticity of the material, enhance its forming ability in a low temperature environment, and reduce the possibility of material fracture; then an intermediate aging treatment is performed, which is beneficial to the formation of fine and evenly distributed precipitation phases in the alloy matrix while maintaining the deformation twins, can effectively hinder the movement of dislocations, and thus improve the strength of the material, and can also reduce the impact of recovery softening caused by the alloy during the precipitation process; then a second deep cold rolling is performed, and the effect of the intermediate aging treatment is utilized to promote the formation of more fine deformation twins, further improving the strength of the material, and through two-step deep cold rolling. The system realizes the refinement of alloy grains under medium deformation (70-80%), thereby enhancing the plasticity of Cu-Ni-Si alloy sheet, and also promotes the uniform distribution of nano-precipitated phases in the alloy. On the basis of maintaining the conductivity of Cu-Ni-Si alloy sheet, the strength of Cu-Ni-Si alloy sheet is significantly improved; finally, through graded aging treatment, on the basis of maintaining deformation twins, the precipitation process in the alloy is precisely controlled to make the distribution of precipitation phase more uniform, effectively reduce the negative impact of dislocation on plasticity, reduce the aggregation of precipitation phase and coarsening of grains, maintain the uniformity and stability of material microstructure, improve the uniformity of material in the process of plastic deformation, thereby improving the elongation, and further improving the comprehensive mechanical properties of Cu-Ni-Si alloy sheet.
[0039] The preparation method of the Cu-Ni-Si alloy plate provided by the present invention can improve the plasticity of the Cu-Ni-Si alloy plate while maintaining high strength and excellent conductivity by rolling with a medium deformation amount (70-80%), thereby obtaining a Cu-Ni-Si alloy plate with excellent comprehensive performance.
[0040] The inventors found that when the total deformation is constant, if the deformation of the first deep cold rolling is too large, the deformation of the subsequent second deep cold rolling process is small, resulting in a small number of deformation twins generated during the rolling process, and the final strength of the plate is reduced. In addition, the insufficient deformation of the second deep cold rolling process will reduce the number of precipitated phases in the graded aging process, and the strength and conductivity of the plate will both decrease. If the total deformation after the second deep cold rolling is too small, the internal energy storage of the material is low, resulting in a reduction in the number of precipitated phases after the subsequent graded aging treatment, resulting in low strength and conductivity, which cannot meet the actual application requirements; if the total deformation after the second deep cold rolling is too large, self-annealing is likely to occur during the second deep cold rolling process, and the material undergoes recovery recrystallization, resulting in a decrease in strength. Even if self-annealing does not occur, the dislocation density of the material will be significantly increased due to deep cold rolling, resulting in a decrease in the plasticity of the final plate.
[0041] According to some preferred embodiments, the hot-rolled Cu-Ni-Si alloy is obtained by subjecting the cast Cu-Ni-Si alloy to solution treatment and hot rolling;
[0042] Preferably, the temperature of the solution treatment is the same as the temperature of the hot rolling;
[0043] More preferably, the temperature of the solution treatment and the hot rolling is 850-950°C (for example, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C or 950°C); and / or, the time of the solution treatment is 1-2h (for example, 1h, 1.2h, 1.4h, 1.5h, 1.6h, 1.8h or 2h).
[0044] In order to promote the recrystallization process of the material and eliminate the lattice distortion caused by deformation, the solution treatment of the present invention selects the same temperature as the hot rolling, and the temperature of the solution treatment and the hot rolling is controlled within the above range, and the coarse grains of the initial cast Cu-Ni-Si alloy are improved by hot rolling, and the uniform distribution of alloy elements is promoted, and the component segregation is reduced. The present invention is selected from but not limited to one of C70250 copper alloy, MAX251 copper alloy, KLFA85 copper alloy (Cu-3.2Ni-0.7Si-1.1Zn), CuNi2Si alloy, and CuNiSi-(Cr, Zr) alloy for Cu-Ni-Si alloy. According to some preferred embodiments, the total deformation after hot rolling is 70-80% of the initial thickness of the cast Cu-Ni-Si alloy (for example, it can be 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%).
[0045] According to some preferred embodiments, the amount of deformation in each pass during the hot rolling process is 15 to 25% (for example, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%) of the initial thickness of the cast Cu-Ni-Si alloy.
[0046] According to some preferred embodiments, the holding time between each pass in the hot rolling process is 5 to 10 minutes (for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes).
[0047] In order to make the internal temperature of the material uniform, ensure the uniform temperature distribution of the rolled plate during the rolling process, and avoid uneven deformation caused by temperature difference, each pass needs to be kept warm for 5 to 10 minutes. After the last pass of rolling, the material is water-cooled and no insulation is required.
[0048] According to some preferred embodiments, the deformation amount in each pass during the first deep cold rolling process is 5-10% (for example, 5%, 6%, 7%, 8%, 9% or 10%) of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
[0049] According to some preferred embodiments, the temperature of the intermediate aging treatment is 400-500°C (for example, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C), preferably 425-475°C (for example, 425°C, 430°C, 435°C, 440°C, 445°C, 450°C, 455°C, 460°C, 465°C, 470°C or 475°C); the intermediate aging treatment in the above temperature range is conducive to the formation of fine and uniformly distributed precipitation phases in the alloy matrix, and these fine and dispersed precipitation phases can effectively hinder the movement of dislocations, thereby improving the strength of the material. At the same time, aging treatment at the above lower temperature range can reduce the impact of recovery softening caused by the alloy during the precipitation process.
[0050] According to some preferred embodiments, the intermediate aging treatment time is 60 to 120 min (for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min).
[0051] According to some preferred embodiments, the second deep cold rolling includes a first stage and a second stage, and the deformation amount of each pass in the second stage is less than the deformation amount of each pass in the first stage; the later stage (second stage) of the second deep cold rolling of the present invention adopts a smaller rolling reduction, which can reduce the risk of cracks on the surface of the material, avoid the phenomenon of hardening or cracking of the material due to excessive deformation, and obtain a flatter and smoother surface. In addition, the rolling with a small deformation amount in the later stage (second stage) can also accurately control the final thickness of the material, ensuring the consistency and accuracy of the product size.
[0052] According to some preferred embodiments, the deformation amount of each pass in the first stage is 8-10% (for example, 8%, 9% or 10%) of the initial thickness of the hot-rolled Cu-Ni-Si alloy; and / or
[0053] The deformation amount of each pass in the second stage is 3% to 5% (for example, 3%, 4% or 5%) of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
[0054] According to some preferred embodiments, the graded aging treatment includes a primary aging treatment and a secondary aging treatment, and the temperature of the secondary aging treatment is greater than the temperature of the primary aging treatment.
[0055] The present invention adopts graded aging to achieve the improvement of comprehensive performance of materials. The low-temperature aging stage of graded aging treatment is conducive to the aggregation of solute atoms in the lattice to form GP zones (atomic segregation regions), which maintain a coherent relationship with the matrix, resulting in lattice distortion, laying the foundation for the improvement of alloy strength, and the formed GP zones (atomic segregation regions) as precursors of precipitation phases can locally pin dislocations, slow down their movement, thereby reducing the overall dislocation density, and helping to maintain the plasticity of the material; then in the high-temperature aging stage, the GP zones gradually transform into more stable precipitation phases, and these precipitation phases keep small size and dispersed distribution during the high-temperature aging process, avoiding excessive growth, and the small and evenly distributed precipitation phases greatly hinder the dislocation movement, thereby improving the strength of the material, and then effectively maintaining the strength and plasticity balance of the material. The high-temperature aging stage also helps to relax internal stress and reduce the work hardening effect, which not only improves the plastic deformation ability of the material, but also further reduces the accumulation of dislocations. In addition, the graded aging treatment promotes the release of internal stress in the material through staged temperature regulation, helps to alleviate the work hardening effect and internal residual stress, and thus significantly improves the plastic deformation capacity of the material. The precipitate phase obtained by the graded aging treatment is more evenly distributed, reducing the aggregation of the precipitate phase and the coarsening of the grains, maintaining the uniformity and stability of the material's microstructure, and improving the uniformity of the material during the plastic deformation process, thereby increasing the elongation.
[0056] In terms of electrical conductivity, since the scattering effect of solid solution atoms on electrons is more significant than that of precipitated phases, and the twin boundaries have low scattering characteristics, the deformation twins introduced by the second deep cold rolling have little effect on the electrical conductivity. Therefore, after the precipitated phase is formed, the electrical conductivity of the material will increase overall. The precipitated phase after graded aging is finer and has less obstruction to the electron transmission path, so it can maintain a higher conductivity.
[0057] The inventors found that the conventional method instead of graded aging treatment after the second deep cold rolling will cause the precipitated phase to be coarser and tend to aggregate to form local concentrated areas, resulting in non-uniformity of material properties. The coarse precipitated phase acts as an obstacle to dislocation movement, increases the work hardening of the material, and thus reduces its plastic deformation capacity. In addition, the larger precipitated phase will increase the scattering effect on electrons, making it difficult to maintain a high conductivity.
[0058] According to some preferred embodiments, the temperature of the primary aging treatment is 150-250°C (for example, it can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C or 250°C). If the temperature of the primary aging treatment of the present invention is too low, the atomic segregation region (GP region) will be formed slowly or incompletely, which is not conducive to the gradual transformation of the GP region into a more stable precipitation phase during the secondary aging treatment. In addition, if the temperature of the primary aging treatment is too low, the residual stress cannot be released, which reduces the elongation of the rolled plate; if the temperature of the primary aging treatment is too high, the atomic segregation region will be formed too quickly and too large, and a coarse stable precipitation phase will be directly precipitated, which reduces the strength of the rolled plate.
[0059] According to some preferred embodiments, after the primary aging treatment, the temperature is raised to the temperature of the secondary aging treatment at a heating rate of 30 to 40°C / min (for example, 30°C / min, 32°C / min, 34°C / min, 35°C / min, 36°C / min, 38°C / min or 40°C / min). In order to uniformly distribute the temperature inside the material and avoid the migration of the twin boundaries due to local overheating, the heating rate should not be too fast, so the present invention preferably sets the heating rate to the above range.
[0060] According to some preferred embodiments, the temperature of the secondary aging treatment is not higher than the temperature of the intermediate aging treatment.
[0061] If the temperature of the secondary aging treatment is too high, the grains of the matrix will grow, the size of the precipitated phase will increase, and the strength of the rolled plate will decrease. At the same time, the precipitated phase will precipitate at the grain boundary of the matrix, and the elongation of the rolled plate will decrease.
[0062] The present invention adopts the process of "first deep cold rolling-intermediate aging treatment-second deep cold rolling-graded aging treatment" to improve the mechanical properties of Cu-Ni-Si alloy. Figure 2 In the intermediate aging treatment stage, a large number of fine and dispersed precipitates have been formed inside the alloy. These precipitates effectively hinder the movement of dislocations during the second deep cold rolling process, and enhance the driving force of twin nucleation, thereby significantly increasing the content of deformation twins. The refinement of the deformation twin bundle caused by the second deep cold rolling further strengthens the hindering effect on dislocations, and the increase in dislocation density promotes the subsequent precipitation process. Therefore, the use of the present invention "first deep cold rolling-intermediate aging treatment-second deep cold rolling-graded aging treatment" can achieve a strength level that reaches or even exceeds the 90% deformation level obtained by the traditional process at a lower deformation amount (70-80%).
[0063] In a second aspect, the present invention provides a high-strength and high-ductility Cu-Ni-Si alloy plate, which is prepared by the preparation method described in the first aspect.
[0064] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the examples. The present invention does not specifically limit the sources of the reagents used in the examples and comparative examples, and the reagents can be directly purchased or synthesized by themselves. The embodiments of the present invention take C70250 copper alloy (chemical analysis results show that the Ni content of the copper alloy is 2.56wt.%, Si content is 0.54wt.%, Mg content is 0.16wt.%, and the rest is Cu), MAX251 copper alloy (chemical analysis results show that the Ni content of the copper alloy is 2wt.%, Si content is 0.5wt.%, Sn content is 0.5wt.%, Zn content is 1wt.%, and the rest is Cu), and KLFA85 copper alloy (chemical analysis results show that the Ni content of the copper alloy is 3.2wt.%, Si content is 0.7wt.%, Zn content is 1.1wt.%, and the rest is Cu) as examples only to illustrate the technical solution of the present invention, but not to limit it. The rolling of other Cu-Ni-Si alloy plates (for example, CuNi2Si alloy, CuNiSi-(Cr, Zr) alloy, etc.) is also applicable to the preparation method of the present invention. It should be noted that the deep cold rolling process of the present invention is first immersed in liquid nitrogen (-196°C) and then quickly taken out and rolled at room temperature. Heat loss is inevitable in this process and cannot be accurately controlled. Therefore, the temperature of deep cold rolling in the embodiment of the present invention is within a range.
[0065] Example 1
[0066] A method for preparing a high-strength and high-ductility Cu-Ni-Si alloy plate comprises:
[0067] S1. After the cast Cu-Ni-Si alloy (C70250 copper alloy) with an initial thickness of 30 mm is solution treated at 900°C for 1 hour, it is hot rolled at 900°C for 4 times with a deformation amount of 20% of the initial thickness. The material needs to be kept warm for 5 minutes between each pass. After the last rolling pass, the material is water-cooled without insulation to obtain a hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm. At this time, the total deformation of the hot rolling is 80% of the initial thickness.
[0068] S2. The hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm was immersed in liquid nitrogen (-196°C) for 30 min, and was subjected to deep cold rolling at -196 to -150°C for 4 times with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and each pass was immersed in liquid nitrogen for 10 min to obtain a first deep cold rolled sheet with a thickness of 3.6 mm. At this time, the total deformation amount was 40% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0069] S3. The first deep cold rolled sheet with a thickness of 3.6 mm was aged at 450° C. for 90 min, and then the aged material was immersed in liquid nitrogen for 30 min, and then the second deep cold rolled was performed at -196 to -150° C., firstly, three deep cold rollings were performed with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and then two deep cold rollings were performed with a deformation amount of 5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and each pass was immersed in liquid nitrogen for 10 min to obtain a second deep cold rolled sheet with a thickness of 1.2 mm, and the total deformation amount was 80% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0070] S4. After the second deep cold rolled plate is water-cooled, it is first subjected to low-temperature aging treatment at 200°C for 1 h, and then heated to 450°C at a heating rate of 35°C / min for high-temperature aging treatment for 30 min to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate. Its performance data are shown in Table 1.
[0071] The metallographic diagram of the hot-rolled Cu-Ni-Si alloy in this embodiment ( Figure 3 ) It can be seen that most of the organization is equiaxed crystals, which helps to improve the processing performance of the material, ensure that the material has good plastic deformation ability, and make it less likely to break when subjected to external forces. In addition, annealing twins also appear during the annealing process, and the grain size is about 79.3μm. Overall, the organization has good uniformity, ensuring that the initial performance of the material in different directions is consistent, laying the foundation for subsequent deep cold rolling.
[0072] The microstructure diagram of the first deep cold rolled plate of this embodiment ( Figure 4) It can be seen that the grains show obvious elongation along the rolling direction. During the deep cold rolling process, the plastic deformation inside the material is mainly achieved through the formation of deformation twins because the low temperature environment suppresses the slip and climb mechanisms of dislocations. Twin boundaries can effectively hinder the movement of dislocations, thereby significantly improving the strength of the material at a lower deformation amount. The formation of twin boundaries also provides favorable nucleation points for the nucleation and growth of precipitates during post-aging treatment. In the intermediate aging treatment after deep cold rolling, the high-density dislocations near these twin boundaries provide favorable nucleation points for the nucleation and growth of precipitates, promote the uniform distribution of precipitates, and thus optimize the comprehensive mechanical properties of the material.
[0073] The grain boundary distribution diagram of the plate structure after intermediate aging treatment in this embodiment ( Figure 5 Left) It can be seen that the deformation twins still exist and are thermally stable. No significant twin boundary migration or merging occurs at the aging temperature of 450°C. SEM image of the plate structure after intermediate aging treatment in this embodiment ( Figure 5 Right) It can be seen that during the intermediate aging treatment, the alloy that has undergone the first deep cold rolling precipitates more fully. In addition to agglomeration along the ordinary grain boundaries, fine precipitates are also observed in the vicinity of the deformation twin bundles. These precipitates not only hinder the movement of dislocations, further improving the strength of the material, but also help to hinder the migration of grain boundaries, inhibit grain coarsening, and maintain the microstructural stability of the material. These precipitates work together with twins to significantly enhance the strength of the material by hindering dislocation movement. It should be noted that Figure 4 and Figure 5 Here, RD is the rolling direction, ND is the normal direction, TD is the transverse direction, and Σ3grain boundary represents the Σ3 type grain boundary (which can be used to represent the twin boundary in the material of the present invention).
[0074] TEM-EDS ( Figure 6 ), it can be seen that the precipitated phase (the arrow in the figure indicates the precipitated phase) has the characteristics of fine size and multi-scale distribution. Precipitated phases of different sizes can achieve a balance between strength and plasticity, among which fine precipitated phases help to improve strength, while larger precipitated phases help to maintain plasticity. From the element distribution map, it can be seen that the enriched areas of nickel and silicon (Si) elements in the local enlarged area are consistent, so it is inferred that the precipitated phase is mainly composed of Ni and Si elements.
[0075] Example 2
[0076] A method for preparing a high-strength and high-ductility Cu-Ni-Si alloy plate comprises:
[0077] S1. After the cast Cu-Ni-Si alloy (MAX251 copper alloy) with an initial thickness of 30 mm is solution treated at 900°C for 1 hour, it is hot rolled at 900°C for 4 times with a deformation amount of 20% of the initial thickness. Each pass needs to be kept warm for 5 minutes. After the last rolling pass, the material is water-cooled without insulation to obtain a hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm. At this time, the total deformation of the hot rolling is 80% of the initial thickness.
[0078] S2. The hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm was immersed in liquid nitrogen for 30 min, and was subjected to deep cold rolling at -196 to -150 ° C for 4 times with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and each pass was placed in liquid nitrogen for 10 min to obtain a first deep cold rolled sheet with a thickness of 3.6 mm. At this time, the total deformation amount was 40% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0079] S3. The first deep cold rolled sheet with a thickness of 3.6 mm was aged at 500° C. for 90 min, and then the aged material was immersed in liquid nitrogen for 30 min, and then the second deep cold rolled was performed at -196 to -150° C., firstly, two deep cold rollings were performed with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and then two deep cold rollings were performed with a deformation amount of 5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and each pass was immersed in liquid nitrogen for 10 min to obtain a second deep cold rolled sheet with a thickness of 1.8 mm, and the total deformation amount was 70% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0080] S4. After the second deep cold rolled plate is water-cooled, it is first subjected to low-temperature aging treatment at 250°C for 1 h, and then the temperature is increased to 450°C at a heating rate of 35°C / min for high-temperature aging treatment for 30 min to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate. Its performance data are shown in Table 1.
[0081] Example 3
[0082] A method for preparing a high-strength and high-ductility Cu-Ni-Si alloy plate comprises:
[0083] S1. After the cast Cu-Ni-Si alloy (KLFA85 copper alloy) with an initial thickness of 30 mm is solution treated at 900°C for 1 hour, it is hot rolled at 900°C for 4 times with a deformation amount of 20% of the initial thickness. The material needs to be kept warm for 5 minutes between each pass. After the last rolling pass, the material is water-cooled without insulation to obtain a hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm. At this time, the total deformation of the hot rolling is 80% of the initial thickness.
[0084] S2. The hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm was immersed in liquid nitrogen for 30 min, and was subjected to deep cold rolling at -196 to -150 ° C for 4 times with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and each pass was placed in liquid nitrogen for 10 min to obtain a first deep cold rolled sheet with a thickness of 3.6 mm. At this time, the total deformation amount was 40% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0085] S3. The first deep cold rolled sheet with a thickness of 3.6 mm was aged at 400°C for 90 min, and then the aged material was immersed in liquid nitrogen for 30 min, and the second deep cold rolled was performed at -196 to -150°C, firstly 3 passes of deep cold rolling with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and then 1 pass of deep cold rolling with a deformation amount of 5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy was performed, and each pass was immersed in liquid nitrogen for 10 min to obtain a second deep cold rolled sheet with a thickness of 1.5 mm, and the total deformation at this time was 75% of the initial thickness of the hot-rolled Cu-Ni-Si alloy;
[0086] S4. After the second deep cold rolled plate is water-cooled, it is first subjected to low-temperature aging treatment at 150°C for 1 h, and then the temperature is increased to 450°C at a heating rate of 35°C / min for high-temperature aging treatment for 30 min to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate. Its performance data are shown in Table 1.
[0087] Comparative Example 1
[0088] The method is basically the same as Example 1, except that: S4. After the second deep cold rolled plate is water-cooled, high temperature aging treatment is performed at 450°C for 30 minutes to obtain a Cu-Ni-Si alloy plate, and its performance data are shown in Table 1.
[0089] Comparative Example 2
[0090] A method for preparing a Cu-Ni-Si alloy plate comprises:
[0091] S1. After a cast Cu-Ni-Si alloy (C70250 copper alloy) with an initial thickness of 30 mm is solution treated at 900°C, it is hot rolled at 900°C for 4 passes with a deformation amount of 20% of the initial thickness. Each pass needs to be kept warm for 5 minutes. After the last rolling pass, the material is water-cooled without insulation to obtain a hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm. At this time, the total deformation is 80% of the initial thickness.
[0092] S2. The hot-rolled Cu-Ni-Si alloy having a thickness of 6 mm is subjected to room temperature rolling with a total deformation amount of 90% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and the deformation amount of each pass is 10% of the deformation amount of the previous pass to obtain a room temperature rolled plate;
[0093] S3. The room temperature rolled plate was aged at 450°C for 90 min to obtain a Cu-Ni-Si alloy plate, the performance data of which are shown in Table 1.
[0094] Comparative Example 3
[0095] A method for preparing a Cu-Ni-Si alloy plate comprises:
[0096] S1. After the cast Cu-Ni-Si alloy (C70250 copper alloy) with an initial thickness of 30 mm is solution treated at 900°C for 1 hour, it is hot rolled at 900°C for 4 times with a deformation amount of 20% of the initial thickness. The material needs to be kept warm for 5 minutes between each pass. After the last rolling pass, the material is water-cooled without insulation to obtain a hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm. At this time, the total deformation of the hot rolling is 80% of the initial thickness.
[0097] S2. The hot-rolled Cu-Ni-Si alloy with a thickness of 6 mm was subjected to 4 room temperature rolling with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy and aged at 450°C for 90 min, and then subjected to 4 more room temperature rolling with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy and aged at 450°C for 90 min to obtain a Cu-Ni-Si alloy sheet with a thickness of 1.2 mm. At this time, the total deformation amount is 80% of the initial thickness of the hot-rolled Cu-Ni-Si alloy. Its performance data are shown in Table 1.
[0098] Comparative Example 4
[0099] It is basically the same as Example 1, except that: S3. The first deep cold rolled plate with a thickness of 3.6 mm is aged at 450°C for 90 min, and then the aged material is immersed in liquid nitrogen for 30 min, and a second deep cold rolling is performed at -196 to -150°C. First, two deep cold rolling passes are performed with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and then one deep cold rolling pass is performed with a deformation amount of 5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy. Each pass needs to be immersed in liquid nitrogen for 10 min to obtain a second deep cold rolled plate with a thickness of 2.1 mm. At this time, the total deformation is 65% of the initial thickness of the hot-rolled Cu-Ni-Si alloy. Its performance data is shown in Table 1.
[0100] Comparative Example 5
[0101] It is basically the same as Example 1, except that: S3. The first deep cold rolled plate with a thickness of 3.6 mm is aged at 450°C for 90 min, and then the aged material is immersed in liquid nitrogen for 30 min, and a second deep cold rolling is performed at -196 to -150°C. First, 4 deep cold rolling passes are performed with a deformation amount of 10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy, and then 2 deep cold rolling passes are performed with a deformation amount of 5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy. Each pass needs to be immersed in liquid nitrogen for 10 min to obtain a second deep cold rolled plate with a thickness of 0.6 mm. At this time, the total deformation is 90% of the initial thickness of the hot-rolled Cu-Ni-Si alloy. Its performance data is shown in Table 1.
[0102] Comparative Example 6
[0103] The method is basically the same as Example 1, except that: S4. After the second deep cold rolled plate is water-cooled, it is first subjected to low-temperature aging treatment at 200°C for 1 hour, and then heated to 550°C at a heating rate of 35°C / min for high-temperature aging treatment for 30 minutes to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate, and its performance data are shown in Table 1.
[0104] Table 1. Performance data of Cu-Ni-Si alloy plates prepared in the embodiments of the present invention and the comparative examples
[0105] Hardness / HV Tensile strength / MPa Elongation / % Electrical conductivity / %IACS Example 1 265.3 892 11.7 37.3 Example 2 252.8 840 11.0 37.1 Example 3 261.2 877 11.6 36.9 Comparative Example 1 242.5 799 9.5 36.1 Comparative Example 2 230.1 728 10.1 26.6 Comparative Example 3 218.4 708 9.8 36.2 Comparative Example 4 231.3 736 9.2 34.3 Comparative Example 5 238.6 762 10.2 36.3 Comparative Example 6 234.1 745 11.5 37.4
[0106] The mechanical properties and electrical conductivity of the Cu-Ni-Si alloy sheet of the present invention under different rolling-aging processes are shown in Table 1. Compared with the alloy sheet with 90% deformation obtained by the conventional "one-step room temperature rolling-ordinary aging treatment" in Comparative Example 2, the alloy sheet obtained by "first deep cold rolling-intermediate aging treatment-second deep cold rolling-ordinary aging treatment" in Comparative Example 1 has an increase of 71MPa in tensile strength and 9.5%IACS in electrical conductivity; compared with the alloy sheet with 80% deformation obtained by "room temperature rolling-ordinary aging treatment-room temperature rolling-ordinary aging treatment" in Comparative Example 3, the elongation and electrical conductivity of the alloy sheet obtained by "first deep cold rolling-intermediate aging treatment-second deep cold rolling-ordinary aging treatment" in Comparative Example 1 are not much different, and the tensile strength is significantly improved. It can be seen that the use of two deep cold rollings is conducive to the significant improvement of the tensile strength of the alloy sheet. Compared with Comparative Example 1, the tensile strength of the alloy sheet obtained by "first deep cold rolling-intermediate aging treatment-second deep cold rolling-graded aging treatment" in Example 1 is increased by 93MPa, the elongation is increased by 2.2%, and the conductivity is also increased to 37.3%IACS. It can be seen that the graded aging treatment after two deep cold rollings is conducive to further improvement of tensile strength, elongation, and conductivity, and greatly improves the comprehensive performance of the alloy sheet. Compared with Example 1, the small total deformation amount of Comparative Example 4 leads to a decrease in the internal energy storage of the material. After the graded aging treatment, the number of precipitated phases is reduced. The tensile strength, conductivity and elongation of the Cu-Ni-Si alloy sheet finally obtained are greatly reduced, the tensile strength is reduced by 156MPa, the conductivity is reduced by 3%IACS, and the elongation is reduced by 2.5%. Compared with Example 1, due to the excessive total deformation, self-annealing occurred in the secondary deep cold rolling process in Comparative Example 5, resulting in a reduction in the number of precipitated phases in the subsequent graded aging process. The tensile strength, electrical conductivity and elongation of the Cu-Ni-Si alloy sheet finally obtained were greatly reduced, with the tensile strength reduced by 130MPa, the electrical conductivity reduced by 1%IACS, and the elongation reduced by 1.5%. Compared with Example 1, the temperature of the high temperature stage of graded aging in Comparative Example 6 was increased, resulting in recrystallization of the alloy, and the precipitated phase became relatively coarse. The electrical conductivity and elongation of the Cu-Ni-Si alloy sheet finally obtained were not much different, but the tensile strength was greatly reduced (reduced by 147MPa).
[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high-strength and high-ductility Cu-Ni-Si alloy sheet, characterized in that: The preparation method comprises: The hot-rolled Cu-Ni-Si alloy is subjected to a first deep cold rolling, an intermediate aging treatment and a second deep cold rolling to obtain a deep cold rolled plate; the total deformation after the first deep cold rolling is 40-45% of the initial thickness of the hot-rolled Cu-Ni-Si alloy; the total deformation after the second deep cold rolling is 70-80% of the initial thickness of the hot-rolled Cu-Ni-Si alloy; The deep cold rolled plate is subjected to graded aging treatment to obtain a high-strength and high-ductility Cu-Ni-Si alloy plate.
2. The preparation method according to claim 1, characterized in that: The hot-rolled Cu-Ni-Si alloy is obtained by subjecting the cast Cu-Ni-Si alloy to solid solution treatment and hot rolling; Preferably, the temperature of the solution treatment is the same as the temperature of the hot rolling; More preferably, the temperature of the solution treatment and the hot rolling is 850-950° C.; and / or the time of the solution treatment is 1-2 h.
3. The preparation method according to claim 2, characterized in that: The total deformation after hot rolling is 70-80% of the initial thickness of the cast Cu-Ni-Si alloy; The deformation amount of each pass during the hot rolling process is 15-25% of the initial thickness of the cast Cu-Ni-Si alloy; and / or The holding time between each pass in the hot rolling process is 5 to 10 minutes.
4. The preparation method according to claim 1, characterized in that: The deformation amount of each pass in the first deep cold rolling process is 5-10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
5. The preparation method according to claim 1, characterized in that: The temperature of the intermediate aging treatment is 400-500°C, preferably 425-475°C; and / or The intermediate aging treatment time is 60 to 120 minutes.
6. The preparation method according to claim 1, characterized in that: The second deep cold rolling includes a first stage and a second stage, and the deformation amount of each pass in the second stage is smaller than the deformation amount of each pass in the first stage.
7. The preparation method according to claim 6, characterized in that: The deformation amount of each pass in the first stage is 8-10% of the initial thickness of the hot-rolled Cu-Ni-Si alloy; and / or The deformation amount of each pass in the second stage is 3-5% of the initial thickness of the hot-rolled Cu-Ni-Si alloy.
8. The preparation method according to claim 7, characterized in that: The graded aging treatment includes a primary aging treatment and a secondary aging treatment, and the temperature of the secondary aging treatment is higher than the temperature of the primary aging treatment.
9. The preparation method according to claim 8, characterized in that: The temperature of the primary aging treatment is 150-250°C; and / or The temperature of the secondary aging treatment is not higher than the temperature of the intermediate aging treatment.
10. A high-strength and high-ductility Cu-Ni-Si alloy sheet, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Beryllium-free super high-strength high-toughness copper alloy and preparation method thereof
CN114990380A
Preparation method of copper-based metal glass composite material with multi-scale structure
CN115058615A
High-strength and high-plasticity conductive copper alloy material and preparation method thereof
CN115961227A
Short-process preparation method of high-strength copper-nickel-silicon alloy
CN117867425A
Preparation method of high-strength copper-nickel-silicon alloy
CN117867426A