Superfine 360-degree light-emitting yarn for intelligent wearable low-power-consumption power generation product and preparation method of superfine 360-degree light-emitting yarn
By using ultra-fine 360° luminous yarns combined with conductive yarns in smart wearable products, the problems of high power consumption and poor comfort in traditional luminous yarns are solved, and high efficiency and low luminous emission are achieved Energy consumption, suitable for light and flexible smart devices.
Patent Information
- Application Number
- CN202411370400.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional luminescent yarns have high power consumption, low luminous efficiency, poor comfort in smart wearable products, and insufficient light distribution and luminous emitting areas are used, resulting in waste of energy.
Design an ultra-fine 360° luminescent yarn, which uses conductive yarn to combine with a small light emitting diode and a fluorescent transparent layer, and connects the light emitting diodes in series or parallel manner. The fluorescent transparent layer contains phosphor and thermoplastic polymer particles to achieve 360° luminescent The effect is prepared by melt spinning technology.
It improves luminous efficiency, reduces energy consumption, enhances product comfort and mechanical performance, and is suitable for thin and flexible smart wearable devices, achieving more efficient luminous effects and wider application prospects.
Smart Images

Figure CN119061550A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of flexible electronic wearable technology, and specifically relates to an ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development and widespread application of smart wearable technology, low-power power generation and lighting technology have become a hot topic of research. The application of traditional luminous technology and power generation materials in smart wearable products faces many challenges, such as high power consumption, low luminous efficiency, and poor comfort. Therefore, the development of a luminous yarn that is efficient, energy-saving, and comfortable has become a technical problem that needs to be solved urgently.
[0003] Traditional luminous yarns mainly rely on large luminous elements and large-area FPC patches. Although these technical solutions have guaranteed luminous effects, they are often unsuitable for the needs of smart wearable products in practical applications due to their large size, heavy weight, and lack of comfort. In addition, these traditional solutions also have limitations in the distribution of light and the utilization of the luminous area, which often leads to waste of light efficiency and energy.
[0004] Therefore, it is urgent to design a new luminous yarn. Summary of the invention
[0005] The present invention overcomes the shortcomings of the prior art and provides an ultra-fine 360° luminous yarn and a preparation method for intelligent wearable low-power power generation products, which ensures that the luminous yarn has softness, wear resistance and waterproofness, while improving luminous efficiency, reducing energy consumption and enhancing product comfort.
[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: an ultra-fine 360° luminous yarn for smart wearable low-power power generation products, including conductive yarn, a plurality of light-emitting diodes and a fluorescent transparent layer.
[0007] The conductive yarn is one or more of conductive high molecular polymers, carbon-based conductive materials, and metal-based conductive materials. The conductive yarn connects the positive and negative electrodes at both ends of the light-emitting diode in series or in parallel to form a core yarn.
[0008] The fluorescent transparent layer comprises thermoplastic polymer particles, fluorescent powder and dispersant, and the fluorescent transparent layer wraps the core yarn.
[0009] Furthermore, the length and width of the light-emitting diode are both less than 2 mm, the light-emitting color is one or more of red, green, yellow, blue, and white, and the light-emitting angle is greater than 120°.
[0010] Furthermore, the phosphor includes one or more of YAG yttrium aluminum garnet phosphor, silicate phosphor, and nitride phosphor.
[0011] Furthermore, the thermoplastic polymer particles include at least one of thermoplastic polyurethane elastomer, polyethylene terephthalate, polytrimethylene terephthalate, polyethylene glycol, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene fluoride, fluororesin, polymethyl methacrylate, polycarbonate, polyethylene, polystyrene, polypropylene, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, transparent nylon, polyphenylene ether, and polyoxymethylene.
[0012] Further, the light emitting diode includes one or more of a gallium phosphide light emitting LED chip, a gallium arsenide phosphide light emitting LED chip, a gallium arsenide light emitting LED chip, a gallium indium phosphide gallium arsenide light emitting LED chip, and a gallium aluminum arsenide light emitting LED chip.
[0013] Furthermore, the diameter of the conductive yarn is less than 1 mm.
[0014] Furthermore, the diameter of the ultra-fine 360° luminous yarn used in the smart wearable low-power power generation product is less than 3 mm.
[0015] The present invention also provides a method for preparing an ultrafine 360° luminous yarn for an intelligent wearable low-power power generation product, which is used to prepare the ultrafine 360° luminous yarn for an intelligent wearable low-power power generation product, comprising the following steps:
[0016] S1. Select one or more of conductive polymers, carbon-based conductive materials, and metal-based conductive materials as raw materials, and process the selected conductive materials into conductive yarns with a diameter of less than 1 mm.
[0017] S2. Select a light-emitting diode with a length and width less than 2 mm and a light-emitting color of one or more of red, green, yellow, blue, and white; use the conductive yarn in S1 to connect the positive and negative electrodes of the light-emitting diode in series or in parallel to form a core yarn.
[0018] S3. Select one or more thermoplastic polymer particles such as thermoplastic polyurethane elastomer and polyethylene terephthalate as the base material, add fluorescent powder and dispersant, mix them evenly, and make a fluorescent transparent layer material.
[0019] S4. Put the fluorescent transparent layer material in S3 and the core yarn in S2 into the hopper of the melt spinning machine respectively, and adjust the temperature of the melt spinning machine to the melting range of the thermoplastic polymer particles to ensure that the materials can be melted and extruded smoothly.
[0020] S5. The core yarn in S4 is used as the core layer and is led out from the spinneret core shaft of the melt spinning machine; the spinneret outer shaft of the melt spinning machine is controlled to melt the fluorescent transparent layer material in S4 and extrude it, and evenly wrap it around the core yarn to make a luminous yarn with a diameter less than 3 mm.
[0021] S6. Cool the luminous yarn in S5 to ensure that the fluorescent transparent layer is solidified and tightly wraps the core yarn, and wind and collect the cooled and stretched luminous yarn.
[0022] Furthermore, in step S4, the screw melting temperature of the fluorescent transparent layer material is between 50°C and 550°C.
[0023] Furthermore, in step S5, the draft ratio of the godet roller 1 and the godet roller 2 is controlled at 1.5-2.4, and the spinning speed is 100-500 m / min.
[0024] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0025] (1) The present invention provides an ultra-fine 360° luminous yarn for use in smart wearable low-power power generation products. The yarn has high luminous efficiency and ultra-fine size, ensuring the luminous effect, and can be applied to scenarios that require lightness, thinness, and flexibility, such as smart wearable devices.
[0026] (2) The fluorescent transparent layer of the present invention uses a combination of fluorescent powder and thermoplastic polymer particles. The fluorescent powder can absorb blue light or ultraviolet light emitted by the light-emitting diode and release visible light; the transparency of the thermoplastic polymer particles can minimize the loss of light. At the same time, part of the light in the luminous yarn is reflected back and excites the fluorescent powder again, which excites the fluorescent transparent layer to emit light again, further improving the luminous efficiency and making the luminous yarn brighter. The present invention can use fewer LED chips to achieve a larger area of light, thereby reducing costs and achieving a more efficient luminous effect.
[0027] (3) The present invention uses a smaller light-emitting diode and a conductive yarn, and uses a thinner fluorescent transparent layer to wrap them. The conductive yarn, the light-emitting diode and the fluorescent transparent layer are tightly wrapped together to achieve an ultra-fine size, and the diameter of the final luminous yarn is less than 3mm. Combined with the preparation method of the ultra-fine 360° luminous yarn for smart wearable low-power power generation products provided by the present invention, ultra-fine luminous yarn can be simply and massively produced, and further woven into 2D, 2.5D or 3D fabrics by one or more methods such as weaving, knitting, and braiding, so as to be applied to various smart wearable devices that need to be thin and flexible.
[0028] (4) The luminous yarn provided by the present invention encapsulates the light-emitting diode and the conductive yarn in a fluorescent transparent layer. The fluorescent transparent layer not only provides secondary luminescence to improve the luminous effect of the luminous yarn, but also makes the luminous yarn have a certain hydrophobicity, softness and aesthetic effect, which can better fit the skin and avoid the discomfort of the wearer. In addition, the luminous yarn provided by the present invention can also be combined with low-power power generation products such as micro batteries, piezoelectric materials, and friction nano-power generation materials to provide 360° luminescence, which has a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 is a schematic diagram of the structure of the luminous yarn of the present invention;
[0031] Figure 2 is a flow chart of the method for preparing the luminous yarn of the present invention;
[0032] In the figure: 1. Conductive yarn; 2. Light-emitting diode; 3. Fluorescent transparent layer. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0035] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present application. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the invention, unless otherwise specified, "multiple" means two or more.
[0036] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood by specific circumstances.
[0037] like Figure 1 As shown, an ultra-fine 360° luminous yarn for smart wearable low-power power generation products includes a conductive yarn 1, a plurality of light-emitting diodes 2 and a fluorescent transparent layer 3.
[0038] The conductive yarn 1 is one or more of conductive high molecular polymer, carbon-based conductive material, and metal-based conductive material. The conductive yarn 1 connects the positive and negative electrodes at both ends of a plurality of light-emitting diodes 2 in series or in parallel to form a core yarn.
[0039] The fluorescent transparent layer 3 includes thermoplastic polymer particles, fluorescent powder and dispersant. The fluorescent transparent layer 3 wraps the core yarn and has good hydrophobicity, softness and aesthetic effect.
[0040] Due to the high transparency of thermoplastic polymer particles, the loss of light can be minimized, the luminous efficiency can be improved, and the luminous yarn can be brighter. At the same time, thermoplastic polymer particles have good weather resistance and good flexibility, ensuring that the luminous yarn can maintain good performance in various environments.
[0041] The light emitting diode 2 emits excitation light including blue light or ultraviolet light, and the fluorescent powder in the fluorescent transparent layer 3 absorbs the blue light or ultraviolet light from the light emitting diode 2. After absorbing the excitation light, the fluorescent powder undergoes energy level transition, then releases energy and emits it in the form of visible light with a longer wavelength. Since the thermoplastic polymer particles in the fluorescent transparent layer 3 have high transparency, the visible light emitted by the fluorescent powder will penetrate the thermoplastic polymer particles and scatter from all angles, increasing the luminous area and achieving a 360° luminous effect. Part of the visible light emitted by the fluorescent powder is reflected in the luminous yarn and passes through the light emitting diode 2 to the fluorescent transparent layer on the other side, stimulating the secondary luminescence of the fluorescent transparent layer, achieving the maximum area luminous effect while using the least number of light emitting diodes 2.
[0042] The length and width of the light emitting diode 2 are both less than 2 mm, and can be tightly wrapped on the conductive yarn 1 to improve the light excitation efficiency.
[0043] The light emitting diode 2 emits one or more colors of red, green, yellow, blue, and white, and the light emitting angle is greater than 120°. A light emitting angle of more than 120° can evenly scatter the light emitted by the light emitting diode 2 over a wider range, so that the phosphor can absorb more light and improve the light emitting effect.
[0044] Phosphors include one or more of YAG yttrium aluminum garnet phosphors, silicate phosphors, and nitride phosphors. Different types of phosphors absorb light in a specific wavelength range and emit different colors. Therefore, appropriate phosphors need to be selected according to different application scenarios. YAG yttrium aluminum garnet phosphors can absorb blue light or ultraviolet light and emit yellow light, which produces white light when mixed with blue light. Silicate phosphors can emit a variety of colors such as red, green, yellow, blue, etc. Nitride phosphors can emit blue and green light with high brightness and high color purity.
[0045] Thermoplastic polymer particles include at least one of thermoplastic polyurethane elastomer, polyethylene terephthalate, polytrimethylene terephthalate, polyethylene glycol, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene fluoride, fluororesin, fluororesin-modified polymethyl methacrylate, polycarbonate, high-density polyethylene, polystyrene, polypropylene, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, transparent nylon, polyphenylene ether, and polyoxymethylene.
[0046] The light emitting diode 2 includes one or more of a low-power gallium phosphide light emitting LED chip, a gallium arsenide phosphide light emitting LED chip, a gallium arsenide light emitting LED chip, a gallium indium phosphide gallium arsenide light emitting LED chip, and a gallium aluminum arsenide light emitting LED chip.
[0047] The diameter of the conductive yarn 1 is less than 1 mm, which can effectively reduce the light blocking area caused by the conductive yarn 1 itself, and ensure that the light of the light emitting diode 2 can be absorbed by the fluorescent transparent layer to the greatest extent.
[0048] The diameter of the ultra-fine 360° luminous yarn used in the above-mentioned smart wearable low-power power generation products is less than 3mm. The smaller light-emitting diodes and conductive yarns are wrapped in a thinner fluorescent transparent layer, making the entire luminous yarn very thin. Through one or more methods such as weaving, knitting, and braiding, the luminous yarn can be woven into 2D, 2.5D or 3D fabrics, which is conducive to application in scenarios that require lightness, thinness, and flexibility, such as smart wearable devices.
[0049] like Figure 2 As shown, a method for preparing an ultrafine 360° luminous yarn for a smart wearable low-power power generation product, which is used to prepare the ultrafine 360° luminous yarn for the above-mentioned smart wearable low-power power generation product, comprises the following steps:
[0050] S1. Connect the positive and negative electrodes of the two ends of the light-emitting diode in series or in parallel with the conductive yarn to form a core yarn. Among them, one or more of the conductive polymer, carbon-based conductive material, and metal-based conductive material are made into the conductive yarn by chemical polymerization and impregnation; one or more of the gallium phosphide light-emitting LED chip, gallium arsenide phosphide light-emitting LED chip, gallium arsenide light-emitting LED chip, indium phosphide gallium arsenide light-emitting LED chip, and gallium arsenide aluminum light-emitting LED chip are formed into the light-emitting structure of the light-emitting diode by metal organic chemical vapor deposition (MOCVD) technology.
[0051] S2. Evenly mix the thermoplastic polymer particles, fluorescent components and dispersant to prepare a fluorescent transparent layer material.
[0052] S3, the core yarn in S1 is used as the core layer and is led out from the spinneret core shaft of the melt spinning machine; the spinneret outer shaft of the melt spinning machine is controlled to melt the fluorescent transparent layer material in S2, extrude it, draw it and evenly wrap it around the core yarn. The screw melting temperature is 50-550°C, the traction ratio of the first and second guide rollers is 1.5-4.2, and the spinning speed is 300-600m / min.
[0053] S4, cooling the luminescent yarn in S3 to ensure that the fluorescent transparent layer is solidified and tightly wraps the core yarn, and winding and collecting the cooled luminescent yarn.
[0054] Example 1
[0055] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0056] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0057] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:2:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0058] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn drying due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0059] Example 2
[0060] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0061] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0062] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:3:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0063] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn drying due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0064] Example 3
[0065] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0066] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0067] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0068] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn drying due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0069] Example 4
[0070] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0071] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0072] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:5:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0073] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn drying due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0074] Example 5
[0075] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0076] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0077] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0078] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn dryness due to uneven cooling. The traction ratio of the first and second guide rollers is 3.0, and the spinning speed is 500m / min to produce luminous yarn.
[0079] Example 6
[0080] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0081] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0082] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0083] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn dryness due to uneven cooling. The traction ratio of the first and second guide rollers is 4.2, and the spinning speed is 500m / min to produce luminous yarn.
[0084] Example 7
[0085] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0086] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0087] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0088] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn dryness due to uneven cooling. The traction ratio of the first and second guide rollers is 1.2, and the spinning speed is 500m / min to produce luminous yarn.
[0089] Example 8
[0090] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0091] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0092] The material of the fluorescent transparent layer in this embodiment is a mixture of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. The thermoplastic polyurethane elastomer particles (TPU) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, and sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0093] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in parallel to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circular cooling and blowing are used to avoid uneven yarn dryness due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0094] Example 9
[0095] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0096] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0097] The material of the fluorescent transparent layer in this embodiment is a mixture of polyethylene terephthalate (PET), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS), wherein the ratio of polyethylene terephthalate (PET), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) is 4:4:2. Polyethylene terephthalate (PET) and YAG yttrium aluminum garnet phosphor are mixed evenly in a mixer, sodium polyacrylate (PAAS) is added to the mixture, and the mixture is continuously mixed until it is completely uniform.
[0098] Conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, and the core yarn is placed in the core layer of the spinneret. The material of the fluorescent transparent layer is placed in a melt spinning machine, the screw melting temperature is 95°C, and the fluorescent outer layer is sprayed from the outer layer of the spinneret. Circulating cooling and blowing are used to avoid uneven yarn drying due to uneven cooling. The traction ratio of the first and second guide rollers is 1.5, and the spinning speed is 500m / min to produce luminous yarn.
[0099] Example 10
[0100] The conductive yarn in this embodiment is a mixture of polypyrrole (PPy), graphene and nano silver wires in a ratio of 5:3:2, which ensures the conductivity and flexibility of the conductive yarn. When preparing the conductive yarn, a polypyrrole PPy coating is formed by in-situ polymerization on a fiber substrate by chemical polymerization; graphene and nano silver wires are dispersed in a solvent and formed into a uniform slurry by ultrasonic treatment; the slurry is mixed with a fiber substrate with a polypyrrole PPy coating, and graphene and nano silver wires are evenly distributed on the PPy coating by impregnation to form a conductive network.
[0101] The light emitting diode in this embodiment is a mixture of gallium phosphide light emitting LED wafer and gallium arsenide light emitting LED wafer, wherein the ratio of gallium phosphide light emitting LED wafer to gallium arsenide light emitting LED wafer is 7:3, and has good light emitting efficiency and light emitting wavelength. In particular, when preparing the light emitting diode in this embodiment, metal organic chemical vapor deposition (MOCVD) technology is used to alternately deposit and grow epitaxial layers of gallium phosphide and gallium arsenide on a substrate to form a light emitting layer structure.
[0102] The conductive yarn connects the positive and negative electrodes of several light-emitting diodes in series to form a core yarn, uses cotton yarn as the outer yarn, and adopts the covering yarn process to weave the cotton yarn onto the core yarn to make the luminous yarn.
[0103] The breaking strength and breaking elongation were tested with reference to GB / T 3916-2013, the water contact angle was tested with reference to DB44 / T1872-2016, the luminous intensity was tested with reference to SN / T 2558.7-2014, and the luminous uniformity and black spot of the luminous yarn were tested. The data obtained are shown in Table 1 (luminous yarn performance table):
[0104] Table 1 Luminous yarn performance table
[0105]
[0106] In Examples 1 to 4, the luminous intensity increases according to Examples 1, 2, and 3, and decreases from Example 3 to Example 4, and the luminous intensity as a whole shows a trend of first increasing and then decreasing. Among them, Example 3 has the highest luminous intensity, the best luminous effect, and the light is uniform and has no black spots. This is because the proportions of YAG yttrium aluminum garnet phosphors in the fluorescent transparent layer in Examples 1 to 4 are different. Properly increasing the proportion of YAG yttrium aluminum garnet phosphors can increase the luminous intensity, improve the luminous uniformity, and reduce black spots, while too high a proportion of YAG yttrium aluminum garnet phosphors will lead to a decrease in luminous intensity. When the amount of phosphor added is too high, the interaction between molecules is enhanced, resulting in non-radiative relaxation of excited state energy, collisions or energy transfer between molecules, reduced luminous efficiency, and the generation of black spots or inconsistent brightness; when the amount of phosphor added is too little, the insufficient amount of phosphors leads to a decrease in its ability to absorb the excitation light of the light-emitting diode, resulting in insufficient luminous intensity and uneven brightness accompanied by black spots. In order to avoid the above problems, it is necessary to precisely control the addition ratio of the phosphor to ensure its uniform distribution in the medium and maximize the luminous efficiency. It is concluded from Examples 1 to 4 that when the ratio of thermoplastic polyurethane elastomer particles (TPU), YAG yttrium aluminum garnet phosphor and sodium polyacrylate (PAAS) in the fluorescent transparent layer is 4:4:2, the luminous intensity and luminous effect are best.
[0107] Among Examples 3, 5, 6, and 7, Example 3 has the highest luminous intensity, the best luminous effect, and the strongest mechanical properties. This is because the luminescence of the phosphor involves the transition of electrons between energy levels. At a draw ratio of 1.5, the spacing distribution between the phosphor particles is conducive to the uniform propagation and scattering of light, making the luminescence more uniform. Too high a draw ratio results in too large a spacing between phosphor particles, reduced light scattering, and decreased luminous intensity; too low a draw ratio makes the particle spacing too small, increases light reabsorption, and results in reduced luminous efficiency.
[0108] Example 3 connects the light emitting diodes in series, while Example 8 connects the light emitting diodes in parallel, and the test data of the light emitting yarns of Example 3 and Example 8 are similar. This is because the way of connecting the light emitting diodes in series or in parallel does not affect the mechanical properties, light intensity and light effect of the light emitting yarn.
[0109] Example 3 uses thermoplastic polyurethane elastomer particles (TPU) as the fluorescent transparent layer material, and Example 9 uses polyethylene terephthalate (PET) as the fluorescent transparent layer material. The mechanical properties, luminous intensity and luminous effect of the luminous yarn of Example 3 are better than those of Example 8. This is because the light transmittance and luminous properties of TPU material are better than those of PET material, and TPU material has better flexibility.
[0110] In Example 3, the conductive yarn is used as the core yarn, and the fluorescent outer layer is directly sprayed out; in Example 10, the conductive yarn is used as the core yarn, and the cotton yarn is used as the outer yarn, and the cotton yarn is woven onto the core yarn by the coating yarn process, and the mechanical properties, luminous intensity and luminous effect of the luminous yarn in Example 3 are worse than those in Example 10. This is because the traditional coating yarn process of practical cotton yarn affects the light transmittance, reduces the luminous effect and has insufficient intensity, which is not as good as the manufacturing process of Example 3.
[0111] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. An ultra-fine 360° luminous yarn for smart wearable low-power power generation products, characterized in that: It includes conductive yarn, a plurality of light emitting diodes and a fluorescent transparent layer; The conductive yarn is one or more of a conductive high molecular polymer, a carbon-based conductive material, and a metal-based conductive material, and the conductive yarn is connected to the light-emitting diodes in series or in parallel to form a core yarn; The fluorescent transparent layer comprises thermoplastic polymer particles, fluorescent powder and dispersant, and the fluorescent transparent layer wraps the core yarn.
2. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 1, characterized in that: The length and width of the light emitting diode are both less than 2 mm, the light emitting color is one or more of red, green, yellow, blue, and white, and the light emitting angle is greater than 120°.
3. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 2, characterized in that: The phosphor includes one or more of YAG yttrium aluminum garnet phosphor, silicate phosphor, and nitride phosphor.
4. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 2, characterized in that: The thermoplastic polymer particles include one or more of thermoplastic polyurethane elastomer, polyethylene terephthalate, polytrimethylene terephthalate, polyethylene glycol, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene fluoride, fluororesin, polymethyl methacrylate, polycarbonate, polyethylene, polystyrene, polypropylene, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, transparent nylon, polyphenylene ether, and polyoxymethylene.
5. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 2, characterized in that: The light emitting diode includes one or more of a gallium phosphide light emitting LED chip, a gallium arsenide phosphide light emitting LED chip, a gallium arsenide light emitting LED chip, a gallium indium phosphide gallium arsenide light emitting LED chip, and a gallium aluminum arsenide light emitting LED chip.
6. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 2, characterized in that: The conductive yarn has a diameter of less than 1 mm.
7. The ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 6, characterized in that: The diameter of the ultra-fine 360° luminous yarn used in smart wearable low-power power generation products is less than 3mm.
8. A method for preparing an ultrafine 360° luminous yarn for a smart wearable low-power power generation product, for preparing the ultrafine 360° luminous yarn according to any one of claims 1 to 7, comprising the following steps: S1, connecting the positive and negative electrodes of the light-emitting diodes in series or in parallel with the conductive yarn to form a core yarn; S2, mixing the thermoplastic polymer particles, the fluorescent component and the dispersant uniformly to prepare a fluorescent transparent layer material; S3, using the core yarn in S1 as the core layer, leading it out from the spinneret core shaft of the melt spinning machine; controlling the spinneret outer shaft of the melt spinning machine, melting the fluorescent transparent layer material in S2, extruding, stretching and evenly wrapping it around the core yarn; S4, cooling the luminescent yarn in S3 to ensure that the fluorescent transparent layer is solidified and tightly wraps the core yarn, and winding and collecting the cooled luminescent yarn.
9. The method for preparing the ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 8, characterized in that: In step S3, the screw melting temperature is 50-550° C., the traction ratio between the first godet roller and the second godet roller is 1.2-4.2, and the spinning speed is 300-600 m / min.
10. The method for preparing the ultra-fine 360° luminous yarn for intelligent wearable low-power power generation products according to claim 9, characterized in that: The content of the phosphor in step S2 is 25%-45%.