Electroplating process for backboard film of electronic product
By using silicon-aluminum alloy material and magnetron sputtering process on the back plate of electronic products, combined with grafting treatment, the problems of low light transmittance and easy oxidation and fall-off of the back plate film are solved, and high light transmittance and corrosion resistance are achieved The back plate film improves heat dissipation and aesthetic effect.
Patent Information
- Application Number
- CN202410912328.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-12-03
AI Technical Summary
The electroplating layer of the back plate film of existing electronic products has low light transmittance and is prone to oxidation and fall off, affecting heat dissipation and aesthetic performance.
Using silicon-aluminum alloy material as the target material, an electroplating layer is formed on the PMMA/PC composite substrate through magnetron sputtering process, and the product inspection, dust removal and grafting are carried out during the sputtering process, combined with specific sputtering parameters and the coating step to form a stable and transparent back plate film.
It improves the light transmittance and corrosion resistance of the back plate film, reduces the fall off and oxidation of the electroplating layer, and enhances the heat dissipation performance and the aesthetic performance of the pattern.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the field of electroplating, and more specifically, to an electroplating process for a backplane film of an electronic product. Background Art
[0002] Electronic products are related products that use electricity as the basis for their work, mainly including: watches, smart phones, telephones, televisions, DVD players, VCRs, camcorders, radios, tape recorders, combination speakers, laser turntables, computers, game consoles, tablets, mobile communication products, etc.
[0003] With the advancement of science and technology, electronic products are becoming more and more advanced, and users are also increasingly demanding on the performance, quality, and appearance of electronic products. In particular, for electronic products such as mobile phones, computers, and tablets, users are not only concerned about their functions, but also about heat dissipation, breakage resistance, wear resistance, and aesthetics.
[0004] The materials used for the back cover of mobile phones, computers, and tablets are mainly plastic, glass, ceramics, and metals. Among them, the metal back cover has better heat dissipation performance, but the oxidation-reduction process is required during the processing to improve the corrosion resistance of the metal, and the oxidation-reduction process is easy to pollute the environment. Glass, ceramics, etc. have poor heat dissipation effects, and the plastic back cover has poor heat dissipation effects.
[0005] Based on the above problems, glass, ceramics and other substrates are used, and then dyed or printed with exquisite patterns, and then a backplane film containing an electroplating layer is attached to the substrate to protect the exquisite patterns and also to dissipate heat. The current backplane film electroplating layer is electroplated by magnetron sputtering coating, electron beam evaporation coating and other processes. The commonly used target materials in the electroplating process include metal materials, ceramic materials, alloy materials, etc. Since metal materials are easily corroded and ceramic materials have low light transmittance, alloy materials are the best choice.
[0006] However, the transmittance of the electroplated layer of the backplane film formed by vacuum evaporation of the current alloy material is low, which in turn affects the color of the backplane or the presentation of exquisite patterns. At the same time, after the backplane film is used to produce the backplane of electronic products such as mobile phones, the electroplated layer is still prone to falling off and oxidation. Therefore, further research is needed. Summary of the invention
[0007] In order to obtain light transmittance and reduce oxidation, shedding and other phenomena, the present application provides an electroplating process for a backplane film of an electronic product.
[0008] This application provides a technical solution that adopts the following: In the first aspect, the present application provides a technical solution using the following: An electroplating process for a backplane film of an electronic product comprises the following steps: 1) The substrate is subjected to quality inspection and dust removal treatment in sequence to obtain a qualified substrate; 2) Using silicon-aluminum alloy material as the target material, through magnetron sputtering, a layer of electroplating layer is plated on the surface of the qualified substrate to obtain a semi-finished product; 3) Laminating the surface of the electroplated layer of the semi-finished product to obtain a backplane film; Among them, the sputtering gas pressure is 0.3-0.8Pa, the sputtering power is 5-20Kw, the target substrate distance is 20-80mm, the sputtering temperature is 70-80℃, the sputtering time is 1-3min, and the gas flow rate is 300-800ml / min.
[0009] The electroplating process of the present application is simple to operate and has high production efficiency. The obtained backplane film will not bubble or fall off when boiled in water at 100°C for 60 minutes. At the same time, it has good light transmittance and corrosion resistance. Therefore, when used for the backplane of electronic products, it can protect the pattern on the backplane, play a role in heat dissipation, and can well present the beauty of the pattern on the backplane.
[0010] Specifically, the substrate is inspected, qualified products are screened, and dust removal is performed to remove dust and other impurities adsorbed on the surface of the substrate to ensure the cleanliness and flatness of the substrate surface, so that the obtained qualified products can be used for coating, and the formed electroplating layer is stably connected to the substrate, reducing the possibility of the electroplating layer falling off.
[0011] Silicon aluminum alloy has a low thermal expansion coefficient, good thermal conductivity, good chemical stability and oxidation protection ability. Therefore, after magnetron sputtering, the electroplated layer formed has better corrosion resistance, thermal conductivity, etc. At the same time, the obtained back panel film has better light transmittance. Therefore, it can be used on the back panels of mobile phones to better present patterns.
[0012] The electroplating layer is coated to prevent it from being scratched or adsorbing dust during transportation or storage.
[0013] The thickness of the electroplated layer of the present application is preferably 60-180nm, and combined with the magnetron sputtering process conditions of the present application, such as sputtering gas pressure of 0.3-0.8Pa, sputtering power of 5-20Kw, target-substrate distance of 20-80mm, sputtering temperature of 70-80℃, and gas flow rate of 300-800ml / min, the electroplated layer can be stably adhered to the surface of the substrate, and can be boiled in 100℃ water for more than 80min, indicating that, through the parameter setting of the present application, the obtained electroplated layer has better adhesion to the substrate.
[0014] In addition, the sputtering time of the present application is 1-3 minutes.
[0015] In summary, the present application ensures the quality of the substrate layer through quality inspection, dust removal and other processes, and adopts silicon-aluminum alloy as the target material, and cooperates with the settings of the sputtering gas pressure, sputtering power, target-substrate distance, sputtering temperature, sputtering time, air flow rate and other settings of the present application, so that the electroplated layer of the backplane film obtained has thermal conductivity, and at the same time has the advantages of good oxidation protection ability, good adhesion and not easy to fall off, and good light transmittance.
[0016] Preferably, the substrate is a PMMA / PC composite material.
[0017] PMMA / PC composite materials have the advantages of both PMMA and PC, and have the advantages of high light transmittance, high toughness, etc. At the same time, it is easy to produce a stable electroplating layer on its surface. Therefore, the prepared backplane film is not prone to falling off during use, and the backplane film also obtains a higher light transmittance.
[0018] The light transmittance of the PMMA / PC composite material of the present application is 90-91%, and preferably 90.8% in the embodiment.
[0019] Preferably, the silicon-aluminum alloy material has the following chemical components in weight percentage: Si15-28% Trace chemical ingredients 0.3-0.5% The balance is Al and inevitable impurities.
[0020] The above raw material ratio is within the preferred range of the present application. After alloying the above Si and Al, the obtained silicon-aluminum alloy has better oxidation protection ability and reduces the corrosion of the backplane film.
[0021] Preferably, the trace chemical components are one or more of Fe, Cu, Mn, Ni, Ti, O, N, and C.
[0022] When the silicon-aluminum alloy of the present application contains one or more trace elements composed of the above Fe, Cu, Mn, Ni, Ti, O, N, and C, the corrosion resistance of the silicon-aluminum alloy is better, and the element distribution of the formed silicon-aluminum alloy is uniform and the light transmittance is better.
[0023] Preferably, the step 1) further comprises surface treatment of the substrate, and the specific process of the step 1) is as follows: The substrate is subjected to quality inspection and dust removal treatment in turn, and then placed in a grafting solution, and grafted by a radiation grafting method to form a grafted layer on its surface to obtain a qualified substrate.
[0024] Since the surface of PMMA / PC composite material is smooth, the inorganic material silicon aluminum alloy is not easy to adsorb on its surface after magnetron sputtering. Therefore, grafted materials are introduced on the surface of the substrate to improve the activity of the PMMA / PC material surface and enhance the adhesion stability of the electroplated layer formed on its surface.
[0025] Preferably, the grafting liquid is composed of acrylate, sodium silicate, inhibitor, water and initiator; the acrylic monomer is composed of at least two of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane and acrylic acid.
[0026] The above-mentioned γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane both have good adhesion to silicon, aluminum and other materials. When combined with acrylic monomers, a grafted layer is formed on the surface of the substrate after radiation grafting. The grafted layer has good adhesion to aluminum alloy materials. Therefore, after electroplating, the formed electroplated layer is stably connected to the substrate, thereby reducing the possibility of the electroplated layer falling off after long-term use of the back panel film of electronic products.
[0027] Preferably, the step 1) also includes further connecting the substrate after radiation grafting. The specific process is: the substrate is inspected and dust-removed in sequence, and then placed in a grafting liquid, and grafted by radiation grafting to form a grafting layer on its surface, and a connecting liquid is applied on the surface of the grafted layer, pre-cured to form a flat grafted film on its surface, and rinsed to obtain a qualified substrate.
[0028] Since it is difficult to ensure that the surface of the grafted layer is smooth after grafting during the radiation grafting process, the surface of the grafted layer of the substrate is rough after radiation grafting, thereby reducing the light transmittance of the substrate; therefore, the present application further uses a connecting liquid to coat the surface of the grafted layer of the substrate, and makes the surface smooth after curing. At the same time, the grafting liquid can further react with the active groups on the surface of the substrate to form a structurally stable grafted film. Since the grafted layer also has good adhesion, it is easy to adhere to the silicon-aluminum alloy material to form a backplane film with a stable layer structure, thereby reducing the occurrence of falling off and the like.
[0029] The pre-curing of the present application is to form a grafted film with a humidity of 52-58% by heating, so as to facilitate the subsequent magnetron sputtering and ensure a stable connection between the formed electroplated layer and the grafted layer.
[0030] Preferably, the connecting liquid consists of a connecting monomer, ammonium persulfate and a solvent.
[0031] Preferably, the linking monomer is 1,2-bis(triethoxysilyl)ethane and / or 2,2-dihydroxymethylpropionic acid.
[0032] 2,2-Dihydroxymethylpropionic acid is an organic compound with two hydroxymethyl groups, one carboxyl group and one methyl group. It has the characteristics of both alcohol and acid compounds and has excellent cross-linking properties. 1,2-Bis(triethoxysilyl)ethane has good adhesion to alloy materials. Therefore, Preferably, the thickness of the grafted film is less than 150 nm.
[0033] In summary, this application has the following beneficial effects: 1. The present application ensures the quality of the substrate layer through quality inspection, dust removal and other processes. By using silicon-aluminum alloy as the target material and coordinating the sputtering gas pressure, sputtering power, target-substrate distance, sputtering temperature, sputtering time, air flow rate and other settings of the present application, the electroplated layer of the backplane film obtained has thermal conductivity, and at the same time has the advantages of good oxidation protection ability, good adhesion and not easy to fall off, and good light transmittance.
[0034] 2. Both γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane have good adhesion to silicon, aluminum and other materials. When combined with acrylic monomers, a grafted layer is formed on the surface of the substrate after radiation grafting. The grafted layer has good adhesion to aluminum alloy materials. Therefore, after electroplating, the formed electroplated layer is stably connected to the substrate, thereby reducing the possibility of the electroplated layer falling off after long-term use of the back panel film of electronic products.
[0035] 3. Use connecting liquid to coat the surface of the grafted layer of the substrate. After curing, the surface is smoothed. At the same time, the grafted liquid can further react with the active groups on the surface of the substrate to form a grafted film with a stable structure. Since the grafted layer also has good adhesion, it is easy to adhere to the silicon-aluminum alloy material to form a backplane film with a stable layer structure, reducing the occurrence of shedding and other phenomena. DETAILED DESCRIPTION
[0036] The present application is further described in detail below with reference to the embodiments. Example
[0037] Example 1 An electroplating process for a backplane film of an electronic product comprises the following steps: 1) Use PMMA / PC composite material as the substrate, and inspect the substrate in turn, such as checking whether there are bending, defects, scratches, etc. If there are no such phenomena, put the substrate into a dust collector for dust removal. After all the dust and other impurities attached to the surface of the substrate are removed, a qualified substrate is obtained.
[0038] 2) A silicon-aluminum alloy material is used as a target material, a qualified substrate is used as a base, and is placed in a magnetron sputtering device, argon gas is introduced, and the parameters are set. The sputtering gas pressure is 0.8 Pa, the sputtering power is 5 kW, the target-substrate distance is 20 mm, the sputtering temperature is 80°C, and the gas flow rate is 300 ml / min, so that one side of the qualified substrate is plated with an electroplating layer with an average thickness of 120 nm to obtain a semi-finished product.
[0039] 3) A PET protective film is attached to one side of the electroplated layer of the semi-finished product to obtain a backplane film.
[0040] The chemical composition of the silicon aluminum alloy material is shown in Table 1 below.
[0041] Example 2 The difference between Example 2 and Example 1 is that the sputtering gas pressure is 0.5 Pa, the sputtering power is 10 Kw, the target substrate distance is 50 mm, the sputtering temperature is 70° C., and the gas flow rate is 400 ml / min. The chemical composition of the silicon aluminum alloy material is shown in Table 1 below.
[0042] Example 3 The difference between Example 3 and Example 1 is that the sputtering gas pressure is 0.3 Pa, the sputtering power is 20 Kw, the target substrate distance is 80 mm, the sputtering temperature is 70°C, the sputtering time is 3 min, and the gas flow rate is 800 ml / min. The chemical composition of the silicon aluminum alloy material is shown in Table 1 below.
[0043] Embodiment 4-5 The difference between Example 4-5 and Example 1 is that the chemical composition of the silicon aluminum alloy material is different, as shown in Table 1; Table 1 Chemical composition of silicon aluminum alloy materials of Examples 1-3 (%) chemical composition Example 1 Example 2 Example 3 Example 4 Example 5 Al 84.5 76.677 71.7 84.5 84.5 Si 15.0 23.0 28.0 15.0 15.0 Fe 0.018 0.018 0.018 0 0.128 Cu 0.06 0.06 0.06 0 0.297 Mn 0.03 0.03 0.03 0.048 0 Ni 0.237 0.06 0.06 0.237 0 Ti 0.08 0.08 0.06 0.14 0 o 0.05 0.05 0.05 0.05 0.05 N 0.015 0.015 0.012 0.015 0.015 C 0.01 0.01 0.01 0.01 0.01 Example 6 The difference between Example 6 and Example 2 is that: in step 1), the substrate is further subjected to surface treatment. The specific process of step 1) is as follows: 1) Using PMMA / PC composite material as the substrate, the substrate is inspected in turn, such as whether there is bending, incompleteness, scratches, etc. If there is no such phenomenon, the substrate is placed in a dust collector for dust removal. After all the dust and other impurities attached to the surface of the substrate are removed, the dust-removed substrate is placed in an electron irradiation chamber, and one side of it is irradiated, wherein the electron beam current intensity is 2 mA, the irradiation dose is 100 kGy, and the irradiation is performed for 30 minutes to obtain an irradiated substrate.
[0044] The irradiated substrate was placed in a grafting solution and subjected to grafting reaction for 1 hour in a constant temperature water bath at 60°C to form a grafting layer on its irradiated surface. The ungrafted monomers on the surface were then washed away to obtain a qualified substrate.
[0045] After magnetron sputtering, an electroplating layer with an average thickness of 120 nm is plated on one side of the grafted layer of the qualified substrate.
[0046] The grafting solution is obtained by the following method: 8 kg of acrylate monomer, 0.1 kg of sodium sulfate, 0.5 kg of ammonium persulfate and 50 kg of water were weighed and put into a stirring device, and stirred at a speed of 100 r / min for 20 min to obtain a grafting solution.
[0047] The acrylate monomer consists of 7 kg of acrylic acid and 1 kg of γ-methacryloxypropyltrimethoxysilane.
[0048] Example 7 The difference between Example 7 and Example 6 is that the acrylate monomer consists of 7 kg of acrylic acid and 1 kg of vinyltrimethoxysilane.
[0049] Example 8 The difference between Example 8 and Example 6 is that the acrylate monomer consists of 6 kg of acrylic acid, 1.5 kg of γ-methacryloxypropyltrimethoxysilane, and 0.5 kg of vinyltrimethoxysilane.
[0050] Example 9 The difference between Example 9 and Example 8 is that: step 1) further includes further connecting the substrate after radiation grafting, and the specific process of step 1) is: 1) Using PMMA / PC composite material as the substrate, the substrate is inspected in turn, such as checking whether there are bending, incompleteness, scratches and the like. If there are no such phenomena, the substrate is placed in a dust removal machine for dust removal. After all the dust and other impurities attached to the surface of the substrate are removed, the dust-removed substrate is placed in an electron irradiation chamber for irradiation, wherein the electron beam current intensity is 2 mA, the irradiation dose is 100 kGy, and the irradiation is performed for 30 minutes to obtain an irradiated substrate.
[0051] The grafting liquid of the irradiated substrate is subjected to grafting reaction for 1 hour in a constant temperature water bath at 60° C. to form a grafting layer on its surface, thereby obtaining a grafted substrate; The grafted layer of the grafted substrate is coated with a connecting liquid and pre-cured at a temperature of 100°C to form a connecting layer with a humidity of 55% on the surface of the connecting layer, thereby forming a smooth grafted film on the surface of the substrate. The average thickness of the grafted film is 98nm, and a qualified substrate is obtained.
[0052] The grafted membrane of the present application comprises a grafted layer and a connecting layer.
[0053] After magnetron sputtering, a plating layer with an average thickness of 120 nm is plated on one side of the qualified substrate grafted film.
[0054] In addition, step 3) also includes further drying the semi-finished product, and the specific process is as follows: The semi-finished product was placed in a 95°C oven and dried for 5 minutes, and a PET protective film was attached to the electroplated layer side of the semi-finished product to obtain a backplane film.
[0055] Because, after coating, in order to further ensure that the connecting layer is completely cured, it is necessary to put it into an oven for drying to make it completely cured, and then stably connect the electroplating layer to the surface of the substrate to reduce the possibility of falling off.
[0056] The connection liquid was prepared by the following method: 5 kg of connecting monomer, 0.5 kg of ammonium persulfate, 0.1 kg of sodium sulfate and 15 kg of water were weighed and put into a stirring device and stirred at a speed of 100 r / min for 20 minutes to obtain a connecting liquid.
[0057] The linking monomer is 1,2-bis(triethoxysilyl)ethane.
[0058] Example 10 The difference between Example 10 and Example 9 is that the linking monomer consists of 4 kg 1,2-bis(triethoxysilyl)ethane and 1 kg 2,2-dihydroxymethylpropionic acid.
[0059] Embodiment 11 The difference between Example 11 and Example 6 is that the specific process of step 1) is as follows: PMMA / PC composite material is used as the substrate, and the substrate is inspected in turn, such as whether there are bends, defects, scratches, etc. If there are no such phenomena, the substrate is placed in a dust collector for dust removal. After all the dust and other impurities attached to the surface of the substrate are removed, the dust-removed substrate is coated with a connecting liquid, pre-cured at a temperature of 100°C, and a connecting layer (8μm grafted film) with a humidity of 55% is formed on the surface of the substrate to obtain a qualified substrate.
[0060] The connection liquid was prepared by the following method: 7 kg of acrylic acid, 1 kg of γ-methacryloxypropyltrimethoxysilane, 5 kg of 1,2-bis(triethoxysilyl)ethane, 0.5 kg of ammonium persulfate, and 65 kg of water were weighed and put into a stirring device and stirred at a speed of 100 r / min for 30 min to obtain a connecting liquid.
[0061] Example 12 The difference between Example 12 and Example 11 is that the connecting liquid is prepared by the following method: 5 kg of connecting monomer, 0.5 kg of ammonium persulfate, and 15 kg of water are weighed and put into a stirring device at a speed of 100 r / min, and stirred for 20 minutes to obtain a connecting liquid.
[0062] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the sputtering gas pressure is 0.1Pa.
[0063] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the sputtering temperature is 50°C.
[0064] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that Si in the chemical composition of the silicon-aluminum alloy material is replaced by B.
[0065] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that Si in the chemical composition of the silicon-aluminum alloy material is replaced by Ag.
[0066] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that Si is 5%, and Al and inevitable impurities are 94.5%.
[0067] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that the chemical composition of the silicon-aluminum alloy material does not contain trace elements, wherein Si accounts for 15%, and Al and unavoidable impurities account for 85%.
[0068] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that the substrate is preferably PET (light transmittance is 90.8%).
[0069] Performance testing Detection method / test method Light transmittance Test (1): The backplane films of Examples 1-12 and Comparative Examples 1-7 were placed at room temperature for 2 hours, and then the transmittance was measured using a spectrophotometer.
[0070] Adhesion stability Test (2): The backplane membranes of Examples 1-5 and Comparative Examples 3-6 were placed in a boiling device and boiled at 100°C. After 60 minutes, the membranes were taken out and observed to see if any bubbling, peeling or other phenomena occurred on the surface of the electroplated layer. If any of the above phenomena occurred, the membranes were deemed unqualified. If no such phenomena occurred, the membranes were continued to be boiled and taken out for observation every 10 minutes. If any bubbling, peeling or other phenomena occurred, the total boiling time was recorded. If the total boiling time reached 180 minutes and no bubbling, peeling or other phenomena occurred, the boiling time was recorded as >180 minutes. The specific data are shown in Table 2.
[0071] Test (3): The backsheet films of Examples 1-12 and Comparative Examples 1-7 were placed in a salt spray machine, wherein the solution was 5% sodium chloride, the temperature was 38° C., the humidity was 85%, and the test time was 72 hours. The light transmittance was then tested.
[0072] The above experiments were tested 3 times and the average value was taken. The specific data are shown in Table 2; Table 2 Experimental data of Examples 1-12 and Comparative Examples 1-7 Combining Example 1 and Comparative Examples 1-2 and Table 2, it can be seen that Comparative Examples 1-2 are boiled in water at 100 degrees Celsius for less than 60 minutes, while the boiling time of the embodiment is as high as 95 minutes, indicating that the electroplating layer formed by the electroplating process of the present application has better adhesion stability.
[0073] Combining Example 1 and Comparative Examples 3-6, it can be seen that the reduction in transmittance of Comparative Examples 3-6 after salt spray treatment is greater than that of Example 1, indicating that the silicon-aluminum alloy material with the chemical composition of the present application has better corrosion resistance, reduces the electroplating layer formed thereon and has better oxidation resistance, reduces the possibility of oxidation of the electronic product backplane film after long-term use, and reduces its transmittance, and the pattern on the backplane of the electronic product is presented.
[0074] Combining Example 2 and Example 6 with Table 2, it can be seen that the boiling time of Example 6 is longer than that of Example 2, indicating that the grafted film obtained by the radiation grafting method is easy to adhere to the silicon-aluminum alloy material, thereby improving the layer structure stability of the backplane film, reducing blistering, wear, and falling off after being applied to the backplane, and improving the practicability of the backplane film.
[0075] It can be seen from the structure of Example 9 and Example 8 combined with Table 2 that the boiling time of Example 9 is longer than that of Example 8, and the light transmittance of test (1) is also higher than that of Example 8, indicating that the present application applies a connecting layer on the grafted layer, and the obtained grafted film has a better adhesion effect on the silicon-aluminum alloy layer material, so that the grafted layer is closely connected to the electroplated layer, reducing the possibility of the electroplated layer on the backplane film falling off. This improves the practicality of the backplane film.
[0076] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An electroplating process for a backplane film of an electronic product, characterized in that: The following steps are involved: 1) Perform quality inspection and dust removal on the substrate in turn to obtain a qualified substrate; 2) Using silicon-aluminum alloy material as the target material, through magnetron sputtering, a layer of electroplating layer is plated on the surface of the qualified substrate to obtain a semi-finished product; 3) Laminating the surface of the electroplated layer of the semi-finished product to obtain a backplane film; Among them, the sputtering gas pressure is 0.3-0.8Pa, the sputtering power is 5-20Kw, the target-substrate distance is 20-80mm, the sputtering temperature is 70-80℃, and the gas flow rate is 300-800ml / min.
2. The electroplating process for the backplane film of an electronic product according to claim 1, characterized in that: The substrate is a PMMA / PC composite material.
3. The electroplating process of the backplane film of an electronic product according to claim 1, characterized in that: The silicon aluminum alloy material has the following chemical components in weight percentage: Si15-28% Trace chemical ingredients 0.3-0.5% The balance is Al and inevitable impurities.
4. The electroplating process of the backplane film of an electronic product according to claim 3, characterized in that: The trace chemical components are one or more of Fe, Cu, Mn, Ni, Ti, O, N, and C.
5. The electroplating process of the backplane film of an electronic product according to claim 1, characterized in that: The step 1) further includes surface treatment of the substrate. The specific process of the step 1) is as follows: The substrate is subjected to quality inspection and dust removal treatment in turn, and then placed in a grafting solution, grafted by a radiation grafting method to form a grafted layer on its surface, and then rinsed to obtain a qualified substrate.
6. The electroplating process for the backplane film of an electronic product according to claim 5, characterized in that: The grafting liquid is composed of acrylate monomer, polymerization inhibitor, water and initiator; the acrylic acid monomer is composed of at least two of gamma-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane and acrylic acid.
7. The electroplating process for the backplane film of an electronic product according to claim 5, characterized in that: The step 1) also includes further connecting the substrate after radiation grafting. The specific process is: the substrate is inspected and dust-removed in sequence, and then placed in a grafting liquid, and grafted by radiation grafting to form a grafting layer on its surface, and a connecting liquid is applied on the surface of the grafted layer, pre-cured to form a flat grafting film on its surface, and rinsed to obtain a qualified substrate.
8. The electroplating process for the backplane film of an electronic product according to claim 7, characterized in that: The connecting liquid consists of a connecting monomer, sodium sulfate, ammonium persulfate and a solvent.
9. The electroplating process for the backplane film of an electronic product according to claim 7, characterized in that: The linking monomer is 1,2-bis(triethoxysilyl)ethane and / or 2,2-dihydroxymethylpropionic acid.
10. The electroplating process for the backplane film of an electronic product according to any one of claim 7, characterized in that: The thickness of the grafted film is less than 150 nm.