Phase shift mask substrate alloy target material and manufacturing method thereof

A molybdenum-silicon alloy target with carbon elements addresses the issues of poor film quality, high costs, and safety hazards in phase-shift film formation by directly incorporating carbon, enhancing film uniformity and stability without using hazardous gases.

CN119061361APending Publication Date: 2024-12-03SHANGHAI CHUANXIN SEMICON CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411173192.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing method of introducing a carbon source into phase-shift films in semiconductor manufacturing using gases like CH4, CO, and CO2 results in poor film quality, high production costs, and potential safety hazards due to increased gas partial pressure and the use of flammable or toxic gases.

Method used

A phase-shift mask substrate alloy target material composed of molybdenum, silicon, and carbon, with a mass ratio of 0.1% to 1% carbon and 1:4 to 1:9 Mo/Si, is used to introduce carbon directly into the film formation process, eliminating the need for carbon-containing gases and improving film formation rate, flatness, and stability.

Benefits of technology

The solution enhances film quality, reduces production costs, and improves safety by avoiding high-pressure gases and toxic substances, resulting in a more stable and uniform film with reduced grain size and improved sputtering efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061361A_ABST
    Figure CN119061361A_ABST
Patent Text Reader

Abstract

The invention provides a phase shift mask base plate alloy target material and a manufacturing method thereof, and the manufacturing method of the phase shift mask base plate alloy target material comprises the following steps: uniformly mixing high-purity Mo powder and Si powder to obtain Mo and Si mixed powder; adding a carbon-containing substance into the Mo and Si mixed powder, and uniformly mixing to obtain carbon-containing Mo and Si mixed powder; the preparation method comprises the following steps: preparing carbon-containing Mo and Si mixed powder into a prefabricated blank by adopting an isostatic pressing process; preparing the prefabricated blank into a phase shift mask base plate alloy target blank by adopting a high-temperature sintering process; and welding the phase shift mask base plate alloy target blank and a back plate to prepare the phase shift mask base plate alloy target material. According to the manufacturing method of the phase shift mask base plate alloy target material, the product stability of the phase shift mask base plate alloy target material can be improved, and the technical problems that in the prior art, a method for introducing a carbon source into a phase shift film is poor in film forming quality and high in production cost, and potential safety hazards exist can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of integrated circuit manufacturing, and in particular to a phase-shift mask substrate alloy target material and a manufacturing method thereof. Background Art

[0002] Semiconductor components are manufactured through a series of processes from wafer, oxidation, exposure to packaging. Among these eight processes, the most important is the exposure process. The exposure process uses a photomask (also known as a photomask, mask, or mask plate) as the original plate and uses exposure equipment to reduce the line width of the projected circuit on the wafer.

[0003] A photomask is a product that uses electron beam exposure technology to etch a fine circuit pattern on a mask substrate. The mask substrate is formed by forming a multi-layer chromium film on a quartz substrate and coating the multi-layer chromium film with photoresist. With the high integration of semiconductor integrated circuits, the photomask route for forming patterns also tends to be high-precision and refined. In order to form finer patterns in semiconductor integrated circuits, high pattern resolution is required. Phase-shift inversion film masks use both the intensity and phase of light to form images, have higher resolution, and are widely used in semiconductor photolithography processes with higher requirements.

[0004] The phase shift mask is a metal film containing MoxSiy compounds deposited on the surface of a glass substrate, so that the light produces a 180-degree phase difference when passing through the film area, thereby enhancing the contrast of the image and improving the resolution. In order to further optimize the performance of the phase shift film, carbon elements can be introduced into the phase shift film (MoSi metal film). After adding carbon elements, the corrosion resistance, mechanical strength and stability of the phase shift film can be enhanced, and the light transmittance and conductivity of the phase shift film can also be improved. The method commonly used in the prior art to introduce a carbon source into the phase shift film is to introduce gases such as CH4, CO and CO2 as carbon sources during the vacuum sputtering process, and to form multi-element metal films or dielectric films such as MoSiONC, MoSiC or MoSiOC by introducing carbon-containing gases. However, the existing method of introducing a carbon source into the phase shift film uses gas as a carbon source. The addition of gas increases the gas partial pressure of the negative ion gas in the sputtering chamber, resulting in a decrease in the film forming rate and the film flatness, which affects the film forming quality of the phase shift film. In addition, the use of high-pressure gas increases the production cost, and the carbon source gas includes flammable or toxic gases, which poses a production safety hazard. Therefore, the existing method of introducing a carbon source into a phase-shift film has technical problems such as poor film quality, high production cost and potential safety hazards. Summary of the invention

[0005] The object of the present invention is to provide a phase shift mask substrate alloy target and a manufacturing method thereof, so as to solve the technical problems of poor film quality, high production cost and potential safety hazards in the existing method of introducing a carbon source into a phase shift film.

[0006] To achieve the above-mentioned purpose, on the one hand, the present invention provides a phase-shift mask substrate alloy target material, including a phase-shift mask substrate alloy target blank and a back plate, the phase-shift mask substrate alloy target blank and the back plate are welded and connected, the phase-shift mask substrate alloy target blank includes molybdenum, silicon and carbon, the mass ratio of carbon is 0.1%~1%, and the mass ratio of molybdenum to silicon is 1:4~1:9.

[0007] The above-mentioned phase-shift mask substrate alloy target provides a molybdenum-silicon alloy target containing carbon elements, which can introduce a carbon source into the molybdenum-silicon alloy target. The phase-shift mask substrate alloy target can be used for sputtering to directly form a MoSi metal film containing carbon elements, so that in the process of sputtering deposition to form a phase-shift film, there is no need to introduce carbon-containing gases such as CH4, CO and CO2 to introduce a carbon source into the phase-shift film, thereby avoiding increasing the gas partial pressure of the negative ion gas in the sputtering chamber, effectively improving the film formation rate and film flatness, and greatly improving the film formation quality of the carbon-containing phase-shift film. Moreover, the mass ratio of molybdenum to silicon is 1:4~1:9, which can reduce the difference in sputtering yield between molybdenum and silicon during magnetron sputtering. At the same time, adding 0.1%~1% carbon can ensure that the Mo / Si ratio is 1:4~1:9, and the solid solubility of molybdenum in silicon is increased to refine the grains and make the grain size more uniform, thereby improving the uniformity of sputtering film formation and forming a carbon-containing phase shift film with uniform film thickness, which is conducive to further improving the flatness of the film formation and further improving the film formation quality. At the same time, the increase in the solid solubility of molybdenum in silicon can eliminate the unevenness and non-solid solution phenomenon in the microscopic area, forming a more stable compound, which can effectively improve the stability of the product.

[0008] In addition, the above-mentioned phase-shift mask substrate alloy target does not need to introduce high-pressure gases such as CH4, CO and CO2 during the sputtering process, which is beneficial to saving the production cost of the sputtering process. Moreover, the introduction of flammable or toxic gases is avoided during the sputtering process, which is beneficial to improving production safety.

[0009] Therefore, the above-mentioned phase-shift mask substrate alloy target has the beneficial effects of high product stability, good film-forming quality, saving the production cost of the carbon-containing phase-shift film, and improving the production safety of the carbon-containing phase-shift film.

[0010] In one embodiment, the average grain size of the phase-shift mask substrate alloy target blank is 30μ~50μm.

[0011] On the other hand, the present invention also provides a method for manufacturing the above-mentioned phase-shift mask substrate alloy target, comprising the following steps: The high purity Mo powder and Si powder are mixed evenly to obtain Mo and Si mixed powder; Adding carbon-containing substances to the Mo and Si mixed powders and mixing them evenly to obtain carbon-containing Mo and Si mixed powders; The carbon-containing Mo and Si mixed powder is made into a preform by isostatic pressing; The preformed body is made into a phase shift mask substrate alloy target blank by adopting a high temperature sintering process; The phase-shift mask substrate alloy target blank is welded to a back plate to form a phase-shift mask substrate alloy target material.

[0012] The manufacturing method of the phase-shift mask substrate alloy target material is used to manufacture the above-mentioned phase-shift mask substrate alloy target material. In the method, a carbon source is introduced into the manufacturing process of the phase-shift mask substrate alloy target material to form a preform containing Mo, Si and carbon, and then the preform is made into a phase-shift mask substrate alloy target blank through a high-temperature sintering process. The addition of carbon can form SiC and MoSi2 in the process of high-temperature sintering of the preform to form the phase-shift mask substrate alloy target blank. SiC and MoSi2 have good interface compatibility and thermodynamic stability, can improve the grain boundary structure, and increase the solid solubility of molybdenum in silicon to refine the grains. Experiments have proved that by introducing carbon elements into the molybdenum-silicon target material through the above-mentioned manufacturing method of the phase-shift mask substrate alloy target material, the average grain size can be reduced from 150μ~300μm to 30μ~50μm, making the grain size more uniform, and can improve the uniformity of sputtering film formation, forming a carbon-containing phase-shift film with uniform film thickness, which is conducive to further improving the film flatness and improving the sputtering film quality. In addition, the increase in the solubility of molybdenum in silicon can eliminate the unevenness and insolubility in microscopic areas, forming more stable compounds, which can effectively improve the product stability of the manufactured phase-shift mask substrate alloy target.

[0013] In addition, the above-mentioned method for manufacturing the phase-shift mask substrate alloy target introduces a carbon source during the manufacturing process of the phase-shift mask substrate alloy target to produce a molybdenum-silicon alloy target containing carbon elements, thereby introducing a carbon source into the molybdenum-silicon alloy target. As a result, during the process of sputtering deposition to form a phase-shift film, there is no need to introduce a carbon-containing gas to introduce a carbon source into the phase-shift film. This can effectively solve the technical problems of poor film quality, high production cost and potential safety hazards in the prior art method of introducing a carbon source into the phase-shift film.

[0014] In summary, the above-mentioned method for manufacturing the phase-shift mask substrate alloy target can improve the product stability of the phase-shift mask substrate alloy target, and can effectively solve the technical problems of poor film quality, high production cost and potential safety hazards in the prior art method of introducing carbon source into the phase-shift film.

[0015] In one embodiment, the step of uniformly mixing high-purity Mo powder and Si powder comprises: using a high-speed powder ball milling device to ball mill the Mo powder and Si powder at a ball milling speed of 2000r / min~5000r / min for 2~3h.

[0016] In one embodiment, the step of adding carbon-containing material to the Mo and Si mixed powders and mixing them uniformly includes: Adding carbon-containing substances to the mixed powder of Mo and Si; The Mo, Si mixed powder and carbon-containing material are ball-milled for 1 h to 2 h using a high-speed powder ball mill at a ball milling speed of not less than 3000 r / min.

[0017] In one embodiment, the carbon-containing material is carbon powder, diamond powder or pure carbon powder in any form.

[0018] In one embodiment, the isostatic pressing pressure of the isostatic pressing process is 20 MPa-30 MPa, and / or the isostatic pressing time is not less than 10 min.

[0019] In one embodiment, the sintering temperature of the high temperature sintering process is 1600°C ± 30°C.

[0020] In one embodiment, the high temperature sintering process performs high temperature sintering on the preform under the protection of an inert gas or nitrogen.

[0021] In one embodiment, the gas flow rate of the inert gas or nitrogen gas is 20 sccm-40 sccm. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic structural diagram of a phase-shift mask substrate alloy target material according to an embodiment; Figure 2 The figure is a schematic diagram of a process for manufacturing a phase-shift mask substrate alloy target according to an embodiment.

[0023] Description of reference numerals: 10-phase shift mask substrate alloy target blank, 20-back plate. DETAILED DESCRIPTION

[0024] In the following description, a large number of specific details are given in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features known in the art are not described. It should be understood that the present invention can be implemented in different forms and should not be interpreted as being limited to the embodiments presented here. On the contrary, providing these embodiments will make the disclosure thorough and complete, and fully convey the scope of the present invention to those skilled in the art. The same reference numerals represent the same elements from beginning to end. It should be understood that when a layer is referred to as being formed on other layers, it can be directly formed on other layers, or there can be an intervening film layer. Among them, the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back" and the like is based on the orientation or positional relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, wherein "longitudinal" can be understood as a direction perpendicular to the substrate surface, and "lateral" can be understood as a direction parallel to the substrate surface. When used herein, the singular forms "a", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "include" is used to determine the presence of features, steps, operations, elements and / or parts, but does not exclude the presence or addition of one or more other features, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items. The terms "same", "equal" and "consistent" include completely equal and identical meanings, and may also include approximately the same or approximately equal meanings under allowed process errors. The terms "first" "second" and the like in the specification are used to distinguish between similar elements, and are not necessarily used to describe a specific order or time sequence. It is to be understood that, where appropriate, these terms used in this way are interchangeable, for example, so that the embodiments of the present invention described herein can be operated in other orders different from those described or shown herein. Similarly, if the method described herein includes a series of steps, the order in which the steps are presented herein is not necessarily the only order in which the steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method. If components in a certain figure are the same as components in other figures, although these components can be easily identified in all figures, in order to make the description of the figures clearer, this specification will not mark all the same component numbers in each figure.

[0025] The present invention is described more clearly and completely below by way of embodiments in conjunction with the accompanying drawings, but the present invention is not limited to the scope of the following embodiments.

[0026] See also Figure 1 The phase shift mask substrate alloy target material of one embodiment includes a phase shift mask substrate alloy target blank 10 and a back plate 20, the phase shift mask substrate alloy target blank 10 and the back plate 20 are welded and connected, and the phase shift mask substrate alloy target blank 10 includes molybdenum, silicon and carbon, wherein the mass ratio of carbon is 0.1% to 1%, and the mass ratio of molybdenum to silicon is 1:4 to 1:9. Further, in one embodiment, the average grain size of the phase shift mask substrate alloy target blank is 30μ to 50μm.

[0027] The above-mentioned phase-shift mask substrate alloy target provides a molybdenum-silicon alloy target containing carbon elements, which can introduce a carbon source into the molybdenum-silicon alloy target. The phase-shift mask substrate alloy target can be used for sputtering to directly form a MoSi metal film containing carbon elements, so that in the process of sputtering deposition to form a phase-shift film, there is no need to introduce carbon-containing gases such as CH4, CO and CO2 to introduce a carbon source into the phase-shift film, thereby avoiding increasing the gas partial pressure of the negative ion gas in the sputtering chamber, effectively improving the film formation rate and film flatness, and greatly improving the film formation quality of the carbon-containing phase-shift film. Moreover, the mass ratio of molybdenum to silicon is 1:4~1:9, which can reduce the difference in sputtering yield between molybdenum and silicon during magnetron sputtering. At the same time, adding 0.1%~1% carbon can ensure that the Mo / Si ratio is 1:4~1:9, and the solid solubility of molybdenum in silicon is increased to refine the grains. The average grain size of the phase-shift mask substrate alloy target blank can be reduced to 30μ~50μm, and the grain size is more uniform, which can improve the uniformity of sputtering film formation and form a carbon-containing phase-shift film with uniform film thickness, which is conducive to further improving the flatness of the film and further improving the film quality. At the same time, the increase in the solid solubility of molybdenum in silicon can eliminate the unevenness and non-solid solution phenomenon in the microscopic area, form a more stable compound, and effectively improve the stability of the product.

[0028] In addition, the above-mentioned phase-shift mask substrate alloy target does not need to introduce high-pressure gases such as CH4, CO and CO2 during the sputtering process, which is beneficial to saving the production cost of the sputtering process. Moreover, the introduction of flammable or toxic gases is avoided during the sputtering process, which is beneficial to improving production safety.

[0029] The above-mentioned phase-shift mask substrate alloy target has the beneficial effects of high product stability, good film-forming quality, saving the production cost of the carbon-containing phase-shift film, and improving the production safety of the carbon-containing phase-shift film.

[0030] See also Figure 2 The present invention also provides a method for manufacturing the above-mentioned phase-shift mask substrate alloy target, comprising the following steps: Step S11: Evenly mix high-purity Mo powder and Si powder to obtain Mo and Si mixed powder.

[0031] Specifically, in order to reduce the difference in sputtering yield between molybdenum and silicon during magnetron sputtering, the Mo powder and Si powder are mixed in a mass ratio of 1:4 to 1:9, and the purity of high-purity Mo powder and Si powder is not less than 99.9% to ensure the purity of the phase-shift mask substrate alloy target. Furthermore. In order to ensure that the Mo powder and Si powder are fully mixed and uniform, a high-speed powder ball milling device is used for mixing. In order to avoid the introduction of impurities during the mixing process, silicon balls are preferably used as ball milling medium balls. In one embodiment, in order to ensure that the Mo powder and Si powder are mixed uniformly, a high-speed powder ball milling device is used to ball mill the Mo powder and Si powder at a ball milling speed of 2000r / min to 5000r / min for 2 to 3 hours.

[0032] Step S12: adding carbon-containing substances to the Mo and Si mixed powders and mixing them evenly to obtain carbon-containing Mo and Si mixed powders.

[0033] Specifically, the carbon-containing substance is carbon powder, diamond powder or pure carbon powder in any form, and the purity of the pure carbon powder is not less than 99.9%. Furthermore, in order to ensure the film-forming quality of the phase-shift mask substrate alloy target, pure carbon powder is added to the Mo and Si mixed powders at a mass ratio of 0.1% to 1% for mixing. Similarly, in order to ensure that the carbon-containing Mo and Si mixed powders are fully mixed and uniform, the pure carbon powder is also homogenized using a high-speed ball mill after being added.

[0034] In one embodiment, step S12 specifically includes the following steps: first, adding carbon-containing substances to the Mo and Si mixed powders, specifically, completing the mixing of Mo powder and Si powder to obtain the Mo and Si mixed powders, and then putting an appropriate amount of pure carbon powder into a high-speed ball mill according to a preset mass ratio. After that, the Mo and Si mixed powders and the carbon-containing substances are ball milled for 1h to 2h at a ball milling speed of not less than 3000r / min using a high-speed powder ball mill to fully mix the pure carbon powder with the Mo powder and Si powder to obtain a carbon-containing Mo and Si mixed powder.

[0035] In this embodiment, the ball milling speed in step S12 is preferably greater than the ball milling speed in step S11. The Mo powder and Si powder are first mixed at a lower ball milling speed in step S11, and then step S12 is performed to add pure carbon powder and increase the ball milling speed for ball milling mixing. On the basis of evenly mixing the pure carbon powder and the Mo and Si mixed powder to obtain the carbon-containing Mo and Si mixed powder, the particle size can be further reduced, which is beneficial to reducing the grain size of the obtained phase shift mask substrate alloy target blank.

[0036] Step S13: using an isostatic pressing process to make a preform from the carbon-containing Mo and Si mixed powder.

[0037] Specifically, the carbon-containing Mo and Si mixed powder is firstly made into the desired target blank shape through a mold, and then is pressed by an isostatic pressing device to form a prefabricated body with a preset shape and size. Figure 1 As shown, in the present embodiment, the phase-shift mask substrate alloy target blank 10 is a circular target blank, so a circular mold is used to make a circular preform. In other embodiments, the phase-shift mask substrate alloy target blank 10 can also be square or anisotropic in shape. During the preform production process, the corresponding grinding tool is selected according to the shape and size of the phase-shift mask substrate alloy target blank 10 as required to make the target blank shape. This embodiment does not make any specific limitation.

[0038] In one embodiment, to ensure that the powder inside the preform is fully bonded, the isostatic pressing pressure of the isostatic pressing process is 20 MPa to 30 MPa. Furthermore, the isostatic pressing time is not less than 10 min, preferably the isostatic pressing time is 10 min to 15 min, to ensure that the powder inside the preform is fully bonded and to improve processing efficiency.

[0039] Step S14: using a high temperature sintering process to make the preform into a phase shift mask substrate alloy target blank.

[0040] Specifically, after the preform is made, the preform is subjected to high-temperature sintering at a sintering temperature of 1600°C±30°C to form the phase-shift mask substrate alloy target blank 10. In this embodiment, the preform is subjected to high-temperature sintering at a sintering temperature of 1600°C±30°C. On the basis of sufficient sintering, it can be ensured that the generated substance is mainly MoSi2, and the grain size can be reduced to 30μ~50μm, making the grain size distribution more uniform.

[0041] Further, in one embodiment, the high temperature sintering process performs high temperature sintering on the prefabricated body under the protection of an inert gas or nitrogen. Specifically, the inert gas may be, but is not limited to, helium or argon. In order to effectively save costs, the protective gas is preferably nitrogen or argon. In this embodiment, an inert gas or nitrogen is used to form a protective atmosphere during the high temperature sintering process to avoid volatilization and oxidation of the sintered material during the high temperature sintering process, thereby ensuring the purity and performance of the sintered phase shift mask substrate alloy target blank 10. Further, in one embodiment, in order to ensure the protective effect, improve the sintering efficiency and product quality, the gas flow rate of the inert gas or nitrogen is preferably 20sccm~40sccm.

[0042] Step S15: welding the phase-shift mask substrate alloy target blank and the back plate to form the phase-shift mask substrate alloy target material. Specifically, after the phase-shift mask substrate alloy target blank 10 is manufactured, the sintered phase-shift mask substrate alloy target blank 10 is first machined and then cleaned, and then the phase-shift mask substrate alloy target blank 10 is welded to the back plate to form the phase-shift mask substrate alloy target material, thereby completing the phase-shift mask substrate alloy target material manufacturing.

[0043] The manufacturing method of the phase-shift mask substrate alloy target material of the present embodiment is used to manufacture the above-mentioned phase-shift mask substrate alloy target material. In the method, a carbon source is introduced into the manufacturing process of the phase-shift mask substrate alloy target material to prepare a preform containing Mo, Si and carbon, and then the preform is made into a phase-shift mask substrate alloy target blank through a high-temperature sintering process. The addition of carbon can form SiC and MoSi2 in the process of high-temperature sintering of the preform to prepare the phase-shift mask substrate alloy target blank. SiC and MoSi2 have good interface compatibility and thermodynamic stability. Stability can improve the grain boundary structure, increase the solid solubility of molybdenum in silicon to refine the grains. Experiments have shown that the introduction of carbon elements into the molybdenum silicon target material through the above-mentioned phase-shift mask substrate alloy target manufacturing method can reduce the average grain size from 150μm~300μm (the average grain size of the traditional molybdenum silicon target material without carbon elements) to 30μm~50μm, making the grain size more uniform, which can improve the uniformity of sputtering film formation, form a carbon-containing phase shift film with uniform film thickness, and help improve the film flatness and sputtering film quality. In addition, the increase in the solid solubility of molybdenum in silicon can eliminate the unevenness and non-solid solution phenomenon in the microscopic area, forming a more stable compound, which can effectively improve the product stability of the manufactured phase-shift mask substrate alloy target material.

[0044] In addition, the above-mentioned method for manufacturing the phase-shift mask substrate alloy target introduces a carbon source during the manufacturing process of the phase-shift mask substrate alloy target to produce a molybdenum-silicon alloy target containing carbon elements, thereby introducing a carbon source into the molybdenum-silicon alloy target. As a result, during the process of sputtering deposition to form a phase-shift film, there is no need to introduce a carbon-containing gas to introduce a carbon source into the phase-shift film. This can effectively solve the technical problems of poor film quality, high production cost and potential safety hazards in the prior art method of introducing a carbon source into the phase-shift film.

[0045] The manufacturing method of the phase-shift mask substrate alloy target material can improve the product stability of the phase-shift mask substrate alloy target material, and can effectively solve the technical problems of poor film quality, high production cost and potential safety hazards in the prior art method of introducing carbon source into the phase-shift film.

[0046] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of the technical solution of the present invention.

Claims

1. A phase-shift mask substrate alloy target material, comprising a phase-shift mask substrate alloy target blank and a back plate, wherein the phase-shift mask substrate alloy target blank and the back plate are welded and connected, characterized in that: The phase-shift mask substrate alloy target blank comprises molybdenum, silicon and carbon, the mass ratio of the carbon element is 0.1% to 1%, and the mass ratio of the molybdenum element to the silicon element is 1:4 to 1:

9.

2. The phase shift mask substrate alloy target according to claim 1, characterized in that: The average grain size of the phase-shift mask substrate alloy target blank is 30μ-50μm.

3. A method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The following steps are involved: The high purity Mo powder and Si powder are mixed evenly to obtain Mo and Si mixed powder; Adding carbon-containing substances to the Mo and Si mixed powder and mixing them evenly to obtain carbon-containing Mo and Si mixed powder; The carbon-containing Mo and Si mixed powder is made into a preform by isostatic pressing; The preformed body is made into a phase shift mask substrate alloy target blank by adopting a high temperature sintering process; The phase-shift mask substrate alloy target blank is welded to a back plate to form a phase-shift mask substrate alloy target material.

4. The method for manufacturing a phase shift mask substrate alloy target according to claim 3, characterized in that: The step of uniformly mixing the high-purity Mo powder and the Si powder comprises: using a high-speed powder ball milling device to ball mill the Mo powder and the Si powder at a ball milling speed of 2000r / min~5000r / min for 2~3h.

5. The method for manufacturing a phase shift mask substrate alloy target according to claim 3, characterized in that: The step of adding carbon-containing substances to the Mo and Si mixed powders and mixing them uniformly comprises: Adding carbon-containing substances to the Mo and Si mixed powders; The Mo and Si mixed powders and the carbon-containing material are ball-milled for 1 h to 2 h at a ball-milling speed of not less than 3000 r / min using a high-speed powder ball-milling device.

6. The method for manufacturing a phase shift mask substrate alloy target according to claim 5, characterized in that: The carbon-containing substance is carbon powder, diamond powder or pure carbon powder in any form.

7. The method for manufacturing a phase shift mask substrate alloy target according to claim 3, characterized in that: The isostatic pressing pressure of the isostatic pressing process is 20 MPa to 30 MPa, and / or the isostatic pressing time is not less than 10 min.

8. The method for manufacturing a phase shift mask substrate alloy target according to claim 3, characterized in that: The sintering temperature of the high temperature sintering process is 1600°C±30°C.

9. The method for manufacturing a phase shift mask substrate alloy target according to claim 3, characterized in that: The high temperature sintering process performs high temperature sintering on the prefabricated body under the protection of an inert gas or nitrogen.

10. The method for manufacturing a phase shift mask substrate alloy target according to claim 9, characterized in that: The gas flow rate of the inert gas or the nitrogen gas is 20 sccm to 40 sccm.

Citation Information

Cited By

  • Molybdenum-silicon target material and preparation method thereof

    CN121896586A

  • Phase-shift mask substrate alloy target and manufacturing method therefor

    WO2026040417A1