Method for preparing fibrilia based on combined degumming of photocatalysis and organic acid treatment
Through the combined method of photocatalytic and organic acid treatment, the problems of incomplete degumming and serious pollution during the degumming of hemp fibers are solved, and efficient and gentle degumming effect is achieved, reducing damage to hemp fibers and environmental pollution.
Patent Information
- Application Number
- CN202411172692.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing degumming methods for hemp fibers have problems such as incomplete degumming, high energy consumption, serious pollution, high cost and complex wastewater treatment. It is difficult to obtain high-quality hemp fibers without damaging the physical properties and chemical structure of the cellulose.
Using a combined method based on photocatalytic and organic acid treatment, the colloidal components in the hemp fiber are removed through weak acid pretreatment and photocatalyst light treatment, the conditions are mild, environmental pollution is reduced, and the degumming effect is improved.
It realizes effective degumming of hemp fibers, reduces damage to fibers, reduces waste liquid generation, improves degumming effect, and is simple to operate and environmentally friendly.
Smart Images

Figure CN119061490A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile processing, and in particular to a method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming. Background Art
[0002] Hemp is a natural bast fiber. As a high-quality natural cellulose resource, hemp fiber is multifunctional. The end products made from hemp can be used in many aspects, such as the textile industry, construction industry, papermaking industry, medical use, biofuel, food and biocomposite materials. Hemp fiber has a bast fiber structure, which is a single cellulose fibril bonded together by a colloid substance. The colloid substance is mainly composed of hemicellulose, pectin, wax, water-soluble materials and lignin. Since a large amount of colloid substance will increase the toughness and yellowness of hemp fiber, it directly limits its further utilization. It is very necessary to extract high-quality hemp fiber from hemp without sacrificing the physical properties or chemical structure of cellulose. Therefore, hemp should be degummed before spinning and preparing textiles to obtain soft and fine spinning hemp fiber.
[0003] At present, the main methods for degumming hemp include physical degumming, traditional alkali degumming, biological degumming, organic solvent degumming and combined degumming. Among them, the physical degumming method is not thorough and is often used as a pretreatment degumming method; the traditional alkali degumming is relatively stable and has a wide range of applications, but it has high energy consumption and serious pollution; biological enzyme degumming can significantly reduce pollution emissions, but the effect of degumming enzymes is single and requires the assistance of chemical reagents; organic solvent degumming can recycle the degumming liquid, but the solvent cost is extremely high, the wastewater needs further treatment, and the degumming effect of organic solvents is limited, and there is also the problem of incomplete degumming. Therefore, it is urgent to develop a degumming method with mild conditions, low environmental pollution and good degumming effect. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming, which has mild reaction conditions, little environmental pollution, good degumming effect, and less damage to hemp fiber.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming, comprising the steps of:
[0007] (1) placing hemp bast fibers into a reactor, adding a weak acid reagent for pretreatment, washing the hemp fibers to neutrality after the pretreatment, and drying them;
[0008] (2) adding a photocatalyst into a glass reactor to prepare a degumming solution, placing the hemp fiber pretreated with a weak acid into the degumming solution for light treatment, and taking out the hemp fiber after the light treatment is completed;
[0009] (3) washing and drying the hemp fiber obtained in step (2) to obtain degummed hemp fiber.
[0010] Furthermore, in the step (1), the solid-to-liquid ratio of the hemp bast fiber to the weak acid reagent is 1:10-30.
[0011] Furthermore, the mass concentration of the weak acid reagent in step (1) is 10-30%.
[0012] Furthermore, in step (1), the weak acid reagent is at least one of glycolic acid and lactic acid.
[0013] Furthermore, in step (1), the weak acid pretreatment temperature is 80-100° C., and the pretreatment time is 2-6 hours.
[0014] Furthermore, in step (2), the photocatalyst is a catalyst that can be excited within the visible light wavelength range, and the amount of the photocatalyst used is 2 to 6 g / kg of hemp fiber.
[0015] In the above technical solution, the photocatalyst is a catalyst that can be excited within the visible light wavelength range, and specifically, TiO 2 -CQDs, ZnO-CQDs, ZnIn 2 S 4 Or other photocatalysts, this type of photocatalyst can be excited within the visible light wavelength range, and visible light accounts for 45% of the total energy of sunlight, and its light utilization rate is high, thereby improving the degumming effect.
[0016] Furthermore, the illumination treatment time in step (2) is 20 to 60 hours.
[0017] Furthermore, the light source used in the illumination treatment in step (2) is sunlight or simulated sunlight, and the simulated sunlight is a light emitting diode or a xenon lamp.
[0018] Furthermore, in the step (2), the solid-bath ratio of the hemp fiber to the degumming solution is 1:10-100.
[0019] Furthermore, the hemp bast fiber is one of ramie, hemp, ramie, kenaf or jute.
[0020] The beneficial effects of the present invention are:
[0021] The present invention provides a method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming, which utilizes weak acid pretreatment and photocatalyst to jointly remove wax, pectin, lignin, hemicellulose and other colloid components in hemp bast fiber. The operation process is simple, the degumming conditions are mild, the degumming effect is good, and the damage to the hemp fiber is small. In addition, the organic acid can be recycled, less waste liquid is generated, and the environmental pollution is small. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 This is the SEM picture of the raw hemp before degumming;
[0024] Figure 2 The TiO provided in Example 1 2 -SEM images of hemp fibers treated with CQDs and acid combined with light. DETAILED DESCRIPTION
[0025] The present invention provides a method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0026] The present invention is described in detail below with reference to the accompanying drawings.
[0027] Example 1
[0028] This embodiment provides a method for preparing hemp fiber by combined degumming based on photocatalysis and organic acid treatment, comprising the steps of:
[0029] (1) placing hemp bast fiber in a reactor, adding a 20% mass concentration of glycolic acid reagent for pretreatment, the solid-liquid ratio of hemp bast fiber to glycolic acid reagent being 1:20, heating at 100° C. for 4 h, and then washing the hemp fiber to neutrality after the pretreatment, and drying in an oven until the fiber weight no longer changes;
[0030] (2) Add 400 ml of 5 g / L TiO 2-The CQDs suspension was added to a 30L glass reactor to prepare a degumming solution, and 1000g of hemp fiber pretreated with weak acid and dried was placed in the degumming solution, water was added to make the solid-bath ratio of the hemp fiber to the degumming solution 1:20, and the hemp fiber was placed under sunlight for 4 days, specifically, 12 hours of light treatment and 12 hours of dark treatment, which was repeated for 4 days. After the light treatment was completed, the hemp fiber was taken out;
[0031] (3) washing and drying the hemp fiber obtained in step (2) to obtain degummed hemp fiber.
[0032] Example 2
[0033] This embodiment provides a method for preparing hemp fiber by combined degumming based on photocatalysis and organic acid treatment, comprising the steps of:
[0034] (1) placing hemp bast fiber in a reactor, adding a 10% mass concentration of glycolic acid reagent for pretreatment, the solid-liquid ratio of hemp bast fiber to glycolic acid reagent being 1:30, heating at 80° C. for 5 h, and then washing the hemp fiber to neutrality after the pretreatment, and drying in an oven until the fiber weight no longer changes;
[0035] (2) Add 500 ml of 8 g / L ZnIn 2 S 4 The suspension was added into a 30L glass reactor to prepare a degumming solution, and 1000g of hemp fiber pretreated with weak acid was placed into the degumming solution, water was added to make the solid-bath ratio of hemp fiber to degumming solution 1:60, and the hemp fiber was treated with LED light for 20h, and the hemp fiber was taken out after the light treatment was completed;
[0036] (3) washing and drying the hemp fiber obtained in step (2) to obtain degummed hemp fiber.
[0037] Comparative Example 1
[0038] This comparative example provides a method for degumming hemp fiber using a photocatalyst, comprising the steps of:
[0039] (1) Add 400 ml 5 g / L TiO 2 -CQDs suspension was added to a 30L glass reactor to prepare a degumming solution, and 1000g of hemp bast fiber was placed in the degumming solution, water was added to make the solid bath ratio of hemp bast fiber to solution 1:20, and dark treatment was carried out for 4 days, and then the hemp fiber was taken out;
[0040] (2) Washing and drying the hemp fiber to obtain degummed hemp fiber.
[0041] Comparative Example 2
[0042] This comparative example provides a method for degumming hemp fiber using a photocatalyst, comprising the steps of:
[0043] (1) Add 400 ml 5 g / L TiO 2 -CQDs suspension was added to a 30L glass reactor to prepare a degumming solution, and 1000g of hemp fiber was placed in the degumming solution, water was added to make the solid-bath ratio of hemp fiber to solution 1:20, and sunlight was applied for 4 days, specifically, 12 hours of light treatment and 12 hours of dark treatment, which was repeated for 4 days, and the hemp fiber was taken out after the light treatment was completed;
[0044] (2) Washing and drying the hemp fiber to obtain degummed hemp fiber.
[0045] Comparative Example 3
[0046] This comparative example provides a method for degumming hemp fiber by acid treatment, comprising the steps of:
[0047] (1) placing hemp bast fiber in a reactor, adding a 20% mass concentration of glycolic acid reagent for pretreatment, the solid-liquid ratio of hemp bast fiber to glycolic acid reagent being 1:20, heating at 100° C. for 4 h, and then washing the hemp fiber to neutrality after the pretreatment, and drying in an oven until the fiber weight no longer changes;
[0048] (2) 1000 g of hemp fiber pretreated with weak acid was placed in a 30 L glass reactor, and water was added, with the solid-bath ratio of hemp fiber to solution being 1:20, and the reactor was kept in the dark for 4 days, and then the hemp fiber was taken out;
[0049] (3) washing and drying the hemp fiber to obtain degummed hemp fiber.
[0050] Comparative Example 4
[0051] This comparative example provides a method for degumming hemp fiber by acid treatment, comprising the steps of:
[0052] (1) placing hemp bast fiber in a reactor, adding a 20% mass concentration of glycolic acid reagent for pretreatment, the solid-liquid ratio of hemp bast fiber to glycolic acid reagent being 1:20, heating at 100° C. for 4 h, and then washing the hemp fiber to neutrality after the pretreatment, and drying in an oven until the fiber weight no longer changes;
[0053] (2) 1000 g of hemp fiber pretreated with weak acid was placed in a 30 L glass reactor, and water was added, the solid-bath ratio of hemp fiber to solution was 1:20, and sunlight was applied for 4 days, specifically, 12 hours of light treatment and 12 hours of dark treatment, which was repeated for 4 days, and then the hemp fiber was taken out;
[0054] (3) washing and drying the hemp fiber to obtain degummed hemp fiber.
[0055] Comparative Example 5
[0056] This comparative example provides a method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming, comprising the steps of:
[0057] (1) placing hemp bast fiber in a reactor, adding a 20% mass concentration of glycolic acid reagent for pretreatment, the solid-liquid ratio of hemp bast fiber to glycolic acid reagent being 1:20, heating at 100° C. for 4 h, and then washing the hemp fiber to neutrality after the pretreatment, and drying in an oven until the fiber weight no longer changes;
[0058] (2) Add 400 ml of 5 g / L TiO 2- The CQDs suspension was added to a 30L glass reactor to prepare a degumming solution, and 1000g of hemp fiber pretreated with weak acid was placed in the degumming solution, and water was added to make the solid-bath ratio of hemp fiber to degumming solution 1:20. The hemp fiber was treated in the dark for 4 days, and the hemp fiber was taken out after the treatment was completed;
[0059] (3) washing and drying the hemp fiber obtained in step (2) to obtain degummed hemp fiber
[0060] The hemp bast fiber before degumming and the degummed hemp fiber of Example 1 were tested using a scanning electron microscope. Figure 1 , 2 .from Figure 1 It can be seen from the figure that the surface of the raw hemp fiber before degumming is rough, covered with thick colloid components, and the fibers are aggregated into bundles; Figure 2 It can be seen that after TiO 2 -CQDs photocatalyst and acid treatment combined with light treatment, the hemp fibers were separated into individual fibers, and the fiber surface was relatively smooth with less colloid content.
[0061] In addition, the chemical composition tests were performed on the degummed hemp fibers prepared in the above-mentioned Example 1 and Comparative Examples 1-5, and the undegummed hemp bast fibers. The test results are shown in Table 1. The physical properties tests were performed on the hemp bast fibers and the degummed hemp fibers prepared in Example 1. The test results are shown in Table 2.
[0062] The above chemical composition test and physical property test methods are as follows:
[0063] Test method for chemical composition: Refer to GB 5889-1986 "Quantitative analysis method for chemical composition of ramie" to test the residual gum rate of degummed hemp fiber.
[0064] Test method for fineness: Refer to GB / T 6100-2007 "Test method for linear density of cotton fibers - mid-section weighing method" to test the fineness of degummed hemp fibers.
[0065] Test method for bundle fiber strength: refer to GB / T 5882-1986 "Test method for breaking strength of ramie bundle fibers" to test the strength of degummed hemp fibers.
[0066] Table 1
[0067]
[0068] Table 2
[0069] Fineness(dtex) Breaking strength (cN / dtex) Hemp bast fiber 8.42±0.08 4.35±0.98 Example 1 6.71±0.14 4.18±0.86
[0070] It can be seen from Table 1 that the above Example 1 uses weak acid and TiO 2 -CQDs were treated under light conditions, and the wax, pectin, lignin, hemicellulose and other colloid removal rates of the prepared hemp fibers were the highest; compared with Example 1, Comparative Example 5 was treated under dark conditions, and its wax, pectin, lignin, hemicellulose and other contents were higher than those of Example 1; Comparative Example 1 used TiO 2 -CQDs were processed in the dark, and the content of each colloid was still very high; Comparative Example 2 only used TiO 2 -CQDs were treated under light conditions, and the content of various gums was still very high, and the gums such as lignin and hemicellulose were only slightly reduced; Comparative Examples 3 and Comparative Examples 4 were treated in the dark or under light using weak acid, and part of the pectin, wax, lignin, hemicellulose, etc. were removed, but the content of pectin, lignin, hemicellulose, etc. was still relatively high.
[0071] It can be seen from Table 2 above that: Example 1 uses weak acid and TiO 2 -CQDs photocatalyst combined degumming process, the fiber fineness after degumming is 6.71dtex, and the breaking strength is 4.18cN / dtex. The degumming effect is good, the colloid bonding between single fibers is reduced, the hemp fiber fineness is finer, and the fiber has better dispersion. The reaction conditions of Example 1 are mild, and the damage to the hemp fiber is less, so that the hemp fiber has better breaking strength, and the breaking strength remains basically unchanged.
[0072] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.
[0073] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming, characterized in that: Includes steps: (1) placing hemp bast fibers into a reactor, adding a weak acid reagent for pretreatment, washing the hemp fibers to neutrality after the pretreatment, and drying them; (2) adding a photocatalyst into a glass reactor to prepare a degumming solution, placing the hemp fiber pretreated with a weak acid into the degumming solution for light treatment, and taking out the hemp fiber after the light treatment is completed; (3) washing and drying the hemp fiber obtained in step (2) to obtain degummed hemp fiber.
2. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: In the step (1), the solid-to-liquid ratio of the hemp bast fiber to the weak acid reagent is 1:10-30.
3. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: The mass concentration of the weak acid reagent in step (1) is 10-30%.
4. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: In the step (1), the weak acid reagent is at least one of glycolic acid and lactic acid.
5. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: In the step (1), the weak acid pretreatment temperature is 80-100° C., and the pretreatment time is 2-6 hours.
6. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: The photocatalyst in step (2) is a catalyst that can be excited within the visible light wavelength range, and the amount of the photocatalyst used is 2-6 g / kg of hemp fiber.
7. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: The illumination treatment time in step (2) is 20 to 60 hours.
8. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: The light source used in the illumination treatment in step (2) is sunlight or simulated sunlight, and the simulated sunlight is a light emitting diode or a xenon lamp.
9. The method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to claim 1, characterized in that: In the step (2), the solid-bath ratio of the flax fiber to the degumming solution is 1:10-100.
10. A method for preparing hemp fiber based on photocatalysis and organic acid treatment combined degumming according to any one of claims 1 to 9, characterized in that: The hemp bast fiber is one of ramie, hemp, apocynum, kenaf or jute.
Citation Information
Patent Citations
Treatment method of textile
CN101643998A
Efficient degumming method for industrial hemp fibers
CN116397336A
A coating method of photocatalyst and oxygen for fabric of fiber, And a fabric of fiber coated by therefor