Ultrafine grain metal target material and preparation method thereof
Rapid rotary forging and cryogenic treatment of metal ingots produce ultrafine-grained targets with improved sputtering rates and uniform thin film deposition, addressing the inefficiencies of existing methods.
Patent Information
- Application Number
- CN202411184827.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for preparing metal targets with fine and uniform grains are complex, costly, and result in uneven grain refinement, limiting their efficiency and uniformity in thin film deposition processes.
A method involving rapid rotary forging of metal ingots followed by cryogenic treatment to suppress grain growth, using a rotary forging process with controlled rotation frequencies and pressures, and liquid nitrogen cooling to achieve ultrafine-grained metal targets.
The method achieves ultrafine-grained metal targets with a simple, low-cost process, ensuring high yield and uniform grain size, enhancing the sputtering rate and thickness distribution of thin films.
Smart Images

Figure CN119061364A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sputtering target materials, and in particular relates to an ultrafine-grained metal target material and a preparation method thereof. Background Art
[0002] Target material is an important material used in thin film preparation processes such as physical coating and chemical vapor deposition. Metal targets are usually made of high-purity metals or alloys, and have the characteristics of high purity, uniformity, and density. Metal targets are widely used in semiconductors, displays, solar cells, optical devices, decorative coatings and other fields. The grain size of the target directly affects the coating process. The finer the grains, the larger the grain boundary area and the greater the impact on the performance. For the same target material, the sputtering rate of a target with fine grains is faster than that of a target with coarse grains; and the thickness distribution of the thin film deposited by the target with a small difference in grain size (uniform distribution) is more uniform. The preparation of metal targets with fine and uniform grains is a necessary condition for achieving efficient and uniform coating.
[0003] At present, the preparation method of metal targets is generally to forge or roll the ingots of smelting or powder metallurgy to obtain dense and fine-grained metal targets. The metal usually needs to undergo severe plastic deformation to obtain fine-grained structure. Commonly used technical means include high-pressure torsion, multi-axis forging, stir friction processing, equal channel angular extrusion, torsion extrusion, etc., but these technologies have high requirements on equipment and stir friction and other means are usually only suitable for surface processing. Patent CN118127358A discloses an oxygen-free high-purity dense fine-grained copper target material and a preparation method thereof, wherein a fine-grained copper target with an average grain size of 40 μm is obtained by two consecutive extrusions; Patent CN109338314A discloses a processing method for an ultrafine-grained copper-manganese alloy target material, wherein the fine-grained copper-manganese alloy target material is prepared through high-temperature forging blanking - multiple rounds of low-temperature three-way forging - recrystallization heat treatment - multiple cold deformation and tempering treatments; Patent CN109201739A discloses a continuous hot rolling-deep cold rolling composite preparation method for high-performance ultrafine-grained copper / aluminum / copper composite strips, wherein fine-grained copper / aluminum / copper composite strips are prepared by continuous hot rolling-deep cold rolling; These methods generally have the problems of complex process flow, high cost, and uneven grain refinement. Summary of the invention
[0004] In view of this, some embodiments provide a method for preparing an ultrafine-grained metal target, comprising:
[0005] Obtain metal ingots;
[0006] The metal ingot is subjected to rapid rotary forging;
[0007] When the metal ingot is rapidly forged to a set temperature, the metal ingot is cryogenically treated to obtain an ultrafine-grained metal target;
[0008] Among them, rapid rotary forging processing includes:
[0009] Placing the metal ingot on a rotating table;
[0010] The metal ingot rotates driven by the rotating table, and pressure is applied from the top and side of the metal ingot during the rotation process; wherein, the rotation frequency of the rotating table is set to 0.2-20 Hz, the working frequency of the rotary forging hammer is set to 100-240 times / min, and the impact energy is greater than 0.1 kJ.
[0011] Furthermore, in some embodiments of the method for preparing ultrafine-grained metal targets, the cryogenic treatment comprises:
[0012] The liquid nitrogen cooling system is used to cool the metal ingot from the bottom and surface.
[0013] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, the set temperature for the rapid rotary forging treatment of the metal ingot is the recrystallization temperature of the metal ingot.
[0014] Some embodiments disclose a method for preparing an ultrafine-grained metal target, wherein the metal ingot comprises a pure metal ingot or an alloy ingot.
[0015] Some embodiments disclose a method for preparing an ultrafine-grained metal target material. For low-melting-point metals, a metal ingot is obtained by a smelting method; for high-melting-point metals, a metal ingot is obtained by a powder metallurgy method.
[0016] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by smelting, a vacuum environment or an inert atmosphere environment is selected; wherein the vacuum degree selection range is 10 -3 ~10 -6 Pa, the inert atmosphere is one or more gases selected from nitrogen, argon or helium.
[0017] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by powder metallurgy, the mechanical pressure of a rotary forging hammer is used to achieve densification of the metal ingots.
[0018] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by powder metallurgy, the mechanical pressure of a rotary forging hammer is used under the protection of an inert atmosphere to achieve densification of the metal ingots.
[0019] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, cold forging is used when rapid rotary forging is used to process metal ingots with high room temperature plasticity; and warm forging is used when rapid rotary forging is used to process metal ingots with low room temperature plasticity.
[0020] On the other hand, some embodiments disclose an ultrafine-grained metal target obtained by a method for preparing an ultrafine-grained metal target.
[0021] The method for preparing an ultrafine-grained metal target disclosed in an embodiment of the present invention subjects a metal ingot to a drastic plastic deformation through a rotary forging process, and then rapidly deep cools it at a suitable temperature to suppress grain growth in a dynamic recrystallization process, thereby obtaining an ultrafine-grained metal target. The method for preparing an ultrafine-grained metal target has a short process, simple operation, low cost, and a high yield rate, and can realize the preparation of a variety of ultrafine-grained metal targets, and has good application prospects in the field of metal target preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the structure of the deep cold rotary forging device disclosed in Example 1.
[0023] Figure 2 This is a fiber optic image of the structure of the ultrafine-grained copper target disclosed in Example 1. DETAILED DESCRIPTION
[0024] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.
[0025] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.
[0026] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0027] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0028] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.
[0029] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.
[0030] In some embodiments, a method for preparing an ultrafine-grained metal target comprises:
[0031] Obtain metal ingots;
[0032] The metal ingot is subjected to rapid rotary forging;
[0033] When the metal ingot is rapidly forged to a set temperature, the metal ingot is cryogenically treated to obtain an ultrafine-grained metal target;
[0034] Among them, rapid rotary forging processing includes:
[0035] Placing the metal ingot on a rotating table;
[0036] The metal ingot rotates driven by the rotating table, and pressure is applied from the top and side of the metal ingot during the rotation process; wherein, the rotation frequency of the rotating table is set to 0.2-20 Hz, the working frequency of the rotary forging hammer is set to 100-240 times / min, and the impact energy is greater than 0.1 kJ.
[0037] Usually, a metal ingot is placed on a rotating table, and a rotary forging hammer is placed around the metal ingot. The rotary forging hammers are located above and on the side of the metal ingot, respectively. The rotary forging hammer located on the side of the metal ingot is placed in two opposite directions in the horizontal direction to apply relative pressure; the rotary forging hammer located above the metal ingot applies pressure downward from above; Figure 1As shown, during the rotation of the turntable, the hammer head located above the metal ingot strikes the ingot axially downward with a set striking energy for forging. At the same time, the turntable rotates at a set rotation speed or frequency, and the two forging hammer heads in the horizontal direction strike the metal ingot radially inward with a set working frequency and striking energy for forging, thereby realizing three-dimensional forging by applying pressure to the metal ingot in three directions. By adjusting the rotation speed of the turntable, the forging frequency of the rotary forging hammer head, and the pressure or striking energy of the rotary forging hammer head, the rotary forging process of different metal ingots is realized.
[0038] The number of rotary forging hammers usually arranged on the side of the metal ingot can be selected according to the size of the metal ingot. One or more groups of rotary forging hammers can be arranged, and the multiple rotary forging hammers are arranged at equal intervals, and the adjacent rotary forging hammers have the same angle. Generally, the larger the diameter of the metal ingot, the more rotary forging hammers can be arranged. For example, one group of rotary forging hammers can be arranged, which are relatively arranged in two opposite directions of the metal ingot; two groups of rotary forging hammers can be arranged, which are relatively arranged in two opposite directions of the metal ingot, and the angle between the two adjacent rotary forging hammers is 90°; three groups of rotary forging hammers can be arranged, which are relatively arranged in pairs on the side of the metal ingot, and the angle between the two adjacent rotary forging hammers is 60°.
[0039] In some embodiments, the working frequency of the forging hammer in the axial direction of the metal ingot is greater than the working frequency of the forging hammer in the radial direction of the metal ingot, and the working frequencies of the two forging hammers in the radial direction of the metal ingot are the same, so as to achieve the deformation of the metal ingot in the axial and radial directions. Generally, under the impact of multiple rotary forging hammers, the metal ingot as a whole undergoes compression deformation in the radial direction and extension deformation in the axial direction.
[0040] In some embodiments, the working frequencies of the forging hammers in multiple directions are the same. The multiple forging hammers arranged in multiple directions strike at the same working frequency. Generally, under the strikes of the multiple rotary forging hammers, the metal ingot as a whole undergoes compression deformation in the radial direction and extension deformation in the axial direction.
[0041] Generally, metals or alloys can be prepared into metal ingots by smelting or powder metallurgy. Generally, low melting point metals or alloys are smelted to obtain ingots, and high melting point refractory metals or alloys are often prepared into ingots by powder metallurgy.
[0042] Usually, metal ingots of specific sizes can be placed on a rotary forging workpiece table, and the rate and amount of rotary forging process can be adjusted according to the type and properties of the metal. At the same time, the rotation speed of the workpiece table can be adjusted for rapid rotary forging to allow the metal ingot to undergo sufficient plastic deformation and grain breakage. During the rotary forging process, the metal ingot heats up due to severe plastic deformation. When the metal ingot heats up to the set temperature, the cooling system is automatically started to achieve deep supercooling to suppress the dynamic recrystallization grain growth, thereby realizing the preparation of ultrafine-grained metal targets.
[0043] In some embodiments of the method for preparing ultrafine-grained metal targets, cryogenic treatment comprises:
[0044] The liquid nitrogen cooling system is used to cool the metal ingot from the bottom and surface. Usually, the device for preparing ultrafine grain metal sheet includes a rotating table, and is provided with a liquid nitrogen cooling system matched with the rotating table, including a cooling circulation system and a liquid nitrogen outward spraying system provided in the device, and the liquid nitrogen cooling system is used to cool the metal ingot from the bottom, surface and other directions of the metal ingot.
[0045] In the preparation method of ultrafine-grained metal target disclosed in some embodiments, the set temperature of the metal ingot rapid rotary forging treatment is the recrystallization temperature of the metal ingot. Generally, the plastic deformation of the metal ingot during the rotary forging process causes its temperature to rise. When the temperature of the metal ingot rises above the recrystallization temperature, it is easy to cause the growth of recrystallized grains. Therefore, when the temperature of the metal ingot reaches the recrystallization temperature, the liquid nitrogen cooling system is started to perform deep supercooling treatment on the metal ingot. The deep supercooling process suppresses the growth of grains and realizes the grain crushing and refinement effect after rotary forging.
[0046] Some embodiments disclose a method for preparing an ultrafine-grained metal target, wherein the metal ingot comprises a pure metal ingot or an alloy ingot.
[0047] In some embodiments, the preparation method of the ultrafine-grained metal target disclosed herein is to obtain metal ingots by smelting for low-melting-point metals, such as aluminum, copper, tantalum, titanium and corresponding metal alloys; and to obtain metal ingots by powder metallurgy for high-melting-point refractory metals, such as tungsten, molybdenum and corresponding metal alloys. Usually, the purity of the metal or metal alloy is above 4N.
[0048] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by smelting, a vacuum environment or an inert atmosphere environment is selected; wherein the vacuum degree selection range is 10 -3 ~10 -6 Pa, the inert atmosphere is one or more gases selected from nitrogen, argon or helium.
[0049] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by powder metallurgy, the mechanical pressure of a rotary forging hammer is used to achieve densification of the metal ingots.
[0050] In the method for preparing ultrafine-grained metal targets disclosed in some embodiments, in the process of obtaining metal ingots by powder metallurgy, the mechanical pressure of a rotary forging hammer is used under the protection of an inert atmosphere to achieve densification of the metal ingots.
[0051] Some embodiments disclose a method for preparing ultrafine-grained metal targets. When rapid rotary forging is used to process metal ingots with high room temperature plasticity, such as copper, aluminum or metal alloys containing copper and aluminum, cold forging is used; when rapid rotary forging is used to process metal ingots with low room temperature plasticity, warm forging is used.
[0052] On the other hand, some embodiments disclose ultrafine-grained metal targets obtained by the method for preparing ultrafine-grained metal targets. Generally, for metal ingots with initial coarse grains obtained by smelting, the average grain size of the prepared ultrafine-grained metal targets can reach 3 to 8 μm; for metal ingots with initial fine grains obtained by powder metallurgy or smelting, the average grain size of the prepared ultrafine-grained metal targets can reach nanometer level.
[0053] The technical details are further illustrated below in conjunction with embodiments.
[0054] Example 1
[0055] Figure 1 This is a fiber optic image of the structure of the ultrafine-grained copper target obtained by the preparation method of the ultrafine-grained metal target disclosed in Example 1.
[0056] In Example 1, the method for preparing an ultrafine-grained copper target includes:
[0057] The cleaned electrolytic copper strips with a purity of 6N were placed in a 2×10 -4 The copper ingot is melted in a vacuum environment of 1300°C at a temperature of 1300°C; a copper ingot with an average particle size of 50 mm is obtained by controlling the cooling rate; the solidified copper ingot is cut into cylindrical copper ingots with a diameter of 200 mm and a height of 30 mm, and the surface is polished to make it clean;
[0058] The copper ingot is placed on a rotary forging worktable, the rotation frequency of the worktable is set to 5 Hz, the working rate of the upper rotary forging head is set to 200 times / minute, the striking energy is set to 1 kJ, and a group of side rotary forging heads are provided, the working rate is set to 100 times / minute, and the striking energy is set to 0.8 kJ; the liquid nitrogen cooling start temperature is set to 480°C, when the temperature of the high-purity copper ingot rises to 480°C due to plastic deformation, the liquid nitrogen cooling system is automatically turned on, so that the temperature of the copper ingot after rotary forging treatment drops rapidly, thereby inhibiting grain growth and realizing the preparation of ultrafine-grained copper targets;
[0059] The average grain size of the copper ingot obtained after smelting is 10 mm. After the copper ingot is treated by the method disclosed in Example 1, an ultrafine-grained copper target is obtained, such as Figure 2 As shown, the average grain size is 3 μm.
[0060] Example 2
[0061] In Example 2, the method for preparing an ultrafine grain high purity copper-manganese alloy target comprises:
[0062] The 5N purity manganese block and 6N copper block, which had been acid-washed and water-washed, were mixed in a weight ratio of 3:7. -4 The copper-manganese alloy ingot is melted in a vacuum environment of 0.04 Pa and at a temperature of 1250° C. The melting is repeated three times to obtain a uniform copper-manganese alloy ingot; the copper-manganese alloy ingot is cut into cylindrical copper-manganese alloy ingots with a diameter of 150 mm and a height of 20 mm, and the surface is polished to make it clean;
[0063] A copper-manganese alloy ingot is placed on a rotary forging worktable, the rotation frequency of the worktable is set to 8 Hz, the working rate of the upper rotary forging ram is set to 150 times / minute, the impact energy is set to 1 kJ, and a group of rotary forging rams are provided on the side of the workpiece, the working rate is set to 90 times / minute, and the impact energy is set to 0.6 kJ; the liquid nitrogen cooling start temperature is set to 500°C, when the temperature of the high-purity copper ingot rises to 500°C due to plastic deformation, the liquid nitrogen cooling system is automatically turned on, so that the temperature of the copper-manganese alloy ingot after rotary forging treatment drops rapidly, thereby inhibiting grain growth and realizing the preparation of ultrafine-grained copper-manganese alloy targets.
[0064] The ultrafine-grained copper-manganese alloy target obtained by the preparation method disclosed in Example 2 has an average grain size of 8 μm.
[0065] Example 3
[0066] In Example 3, the method for preparing an ultrafine-grained molybdenum-rhenium alloy target comprises:
[0067] Nano-scale molybdenum powder and rhenium powder were mixed in a weight ratio of 97:3, and after ball milling, vacuum hot pressing sintering was performed at 1700°C and 40MPa for 100 minutes to obtain a cylindrical molybdenum-rhenium alloy ingot with a diameter of 200 mm and a height of 30 mm; then the surface was polished to make it clean;
[0068] A molybdenum-rhenium alloy ingot is placed on a rotary forging worktable, the rotation frequency of the worktable is set to 2 Hz, the working rate of the upper rotary forging ram is set to 200 times / min, the impact energy is set to 2 kJ, and a group of side rotary forging rams are provided, the working rate is set to 120 times / min, and the impact energy is set to 1 kJ; the liquid nitrogen cooling start temperature is set to 1100°C, so that the temperature of the molybdenum-rhenium ingot after rotary forging treatment drops rapidly, thereby inhibiting grain growth and realizing the preparation of ultrafine-grained molybdenum-rhenium alloy targets; the ultrafine-grained molybdenum-rhenium alloy target obtained by the preparation method disclosed in Example 3 has an average grain size of 550nm.
[0069] The method for preparing an ultrafine-grained metal target disclosed in an embodiment of the present invention subjects a metal ingot to a rotary forging process to cause it to undergo drastic plastic deformation, and then performs rapid deep cooling at an appropriate temperature to suppress grain growth in a dynamic recrystallization process, thereby obtaining an ultrafine-grained metal target. The method for preparing an ultrafine-grained metal target has a short process, simple operation, low cost, and a high yield rate, and can realize the preparation of a variety of ultrafine-grained metal targets, and has good application prospects in the field of metal target preparation.
[0070] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an ultrafine-grained metal target, characterized in that: include: Obtain metal ingots; The metal ingot is subjected to rapid rotary forging; When the metal ingot is rapidly forged to a set temperature, the metal ingot is cryogenically treated to obtain an ultrafine-grained metal target; Among them, rapid rotary forging processing includes: Placing the metal ingot on a rotating table; The metal ingot rotates driven by the rotating table, and pressure is applied from the top and side of the metal ingot during the rotation process; wherein, the rotation frequency of the rotating table is set to 0.2-20 Hz, the working frequency of the rotary forging hammer is set to 100-240 times / min, and the impact energy is greater than 0.1 kJ.
2. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: Cryogenic treatment includes: The liquid nitrogen cooling system is used to cool the metal ingot from the bottom and surface.
3. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: The set temperature of the metal ingot rapid rotary forging process is the recrystallization temperature of the metal ingot.
4. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: The metal ingots include pure metal ingots and alloy ingots.
5. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: For low melting point metals, metal ingots are obtained by smelting; for high melting point metals, metal ingots are obtained by powder metallurgy.
6. The method for preparing an ultrafine-grained metal target according to claim 5, characterized in that: In the process of obtaining metal ingots by smelting, a vacuum environment or an inert atmosphere environment is selected; wherein the vacuum degree selection range is 10 -3 ~10 -6 Pa, the inert atmosphere is one or more gases selected from nitrogen, argon or helium.
7. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: In the process of obtaining metal ingots by powder metallurgy, the mechanical pressure of the rotary forging hammer is used to achieve the densification of the metal ingot.
8. The method for preparing an ultrafine-grained metal target according to claim 7, characterized in that: Under the protection of inert atmosphere, the mechanical pressure of the rotary forging hammer is used to achieve the densification of the metal ingot.
9. The method for preparing an ultrafine-grained metal target according to claim 1, characterized in that: When rapid rotary forging is used to process metal ingots with high room temperature plasticity, cold forging is adopted; when rapid rotary forging is used to process metal ingots with low room temperature plasticity, warm forging is adopted.
10. Ultrafine-grained metal target, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Continuous hot rolling-cryogenic rolling composite preparation method for high performance ultrafine crystal copper / aluminum / copper composite strips
CN109201739A
Processing method of ultrafine-grained copper manganese alloy target material
CN109338314A
Oxygen-free high-purity compact fine-grain copper target material and preparation method thereof
CN118127358A