Zn whisker containing Sn at top and preparation method thereof
By hot-dipping of Al-Sn-Si alloy in Fe-Cr-B cast steel and soaking in ZnCl2 molten salt, the problem of difficulty in growing Zn whiskers after hot-diping of Fe-Cr-B cast steel is solved, and the problem of Zn whiskers growth after hot-diping of aluminum-plated alloy is realized Preparation of Zn whiskers with Sn tops simplifies operation and enriches whisker types.
Patent Information
- Application Number
- CN202411193466.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to self-grow Zn-containing whiskers after hot-dip aluminum-plated alloy of Fe-Cr-B cast steel, especially Zn whiskers, and few have been reported.
Al-Sn-Si alloy heat treatment was carried out by hot-dip plating of Fe-Cr-B cast steel and soaked in subsequent ZnCl2 molten salt, which prompts the solid solution area of Cr-(Al,Sn)-B MAB phase to form Zn with a top Sn Whiskers are used to react diffusion heat and ZnCl2 molten salt to form a solid solution of Cr-(Al, Sn, Zn)-B MAB phase to achieve the growth of Zn whiskers.
Zn whiskers with Sn on the top were successfully prepared. The main body of the whiskers was Zn, and a small amount of Sn was distributed on the top. Sn promoted the formation of Zn vacancies, simplified the operation process, and expanded the types of MAB phases and whisker growth types.
Smart Images

Figure CN119061485A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of new materials, and in particular to a Zn whisker with Sn on the top and a preparation method thereof. Background Art
[0002] The applicant's previous research found that when Fe-Cr-B cast steel is hot-dip aluminum-plated, a periodic lamellar structure (PLS) will be generated at the interface between the boride (Cr,Fe)2B in its structure and the aluminum liquid. The PLS is composed of alternating FeAl3 and Cr-Al-B MAB phases. Elements such as Zn, Si, Sn in the aluminum liquid will significantly affect the composition of the Cr-Al-B MAB phase, and partially replace the Al atoms in the Cr-Al-B MAB phase to form a solid solution. The MAB phase is a special type of atomic layered compound, in which M is a transition metal element, A is a 13-16 group element, and B is a boron element. Among them, when hot-dip Al-Sn alloy is hot-dip plated, Sn whiskers will also spontaneously grow in the Cr-(Al,Sn)-B MAB phase solid solution region formed. However, although the Cr-(Al,Zn)-B MAB phase solid solution is formed when hot-dip Al-Zn alloy is hot-dip plated, Zn whiskers cannot grow. However, Zn whiskers can grow slowly in the solid solution region of Cr-(Al,Zn)-B MAB phase formed by the reaction of Cr-Al-B MAB phase and ZnCl2 molten salt. Therefore, it is still unknown whether it is possible to spontaneously grow Zn whiskers in Fe-Cr-B cast steel after hot-dip aluminum alloying through further alloying.
[0003] The MAB phase is similar to another widely-regarded ternary layered compound MAX phase (X is C or N). In fact, there are many reports on the spontaneous growth of A-site whiskers in the MAX phase, but they are mainly concentrated on Sn whiskers, and there are few reports on Zn whiskers. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a Zn whisker with Sn as the top and a preparation method thereof.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] The invention discloses a Zn whisker with Sn on the top. The whisker has a main body of Zn and a Sn on the top, and grows in a Cr-(Al, Sn, Zn)-B MAB phase solid solution region in a periodic lamellar structure.
[0007] A method for preparing a Zn whisker with Sn on the top comprises the following steps:
[0008] (1) Hot-dip aluminum
[0009] The Fe-Cr-B cast steel was hot-dip plated with Al-Sn-Si alloy, the aluminum melt temperature was 750°C, the hot-dip plating time was 30 minutes, and after reaching the set time, it was taken out and air-cooled to room temperature;
[0010] (2) Diffusion heat treatment
[0011] The sample prepared in step 1 is placed in a muffle furnace for diffusion heat treatment, kept at 750°C for 1 hour, and cooled to room temperature with the furnace after reaching the set temperature;
[0012] (3) Immersion in ZnCl2 molten salt
[0013] The sample prepared in step 2 is immersed in ZnCl2 molten salt at 400-600°C for a certain period of time (5-90 minutes), then taken out and cooled to room temperature; any surface of the prepared sample containing the coating is ground and polished.
[0014] (4) Whisker cultivation
[0015] The polished sample prepared in step 3 is placed in a vacuum or inert or methane atmosphere, kept at 200-300°C for 4 hours, and cooled to room temperature with the furnace after reaching the set temperature. Then, the spontaneous growth of whiskers with complex composition and structure can be observed.
[0016] A Zn whisker with Sn on the top, wherein the main body of the whisker is pure Zn and the top of the whisker is pure Sn, and the two are connected as one.
[0017] A Zn whisker with Sn on the top, a Cr-(Al, Sn, Zn)-B MAB phase solid solution can simultaneously form Sn and Zn vacancies, and Sn can promote the formation of Zn atomic vacancies in the Cr-(Al, Sn, Zn)-B MAB phase solid solution.
[0018] A method for preparing a Zn whisker with Sn on the top, wherein a periodic lamellar structure containing a Cr-(Al, Sn)-B MAB phase solid solution is generated during hot-dip Al-Sn-Si alloy-diffusion heat treatment and then chemically reacts with ZnCl2 molten salt and transforms into a Cr-(Al, Sn, Zn)-B MAB phase solid solution.
[0019] A method for preparing a Zn whisker with Sn on the top, wherein the chemical reaction between a Cr-(Al, Sn)-B MAB phase solid solution and a ZnCl2 molten salt is: Cr-(Al, Sn)-B MAB phase solid solution (solid) + ZnCl2 (liquid) → Cr-(Al, Sn, Zn)-B MAB phase solid solution (solid) + AlCl3 (gas) + Zn (solid).
[0020] A method for preparing a Zn whisker with Sn on the top, wherein the pure Zn phase generated by reaction is distributed on the grain boundary of a Cr-(Al, Sn, Zn)-BMAB phase solid solution.
[0021] A method for preparing a Zn whisker with Sn on the top. The material source of the Zn whisker with Sn on the top is: nanometer-sized pure Zn phase on the grain boundary → Cr-(Al, Sn, Zn)-B MAB phase solid solution → whisker.
[0022] A method for preparing Zn whiskers with Sn on the top, when immersed in ZnCl2 molten salt, the pure Sn phase formed at the grain boundary during the hot-dip Al-Sn-Si alloy-diffusion heat treatment will accelerate the replacement of Al atoms in the Cr-Al-B MAB phase until the pure Sn phase disappears, and the pure Zn phase will be precipitated again at the grain boundary as the main component source for the subsequent whisker growth.
[0023] A method for preparing a Zn whisker with Sn on top, Sn atoms and subsequent Zn 2+ They can only partially replace the Al atoms in the Cr-Al-BMAB phase and form a Cr-(Al,Sn,Zn)-BMAB phase solid solution, but cannot completely replace it.
[0024] The present invention provides a whisker material with complex components and a preparation method thereof, which has the following beneficial effects:
[0025] 1. Cr-(Al, Sn, Zn)-B MAB phase solid solution can be prepared by hot-dip plating of Fe-Cr-B cast steel with Al-Sn-Si alloy, diffusion heat treatment and subsequent immersion in ZnCl2 molten salt. After grinding and polishing, spontaneously grown whiskers with complex components can be observed.
[0026] 2. The main component of the whiskers is Zn, and a small amount of Sn is randomly distributed on the top of the Zn whiskers;
[0027] 3. Sn can promote the formation of Zn vacancies in the Cr-(Al,Sn,Zn)-B MAB phase solid solution, thereby accelerating the Zn;
[0028] 4. Expanded the types of MAB phases and enriched the types of whisker growth;
[0029] 5. When immersing in ZnCl2 molten salt, there is no special requirement for the mass ratio of the sample to the molten salt. There is no need to strictly control the ratio. As long as the sample can be immersed in the molten salt, the operation is greatly simplified and convenient. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0031] Figure 1The cross-sectional microstructure of the Fe-Cr-B cast steel prepared in Example 1 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0032] Figure 2 Cr element distribution diagram of the cross section of the Fe-Cr-B cast steel prepared in Example 1 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0033] Figure 3 The Sn element distribution diagram of the cross section of the Fe-Cr-B cast steel prepared in Example 1 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0034] Figure 4 The Zn element distribution diagram of the cross section of the Fe-Cr-B cast steel prepared in Example 1 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0035] Figure 5 The cross-sectional microstructure of the Fe-Cr-B cast steel prepared in Example 2 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0036] Figure 6 The Sn element distribution diagram of the cross section of the Fe-Cr-B cast steel prepared in Example 2 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt;
[0037] Figure 7 This is the Zn element distribution diagram of the cross section of the Fe-Cr-B cast steel prepared in Example 2 after hot-dip plating of Al-Sn-Si alloy-diffusion heat treatment and then immersion in ZnCl2 molten salt. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be further described below in conjunction with the accompanying drawings.
[0039] It is clear and complete that the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Fe-Cr-B cast steel is prepared by the following method:
[0041] 1. Ingredients: According to the designed alloy composition, calculate the required weight of low-carbon ferrochrome Fe-58wt.%Cr-0.06wt.%C, Fe-18wt.%B master alloy and pig iron, the total weight is 10kg.
[0042] 2. Melting: The raw materials weighed in step ① are loaded into a vacuum melting furnace, and after being completely melted, they are superheated to 1600° C. and kept warm for 15 minutes, and then poured into a metal mold. After cooling, Fe-Cr-B cast steel is obtained.
[0043] The microstructure of the prepared Fe-Cr-B cast steel is mainly composed of gray-black (Cr,Fe)2B phase and gray-white α-Fe. The microstructure in the embodiment is photographed using a backscattered electron mode of a scanning electron microscope. The whiter the contrast, the larger the average atomic number.
[0044] Embodiment 1:
[0045] The prepared Fe-Cr-B cast steel was hot-dip plated with Al-15Sn-5Si (mass percentage, the same below) alloy. The temperature of the aluminum alloy melt was 750°C and the immersion time was 30 minutes. The steel was then taken out and air-cooled to room temperature. The sample was cut in the middle by wire cutting, and a metallographic specimen was prepared after grinding and polishing. The structure was observed using the backscattered electron mode of a scanning electron microscope. It was found that after hot-dip aluminum plating, a periodic lamellar structure consisting of alternating FeAl3 and Cr-Al-B MAB phases was generated on the (Cr,Fe)2B / aluminum alloy melt interface. Among them, the Cr-Al-B MAB phase showed a white contrast ratio in the backscattered electron mode of a scanning electron microscope (representing that its average atomic number becomes larger, replaced by "whitening"), and Sn whiskers can grow. It should be noted that the (Cr,Fe)2B / Al interface reaction occurs first to generate a periodic lamellar structure, and then the Cr-Al-B MAB phase whitening phenomenon occurs due to the diffusion of Sn, that is, the Cr-(Al,Sn)-B MAB phase solid solution is generated. The hot-dip Al-15Sn-4.8Si alloy sample was placed in a muffle furnace for diffusion heat treatment at a temperature of 750°C for 60 minutes and then cooled in the furnace.
[0046] Then, it was immersed in molten ZnCl2 at 500℃ for 10 minutes, and then taken out and air-cooled to room temperature. The sample was cut from the center by wire cutting, and the cross-sectional microstructure was observed by scanning electron microscopy after grinding and polishing. Figure 1 As shown, combined Figure 2 Cr (representing the position of Cr-Al-B MAB phase) shown Figure 3 Sn shown, Figure 4 The surface distribution of Zn elements shown in the figure shows that whiskers with complex structures, whose heads are Sn and whose bodies are Zn, grow spontaneously on the "whitish" Cr-Al-B MAB phase. The Si element in the hot-dip Al-Sn-Si alloy does not participate in the composition of whiskers, but can reduce the oxidation holes in the coating during the subsequent diffusion heat treatment process.
[0047] It should be noted that when immersing in ZnCl2 molten salt, there is no special requirement for the mass ratio of the sample to the molten salt, as long as the sample can be immersed in the molten salt.
[0048] Embodiment 2:
[0049] The prepared Fe-Cr-B cast steel was hot-dip plated with Al-15Sn-5Si alloy. The temperature of the aluminum alloy melt was 750℃, the immersion time was 30 minutes, and then it was taken out and air-cooled to room temperature. The sample was cut from the middle by wire cutting, and the metallographic specimen was prepared after grinding and polishing. The structure was observed by the backscattered electron mode of the scanning electron microscope. It was found that after hot-dip aluminum plating, a periodic lamellar structure composed of FeAl3 and Cr-Al-B MAB phases alternating was generated on the (Cr,Fe)2B / aluminum alloy melt interface. Among them, the Cr-Al-B MAB phase showed a white contrast in the backscattered electron mode of the scanning electron microscope (representing that its average atomic number becomes larger, replaced by "whitening"), and Sn whiskers can grow. It should be noted that the (Cr,Fe)2B / Al interface reaction first occurs to generate a periodic lamellar structure, and then the Cr-Al-B MAB phase whitening phenomenon caused by the diffusion of Sn occurs, that is, the Cr-(Al,Sn)-B MAB phase solid solution is generated. The hot-dip plated Al-15Sn-4.8Si alloy sample was placed in a muffle furnace for diffusion heat treatment at a temperature of 750°C for 60 minutes and then cooled in the furnace.
[0050] Then, it was immersed in ZnCl2 molten salt at 550℃ for 10 minutes, and then taken out and cooled to room temperature. The sample was cut from the center by wire cutting, and after grinding and polishing, it was placed in argon atmosphere for whisker cultivation for 4 hours, and then the cross-sectional microstructure was observed by scanning electron microscopy. Figure 5 As shown, combined Figure 6 Sn shown, Figure 7 The surface distribution of Zn elements shown in the figure shows that whiskers with complex structures, whose heads are Sn and whose bodies are Zn, grow spontaneously on the "whitish" Cr-Al-BMAB phase. The Si element in the hot-dip Al-Sn-Si alloy does not participate in the composition of whiskers, but can reduce the oxidation holes in the coating during the subsequent diffusion heat treatment process.
[0051] It should be noted that when immersing in ZnCl2 molten salt, there is no special requirement for the mass ratio of the sample to the molten salt, as long as the sample can be immersed in the molten salt.
[0052] Embodiment 3:
[0053] The prepared Fe-Cr-B cast steel was hot-dip plated with Al-15Sn-5Si alloy. The temperature of the aluminum alloy melt was 750℃, the immersion time was 30 minutes, and then it was taken out and air-cooled to room temperature. The sample was cut from the middle by wire cutting, and the metallographic specimen was prepared after grinding and polishing. The structure was observed by the backscattered electron mode of the scanning electron microscope. It was found that after hot-dip aluminum plating, a periodic lamellar structure composed of FeAl3 and Cr-Al-B MAB phases alternating was generated on the (Cr,Fe)2B / aluminum alloy melt interface. Among them, the Cr-Al-B MAB phase showed a white contrast in the backscattered electron mode of the scanning electron microscope (representing that its average atomic number becomes larger, replaced by "whitening"), and Sn whiskers can grow. It should be noted that the (Cr,Fe)2B / Al interface reaction first occurs to generate a periodic lamellar structure, and then the Cr-Al-B MAB phase whitening phenomenon caused by the diffusion of Sn occurs, that is, the Cr-(Al,Sn)-B MAB phase solid solution is generated. The hot-dip plated Al-15Sn-4.8Si alloy sample was placed in a muffle furnace for diffusion heat treatment at a temperature of 750°C for 60 minutes and then cooled in the furnace.
[0054] Then it was immersed in 500℃ ZnCl2 molten salt for 90 minutes, and then taken out and air-cooled to room temperature. The sample was cut from the center by wire cutting, and after grinding and polishing, it was placed in an argon atmosphere for whisker cultivation for 4 hours. Then the cross-sectional microstructure was observed by scanning electron microscopy, and it can be seen that whiskers with Sn as the head and Zn as the body and complex structure spontaneously grew on the "whitish" Cr-Al-B MAB phase. The Si element in the hot-dip Al-Sn-Si alloy does not participate in the composition of the whiskers, but can reduce the oxidation holes in the coating during the subsequent diffusion heat treatment process.
[0055] It should be noted that when immersing in ZnCl2 molten salt, there is no special requirement for the mass ratio of the sample to the molten salt, as long as the sample can be immersed in the molten salt.
[0056] The above embodiments are only preferred technical solutions of the invention and should not be regarded as limitations of the invention. The protection scope of the invention should be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the invention.
Claims
1. A Zn whisker with Sn at the top, characterized in that: The whisker has a main body of Zn and a top of Sn, and grows in a Cr-(Al, Sn, Zn)-B MAB phase solid solution region in a periodic lamellar structure.
2. The method for preparing a Zn whisker with Sn at the top according to claim 1, characterized in that: The following steps are involved: (1) Hot-dip aluminum The Fe-Cr-B cast steel was hot-dip plated with Al-Sn-Si alloy, the aluminum melt temperature was 750°C, the hot-dip plating time was 30 minutes, and after reaching the set time, it was taken out and air-cooled to room temperature; (2) Diffusion heat treatment The sample prepared in step 1 is placed in a muffle furnace for diffusion heat treatment, kept at 750°C for 1 hour, and cooled to room temperature with the furnace after reaching the set temperature; (3) Immersion in ZnCl2 molten salt The sample prepared in step 2 is immersed in ZnCl2 molten salt at 400-600°C for a certain period of time (5-90 minutes), then taken out and cooled to room temperature; any surface of the prepared sample containing the coating is ground and polished. (4) Whisker cultivation The polished sample prepared in step 3 is placed in a vacuum or inert or methane atmosphere, kept at 200-300°C for 4 hours, and cooled to room temperature with the furnace after reaching the set temperature. Then, the spontaneous growth of whiskers with complex composition and structure can be observed.
3. The Zn whisker with Sn at the top according to claim 1, characterized in that: The main body of the whisker is pure Zn, while its top is pure Sn, and the two are connected as one.
4. The Zn whisker with Sn at the top according to claim 1, characterized in that: The Cr-(Al,Sn,Zn)-B MAB phase solid solution can form Sn and Zn vacancies at the same time, and Sn can promote the formation of Zn atomic vacancies in the Cr-(Al,Sn,Zn)-B MAB phase solid solution.
5. The method for preparing a Zn whisker with Sn at the top according to claim 2, characterized in that: The periodic lamellar structure containing Cr-(Al,Sn)-B MAB phase solid solution generated during the hot-dip Al-Sn-Si alloy-diffusion heat treatment subsequently reacts chemically with ZnCl2 molten salt and transforms into Cr-(Al,Sn,Zn)-B MAB phase solid solution.
6. The method for preparing a Zn whisker with Sn at the top according to claim 2, characterized in that: The chemical reaction between Cr-(Al,Sn)-B MAB phase solid solution and ZnCl2 molten salt is: Cr-(Al,Sn)-B MAB phase solid solution (solid) + ZnCl2 (liquid) → Cr-(Al,Sn,Zn)-B MAB phase solid solution (solid) + AlCl3 (gas) + Zn (solid).
7. The method for preparing a Zn whisker with Sn at the top according to claim 6, characterized in that: The pure Zn phase generated by the reaction is distributed on the grain boundaries of the Cr-(Al,Sn,Zn)-B MAB phase solid solution.
8. The method for preparing a Zn whisker with Sn at the top according to claim 2, characterized in that: The material origin of the Zn whiskers with Sn on the top is: nano-sized pure Zn phase on the grain boundary → Cr-(Al, Sn, Zn)-B MAB phase solid solution → whiskers.
9. The method for preparing a Zn whisker with Sn at the top according to claim 2, characterized in that: When immersed in ZnCl2 molten salt, the pure Sn phase formed at the grain boundary during the hot-dip Al-Sn-Si alloy-diffusion heat treatment will accelerate the replacement of Al atoms in the Cr-Al-B MAB phase until the pure Sn phase disappears, and the pure Zn phase will re-precipitate at the grain boundary as the main component source for subsequent whisker growth.
10. The method for preparing a Zn whisker with Sn at the top according to claim 2, characterized in that: Sn atoms and subsequent Zn 2+ They can only partially replace the Al atoms in the Cr-Al-B MAB phase and form a Cr-(Al,Sn,Zn)-B MAB phase solid solution, but cannot completely replace it.