Manufacturing method of phase shift mask substrate alloy target material

By introducing carbon elements in high-temperature sintering during the manufacturing process of phase shift mask base alloy target, the problem of poor film formation quality in the prior art is solved, the film formation rate and flatness are improved, and the product stability is enhanced sex.

CN119061362APending Publication Date: 2024-12-03SHANGHAI CHUANXIN SEMICON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411173215.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The method of introducing a carbon source to a phase shift film in the prior art leads to poor film formation quality, reduced film formation rate and flatness, and affects the performance of the phase shift film.

Method used

By introducing carbon-containing gas in the high-temperature sintering process, a phase shift mask substrate alloy target containing carbon elements is formed, so as to avoid introducing carbon-containing gas during sputtering, and the film formation rate and flatness are improved.

Benefits of technology

It effectively improves the film formation quality of the carbon-containing phase shift film, improves grain boundary structure and grain uniformity, enhances product stability, and forms a more uniform film thickness and a higher film formation flatness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061362A_ABST
    Figure CN119061362A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a phase shift mask substrate alloy target material, which comprises the following steps: uniformly mixing high-purity Mo powder and Si powder to obtain Mo and Si mixed powder; preparing the Mo and Si mixed powder into a prefabricated target blank by adopting an isostatic pressing process; and performing high-temperature sintering on the prefabricated target blank by adopting a high-temperature sintering process, and introducing carbon-containing gas in the high-temperature sintering process to prepare the phase shift mask base plate alloy target material containing the carbon element. According to the manufacturing method of the phase shift mask base plate alloy target material, the film forming quality of the carbon-containing phase shift film can be improved, the technical problem of poor film forming quality of a method for introducing a carbon source into the phase shift film in the prior art is effectively solved, and the product stability of the phase shift mask base plate alloy target material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of integrated circuit manufacturing, and in particular to a method for manufacturing a phase-shift mask substrate alloy target material. Background Art

[0002] Semiconductor components are manufactured through a series of processes from wafer, oxidation, exposure to packaging. Among these eight processes, the most important is the exposure process. The exposure process uses a photomask (also known as a photomask, mask, or mask plate) as the original plate and uses exposure equipment to reduce the line width of the projected circuit on the wafer.

[0003] A photomask is a product that uses electron beam exposure technology to etch a fine circuit pattern on a mask substrate. The mask substrate is formed by forming a multi-layer chromium film on a quartz substrate and coating the multi-layer chromium film with photoresist. With the high integration of semiconductor integrated circuits, the photomask route for forming patterns also tends to be high-precision and refined. In order to form finer patterns in semiconductor integrated circuits, high pattern resolution is required. Phase-shift inversion film masks use both the intensity and phase of light to form images, have higher resolution, and are widely used in semiconductor photolithography processes with higher requirements.

[0004] The phase shift mask is a metal film containing MoxSiy compounds deposited on the surface of a glass substrate, so that the light produces a 180-degree phase difference when passing through the film area, thereby enhancing the contrast of the image and improving the resolution. In order to further optimize the performance of the phase shift film, carbon elements can be introduced into the phase shift film (MoSi metal film). After adding carbon elements, the corrosion resistance, mechanical strength and stability of the phase shift film can be enhanced, and the light transmittance and conductivity of the phase shift film can also be improved. The method commonly used in the prior art to introduce a carbon source into the phase shift film is to introduce gases such as CH4, CO and CO2 as carbon sources during the vacuum sputtering process, and to form multi-element metal films or dielectric films such as MoSiONC, MoSiC or MoSiOC by introducing carbon-containing gases. However, the existing method of introducing a carbon source into the phase shift film uses gas as a carbon source. The addition of gas increases the gas partial pressure of the negative ion gas in the sputtering chamber, resulting in a decrease in the film forming rate and the film flatness, which affects the film forming quality of the phase shift film. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a phase-shift mask substrate alloy target material, so as to solve the technical problem of poor film quality in the existing method of introducing a carbon source into a phase-shift film.

[0006] To achieve the above object, the present invention provides a method for manufacturing a phase-shift mask substrate alloy target, comprising the following steps: The high purity Mo powder and Si powder are mixed evenly to obtain Mo and Si mixed powder; The Mo and Si mixed powders are made into a prefabricated target blank by isostatic pressing; The prefabricated target blank is sintered at high temperature by adopting a high temperature sintering process, and a carbon-containing gas is introduced during the high temperature sintering process to produce a phase shift mask substrate alloy target material containing carbon elements.

[0007] The above-mentioned method for manufacturing a phase-shift mask substrate alloy target is used to manufacture a phase-shift mask substrate alloy target containing carbon elements. In the process of high-temperature sintering a prefabricated target blank, a carbon-containing gas is introduced. During the high-temperature sintering process, the carbon element enters the interior of the prefabricated target blank in a gaseous phase and combines with molybdenum and silicon elements to form a phase-shift mask substrate alloy target containing carbon elements. This method introduces carbon elements in advance during the process of manufacturing the phase-shift mask substrate alloy target to form a phase-shift mask substrate alloy target containing carbon elements, so that during the process of sputtering deposition to form a phase-shift film, it is possible to introduce a carbon source into the phase-shift film without introducing a carbon-containing gas, thereby avoiding increasing the gas partial pressure of the negative ion gas in the sputtering chamber, and can effectively improve the film forming rate and film flatness, and greatly improve the film forming quality of the carbon-containing phase-shift film.

[0008] In addition, the addition of carbon can form SiC and MoSi2 in the process of high-temperature sintering of the prefabricated target blank to form a phase-shift mask substrate alloy target. SiC and MoSi2 have good interface compatibility and thermodynamic stability, which can improve the grain boundary structure and increase the solid solubility of molybdenum in silicon to refine the grains. Experiments have shown that the introduction of carbon elements into the molybdenum silicon target through the above-mentioned manufacturing method of the phase-shift mask substrate alloy target can reduce the average grain size from 150μ~300μm to 30μ~50μm, making the grain size more uniform, improving the uniformity of sputtering film formation, forming a carbon-containing phase shift film with uniform film thickness, which is conducive to further improving the film flatness and further improving the sputtering film quality. In addition, the increase in the solid solubility of molybdenum in silicon can eliminate the unevenness and non-solid solution phenomenon in the microscopic area, forming a more stable compound, which can effectively improve the product stability of the manufactured phase-shift mask substrate alloy target.

[0009] In summary, the above-mentioned method for manufacturing the phase-shift mask substrate alloy target can improve the film forming quality of the carbon-containing phase-shift film, effectively solve the technical problem of poor film forming quality in the method of introducing a carbon source into the phase-shift film in the prior art, and can improve the product stability of the phase-shift mask substrate alloy target.

[0010] In one embodiment, the carbon-containing gas includes at least one of CO, CO2 and CH4.

[0011] In one embodiment, the gas flow rate of the carbon-containing gas is 0.1 sccm-1 sccm.

[0012] In one embodiment, the step of uniformly mixing high-purity Mo powder and Si powder comprises: using a high-speed powder ball milling device to ball mill the Mo powder and Si powder at a ball milling speed of 2000r / min~5000r / min for 2~3h.

[0013] In one embodiment, the isostatic pressing pressure of the isostatic pressing process is 20 MPa-30 MPa, and / or the isostatic pressing time is not less than 10 min.

[0014] In one embodiment, the sintering temperature of the high temperature sintering process is 1400° C. to 1600° C., and the process pressure is 0.5 Pa to 5 Pa.

[0015] In one embodiment, the high temperature sintering process performs high temperature sintering on the prefabricated target blank under the protection of an inert gas or nitrogen.

[0016] In one embodiment, the gas flow rate of the inert gas or nitrogen gas is 20 sccm-40 sccm.

[0017] In one embodiment, the phase-shift mask substrate alloy target material contains carbon in a mass ratio of 0.1% to 1%, and molybdenum and silicon in a mass ratio of 1:4 to 1:9.

[0018] In one embodiment, the average grain size of the phase-shift mask substrate alloy target is 30μ~50μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The figure is a schematic diagram of a process for manufacturing a phase-shift mask substrate alloy target according to an embodiment. DETAILED DESCRIPTION

[0020] In the following description, a large number of specific details are given in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features known in the art are not described. It should be understood that the present invention can be implemented in different forms and should not be interpreted as being limited to the embodiments presented here. On the contrary, providing these embodiments will make the disclosure thorough and complete, and fully convey the scope of the present invention to those skilled in the art. The same reference numerals represent the same elements from beginning to end. It should be understood that when a layer is referred to as being formed on other layers, it can be directly formed on other layers, or there can be an intervening film layer. Among them, the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back" and the like is based on the orientation or positional relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, wherein "longitudinal" can be understood as a direction perpendicular to the substrate surface, and "lateral" can be understood as a direction parallel to the substrate surface. When used herein, the singular forms "a", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "include" is used to determine the presence of features, steps, operations, elements and / or parts, but does not exclude the presence or addition of one or more other features, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items. The terms "same", "equal" and "consistent" include completely equal and identical meanings, and may also include approximately the same or approximately equal meanings under allowed process errors. The terms "first" "second" and the like in the specification are used to distinguish between similar elements, and are not necessarily used to describe a specific order or time sequence. It is to be understood that, where appropriate, these terms used in this way are interchangeable, for example, so that the embodiments of the present invention described herein can be operated in other orders different from those described or shown herein. Similarly, if the method described herein includes a series of steps, the order in which the steps are presented herein is not necessarily the only order in which the steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method. If components in a certain figure are the same as components in other figures, although these components can be easily identified in all figures, in order to make the description of the figures clearer, this specification will not mark all the same component numbers in each figure.

[0021] The present invention is described more clearly and completely below by way of embodiments in conjunction with the accompanying drawings, but the present invention is not limited to the scope of the following embodiments.

[0022] See also Figure 1 A method for manufacturing a phase-shift mask substrate alloy target according to an embodiment of the present invention comprises the following steps: Step S11: Evenly mix high-purity Mo powder and Si powder to obtain Mo and Si mixed powder.

[0023] Specifically, the purity of high-purity Mo powder and Si powder is not less than 99.9% to ensure the purity of the phase-shift mask substrate alloy target. Furthermore, to ensure that the Mo powder and Si powder are fully mixed, a high-speed powder ball mill is used to mix the materials. To avoid the introduction of impurities during the mixing process, silicon balls are preferably used as ball milling media. In one embodiment, to ensure that the Mo powder and Si powder are mixed evenly, a high-speed powder ball mill is used to mill the Mo powder and Si powder at a ball milling speed of 2000r / min~5000r / min for 2~3h.

[0024] Furthermore, in one embodiment, in order to reduce the difference in sputtering yields between molybdenum and silicon during magnetron sputtering, Mo powder and Mo powder are mixed in a mass ratio of 1:4 to 1:9.

[0025] Step S12: using an isostatic pressing process to prepare a prefabricated target blank from the Mo and Si mixed powders.

[0026] Specifically, the Mo and Si mixed powder is first made into the desired target blank shape through a mold, and then isostatic pressing equipment is used to press it to make a prefabricated target blank with a preset shape and size. In one embodiment, the phase-shift mask substrate alloy target material is a circular target blank, so a circular prefabricated target blank is made using a circular mold. In other embodiments, the phase-shift mask substrate alloy target material can also be square or anisotropic in shape. During the production of the prefabricated target blank, the corresponding grinding tool is selected according to the shape and size of the phase-shift mask substrate alloy target material to make the desired target blank shape, and this embodiment does not make specific limitations.

[0027] In one embodiment, to ensure that the powder inside the preform is fully bonded, the isostatic pressing pressure of the isostatic pressing process is 20 MPa to 30 MPa. Furthermore, the isostatic pressing time is not less than 10 min, preferably the isostatic pressing time is 10 min to 15 min, to ensure that the powder inside the preform is fully bonded and to improve processing efficiency.

[0028] Step S13: adopting a high temperature sintering process to perform high temperature sintering on the prefabricated target blank, and introducing a carbon-containing gas during the high temperature sintering process to produce a phase shift mask substrate alloy target material containing carbon elements.

[0029] Specifically, the carbon-containing gas includes at least one of CO, CO2 and CH4. In this embodiment, the carbon-containing gas is introduced during the high-temperature sintering of the prefabricated target blank. During the high-temperature sintering process, the carbon element enters the interior of the prefabricated target blank in a gas phase and combines with the molybdenum element and the silicon element to form SiC and MoSi2, thereby forming a phase-shift mask substrate alloy target material containing the carbon element. Furthermore, after the phase-shift mask substrate alloy target blank is manufactured, the fired phase-shift mask substrate alloy target blank is machined and then cleaned, and then the phase-shift mask substrate alloy target blank is welded to the back plate to form a phase-shift mask substrate alloy target assembly, which can be used for subsequent sputtering processes.

[0030] In one embodiment, in order to ensure the film forming quality of the phase-shift mask substrate alloy target material, the mass ratio of the carbon element introduced into the phase-shift mask substrate alloy target material during the high-temperature sintering process is controlled to be 0.1%~1%. Specifically, the carbon content infiltrated into the phase-shift mask substrate alloy target blank can be controlled by adjusting the partial pressure ratio of the carbon-containing gas to control the mass ratio of the carbon element introduced into the phase-shift mask substrate alloy target material, and the partial pressure ratio of the carbon-containing gas can be further adjusted by adjusting the gas flow rate of the carbon-containing gas. Preferably, in order to ensure that the mass ratio of the introduced carbon element is 0.1%~1%, in one embodiment, the gas flow rate of the carbon-containing gas is 0.1sccm~1sccm.

[0031] In one embodiment, the sintering temperature of the high temperature sintering process is 1400°C~1600°C, and the process pressure is 0.5Pa~5Pa. After the prefabricated target blank is made, the prefabricated body is subjected to high temperature sintering at a sintering temperature of 1400°C~1600°C and a process pressure of 0.5Pa~5Pa to form a phase shift mask substrate alloy target. This embodiment uses a sintering temperature of 1400°C~1600°C and a process pressure of 0.5Pa~5Pa to sinter the prefabricated body at high temperature. On the basis of sufficient sintering, it can ensure that the generated substance is mainly MoSi2, and the grain size can be reduced to 30μ~50μm, making the grain size distribution more uniform.

[0032] In one embodiment, the high-temperature sintering process performs high-temperature sintering on the prefabricated target blank under the protection of an inert gas or nitrogen. Specifically, the inert gas can be but is not limited to helium or argon. In order to effectively save costs, the protective gas preferably uses nitrogen or argon. In this embodiment, an inert gas or nitrogen is used to form a protective atmosphere during the high-temperature sintering process to avoid volatilization and oxidation of the sintered material during the high-temperature sintering process, thereby ensuring the purity and performance of the sintered phase-shift mask substrate alloy target blank 10. Furthermore, in one embodiment, in order to ensure the protection effect, improve the sintering efficiency and product quality, and ensure the partial pressure of the carbon-containing gas, the gas flow rate of the inert gas or nitrogen is preferably 20sccm~40sccm.

[0033] The phase-shift mask substrate alloy target material manufactured by the manufacturing method of the above-mentioned phase-shift mask substrate alloy target material contains a carbon element mass ratio of 0.1%~1%, and a molybdenum element and a silicon element mass ratio of 1:4~1:9. The mass ratio of molybdenum element and silicon element is 1:4~1:9, which can reduce the difference in sputtering yield between molybdenum and silicon during magnetron sputtering, and at the same time add 0.1%~1% carbon, which can ensure that the Mo / Si ratio is 1:4~1:9. Increase the solid solubility of molybdenum in silicon to refine the grains. In one embodiment, the average grain size of the phase-shift mask substrate alloy target material is 30μ~50μm, and the average grain size is reduced to 30μ~50μm, and the grain size is more uniform, which can improve the uniformity of sputtering film formation and further improve the film formation quality.

[0034] The above-mentioned method for manufacturing a phase-shift mask substrate alloy target is used to manufacture a phase-shift mask substrate alloy target containing carbon elements. In the process of high-temperature sintering a prefabricated target blank, a carbon-containing gas is introduced. During the high-temperature sintering process, the carbon element enters the interior of the prefabricated target blank in a gaseous phase and combines with molybdenum and silicon elements to form a phase-shift mask substrate alloy target containing carbon elements. This method introduces carbon elements in advance during the process of manufacturing the phase-shift mask substrate alloy target to form a phase-shift mask substrate alloy target containing carbon elements, so that during the process of sputtering deposition to form a phase-shift film, it is possible to introduce a carbon source into the phase-shift film without introducing a carbon-containing gas, thereby avoiding increasing the gas partial pressure of the negative ion gas in the sputtering chamber, and can effectively improve the film forming rate and film flatness, and greatly improve the film forming quality of the carbon-containing phase-shift film.

[0035] In addition, the addition of carbon can form SiC and MoSi2 in the process of high-temperature sintering of the prefabricated target blank to form a phase-shift mask substrate alloy target. SiC and MoSi2 have good interface compatibility and thermodynamic stability, which can improve the grain boundary structure and increase the solid solubility of molybdenum in silicon to refine the grains. Experiments have shown that the introduction of carbon elements into the molybdenum silicon target through the above-mentioned manufacturing method of the phase-shift mask substrate alloy target can reduce the average grain size from 150μ~300μm to 30μ~50μm, making the grain size more uniform, improving the uniformity of sputtering film formation, forming a carbon-containing phase shift film with uniform film thickness, which is conducive to further improving the film flatness and further improving the sputtering film quality. In addition, the increase in the solid solubility of molybdenum in silicon can eliminate the unevenness and non-solid solution phenomenon in the microscopic area, forming a more stable compound, which can effectively improve the product stability of the manufactured phase-shift mask substrate alloy target.

[0036] The manufacturing method of the phase-shift mask substrate alloy target can improve the film quality of the carbon-containing phase-shift film, effectively solve the technical problem of poor film quality in the method of introducing a carbon source into the phase-shift film in the prior art, and can improve the product stability of the phase-shift mask substrate alloy target.

[0037] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of the technical solution of the present invention.

Claims

1. A method for manufacturing a phase shift mask substrate alloy target, characterized in that: The following steps are involved: The high purity Mo powder and Si powder are mixed evenly to obtain Mo and Si mixed powder; The Mo and Si mixed powder is made into a prefabricated target blank by adopting an isostatic pressing process; The prefabricated target blank is sintered at high temperature by adopting a high temperature sintering process, and a carbon-containing gas is introduced during the high temperature sintering process to prepare a phase-shift mask substrate alloy target material containing carbon elements.

2. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The carbon-containing gas includes at least one of CO, CO2 and CH4.

3. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The gas flow rate of the carbon-containing gas is 0.1 sccm~1 sccm.

4. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The step of uniformly mixing the high-purity Mo powder and the Si powder comprises: using a high-speed powder ball milling device to ball mill the Mo powder and the Si powder at a ball milling speed of 2000r / min~5000r / min for 2~3h.

5. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The isostatic pressing pressure of the isostatic pressing process is 20 MPa to 30 MPa, and / or the isostatic pressing time is not less than 10 min.

6. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The sintering temperature of the high temperature sintering process is 1400° C. to 1600° C., and the process pressure is 0.5 Pa to 5 Pa.

7. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The high temperature sintering process performs high temperature sintering on the prefabricated target blank under the protection of an inert gas or nitrogen.

8. The method for manufacturing a phase shift mask substrate alloy target according to claim 7, characterized in that: The gas flow rate of the inert gas or the nitrogen gas is 20 sccm to 40 sccm.

9. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The phase-shift mask substrate alloy target material contains carbon in a mass ratio of 0.1% to 1%, and molybdenum and silicon in a mass ratio of 1:4 to 1:

9.

10. The method for manufacturing a phase shift mask substrate alloy target according to claim 1, characterized in that: The average grain size of the phase-shift mask substrate alloy target material is 30μ-50μm.

Citation Information

Cited By

  • Molybdenum-silicon target material and preparation method thereof

    CN121896586A