Preparation method of skin-friendly soft fabric
By combining dyeing, air soft finishing, durable soft finishing, baking and silk protein finishing processes, the problems of bacterial growth and mold prone to home textile fabrics during use are solved, and a hydrophilic fabric with high durability and skin-friendly properties are achieved. Ensure that the fabric is smooth, wash-resistant and formaldehyde-free, meeting the needs of green and environmental protection.
Patent Information
- Application Number
- CN202411035919.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-03
Smart Images

Figure CN119061689A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a fabric, in particular to a method for preparing a skin-friendly and soft fabric, and belongs to the technical field of fabrics. Background Art
[0002] As people's living standards improve, the requirements for home textile fabrics are getting higher and higher. In addition to the requirements for beauty and comfort, the requirements for functionality are also getting higher and higher. Therefore, many functional home textile fabrics are produced to meet the needs of consumers and bring more convenience to people's daily lives. As people's scientific concepts continue to improve, green concepts such as ecology, environmental protection, and pollution-free are becoming more and more popular, and home textile fabrics with green concepts are getting more and more attention from people, and the development prospects are very broad.
[0003] In the prior art, common home textile fabrics for close-fitting include pure cotton fabrics, silk fabrics, linen fabrics, and artificial fiber fabrics or mixed textile fabrics of these raw materials. Although pure cotton fabrics are comfortable, they will breed a large number of bacteria and mites during use, and are prone to mold and taste change. Moreover, they are not suitable for long-term soaking in detergent or long-term exposure, which brings inconvenience to consumers. Although people have tried to add antibacterial agents to treat cotton fabrics with antibacterial agents, such additives are not environmentally friendly and may have a certain impact on human health; silk fabrics have the disadvantages of being difficult to wash and maintain, not easy to take care of, easy to deform and fade, and expensive; linen fabrics have the disadvantages of poor wrinkle resistance, rough surface, dullness, and lack of luster, and are not suitable for skin-friendly clothing; artificial fiber fabrics are uncomfortable when worn and touched by the human body, are easy to irritate the skin, are easy to generate static electricity, and have poor biodegradability and poor skin-friendly performance.
[0004] Existing technical means to improve the softness of fabrics include adding softeners, air finishing, etc. However, although adding softeners can achieve a soft feel, after washing, the softeners are washed away and the fabrics still become hard. Existing air finishing methods to improve the softness of fabrics are to air finish after shaping, which can make the fabric feel soft but the fabric surface is wrinkled and not washable. Although resin finishing can improve durability, general resin finishing has a certain formaldehyde content and cannot meet the standards for infant fabrics.
[0005] Therefore, it is of great significance to develop a method for preparing skin-friendly and soft fabrics that can improve durability and is green and environmentally friendly to meet the existing market consumption needs. Summary of the invention
[0006] In view of the defects of the prior art, the present invention aims to provide a method for preparing skin-friendly and soft fabrics. The fabrics prepared by the method are highly hydrophilic, soft, moist and skin-friendly, and are washable and wrinkle-free, completely formaldehyde-free, and green and safe.
[0007] In order to achieve the above technical objectives, the present invention provides a method for preparing a skin-friendly and soft fabric, which comprises the following steps in sequence:
[0008] Dyeing: The semi-finished fabrics are dyed using continuous reactive dye pad dyeing process;
[0009] Air softening finishing: Use open width air softening machine to air soften the dyed fabrics;
[0010] Durable soft finishing: Use a setting machine to perform durable soft finishing on the fabric that has been air softened;
[0011] Baking: Use a baking machine to bake the durable and soft finished fabrics;
[0012] Silk protein finishing: Use a setting machine to finish the baked fabric with silk protein;
[0013] Calendering: Calendering the fabric treated with silk protein using a calendering machine;
[0014] Pre-shrinkage: Use a pre-shrinkage machine to pre-shrink the calendered fabric.
[0015] The present invention arranges air finishing after dyeing, and then makes the fabric soft after air finishing to ensure that the fabric surface is wrinkle-free; the durability of the fabric is improved through durable soft finishing, and at the same time, combined with the baking process, the resin, softener and fiber in the durable soft finishing process are further cross-linked to achieve smooth, washable and formaldehyde-free durable softness; after baking, on the basis of durable soft finishing, silk protein finishing is further performed to further enhance the skin-friendliness of the fabric.
[0016] As a preferred solution, the durable soft finishing process is: the air-softened fabric is dipped into the durable soft finishing working solution, and then dried and shaped. The drying and shaping temperature is 150-160°C and the time is 2-3 minutes.
[0017] As a preferred solution, the durable soft finishing working solution includes silicone softener, polyurethane softener, modified dimethylol vinyl urea formaldehyde-free resin, magnesium chloride catalyst and acetic acid pH regulator. The present invention adopts modified dimethylol vinyl urea formaldehyde-free resin to ensure the flatness of the fabric surface while achieving formaldehyde-free components, achieving a green and healthy effect.
[0018] As a preferred solution, the concentration of the organic silicon softener is 10-20 g / L. The organic silicon softener includes polyether, amino, epoxy, carboxyl and other modified fabric softeners.
[0019] As a preferred solution, the concentration of the polyurethane softener is 20-40 g / L.
[0020] As a preferred solution, the concentration of the modified dimethylol vinyl urea formaldehyde-free resin is 80-180 g / L.
[0021] As a preferred solution, the concentration of the magnesium chloride catalyst is 20-40 g / L.
[0022] As a preferred solution, the concentration of the acetic acid pH regulator is 1-4 g / L.
[0023] As a preferred solution, during the baking process, the temperature is 150° C. to 160° C. and the time is 2 to 3 minutes.
[0024] As a preferred solution, the silk protein finishing process is: the baked fabric is dipped into the silk protein finishing working solution, and then dried and shaped. The drying and shaping temperature is 150-160°C and the time is 2-3 minutes.
[0025] As a preferred solution, the silk protein finishing working solution includes a silk protein finishing agent and a silicone softener.
[0026] As a preferred solution, the concentration of the silk protein finishing agent is 10-50 g / L.
[0027] As a preferred solution, the concentration of the silicone softener is 5 to 20 g / L.
[0028] As a preferred solution, during the calendering process, the temperature of the mirror roller is 100-120°C, the line pressure is 60-150N / MM, and the vehicle speed is 30-50m / min.
[0029] As a preferred solution, during the pre-shrinking process, the pressure of the load-bearing roller is 10-15 kg, the temperature is 60-80° C., and the vehicle speed is 30-40 m / min.
[0030] As a preferred solution, the semi-finished fabric is obtained by subjecting the original fabric to sequential treatments of singeing, desizing, scouring and bleaching, mercerizing and bio-enzyme polishing.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention improves the hydrophilicity of the fabric. Since the fabric has strong hydrophilicity, the skin feel is improved. The prepared fabric has a soft and moist skin-friendly feel, which improves the sensory evaluation of users and has a good application prospect;
[0033] (2) The fabric prepared by the present invention has a smooth surface and is formaldehyde-free. At the same time, combined with the baking process, the resin, the softener and the fiber are further cross-linked to achieve smoothness, washability, formaldehyde-free and durable softness; after baking, on the basis of durable soft finishing, silk protein finishing is performed to further enhance the skin-friendliness of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0035] Figure 1 The present invention is a process flow chart of preparing a skin-friendly and soft fabric. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The organic silicon softener used in the present invention is a ternary copolymer block silicone oil softener purchased from Suzhou Liansheng Chemical Co., Ltd.
[0038] The silk protein product used in the present invention is Silk Protein was purchased from Zhejiang Fulpusheng New Materials Co., Ltd.
[0039] Example 1
[0040] The following is a preparation method of a skin-friendly and soft fabric finishing process, comprising the following steps:
[0041] (1) Preparation of semi-finished products
[0042] a. Singeing
[0043] A gas singeing machine is used for singeing treatment, with a machine speed of 100m / min. The warp side of the fabric is singed twice, and the weft side is singed twice. The flame temperature of each burner is 1000℃, which ensures that the fabric surface has no long lint and has a good finish.
[0044] b. Desizing
[0045] The desizing machine is used for desizing treatment, with a speed of 100m / min, enzyme stacking for desizing and water washing. After the fabric is singed by open flame, the temperature of the fabric surface is relatively high. It passes through a material trough and a rolling car containing the first working liquid, with a rolling rate of 100%, so that the residual fire on the fabric surface is extinguished, and the first working liquid is rolled into the fabric. The composition of the first working liquid: 3g / L wide-temperature desizing enzyme, 2g / L refining penetrant (alkyl alcohol polyoxyethylene ether fatty acid ester), and the rest is water. Then the fabric is rolled and stacked for 5h, and then passed through a 6-grid washing tank for 6-grid water washing, and washed clean with hot water at a temperature of 95°C to inactivate the wide-temperature desizing enzyme.
[0046] c. Scouring and bleaching
[0047] The fabric is scourred and bleached by an oxygen bleaching machine at a speed of 60 m / min, washed in 4 grids in a 4-grid washing tank with a hot water temperature of more than 90°C, and then passed through a trough containing a working solution and a rolling mill with a rolling rate of 90%. The working solution comprises 10 g / L of a multifunctional scouring agent (alkyl alcohol polyoxyethylene ether fatty acid ester), 6 g / L of a chelating agent (ethylenediaminetetraacetic acid), 4 g / L of a dewaxing agent (sodium fatty acid methyl ester ethoxylate sulfonate), 6 g / L of hydrogen peroxide (100%), and 0.5 g / L of caustic soda flakes; steamed at 101°C for 45 minutes, and then washed in 9 grids in a 9-grid washing tank, and rinsed clean with hot water at a hot water temperature of 95°C.
[0048] d. Mercerizing
[0049] The fabric is mercerized by a straight roller mercerizing machine at a speed of 60 m / min. The fabric passes through multiple pairs of straight rollers for multiple immersion and rolling in NaOH alkali solution with a rolling rate of 100%. The concentration of the NaOH alkali solution is 220 g / L and the temperature of the NaOH alkali solution is 50°C. The fabric is then washed in a 7-grid washing tank with 7 grids and washed clean with hot water at a temperature of 95°C.
[0050] e. Bio-enzyme polishing
[0051] The fabric was polished by bio-enzyme using a jigger. Based on the total mass of the fabric, a bio-enzyme polishing working solution was added. The composition of the bio-enzyme polishing working solution was 2% (owf) cellulase and 0.25% (owf) acetic acid. The working solution temperature was 55°C and the fabric was rotated back and forth for 60 minutes. Then, 2 g / L of soda ash was added, the temperature was raised to 90°C, and the fabric was rotated back and forth for 30 minutes. Then, the fabric was washed with water for 30 minutes.
[0052] f. Dyeing
[0053] The fabric is dyed by continuous reactive dye pad dyeing process using a pad dyeing machine, with a speed of 50m / min, padding dye solution, and a padding rate of 60%. It is then dried with hot air at 100℃ for 2min, and then dipped in a saline-alkali working solution with a padding rate of 60%. The saline-alkali working solution includes 2g / L caustic soda, 20g / L soda ash and 200g / L sodium chloride. It is then steamed at 101℃ for 1 minute, and then washed in a 9-grid washing tank for 9 grids. The fabric is then washed with hot water at a temperature of 95℃.
[0054] g. Air soft finishing
[0055] The fabric is air softened by an open-width air softening machine at a speed of 40m / min. The airflow at 100℃ is sent into the air box at a speed of 2500m / min, sucking the fabric in and kneading the fabric during acceleration. The pressure is released when the fabric is ejected from the air duct, allowing the fabric to expand. When the fabric hits the fence, it is moderately hit and beaten, moving back and forth; the finished fabric has a smooth, soft, fluffy, skin-friendly and soft feel.
[0056] (2) Preparation of skin-friendly and soft fabrics
[0057] The skin-friendly, soft and waxy base fabric obtained by the above process is processed by durable soft finishing and combined with silk protein finishing to obtain a skin-friendly, soft and washable fabric, which specifically includes the following steps:
[0058] h. Durable and soft finishing
[0059] The fabric was subjected to durable soft finishing by using a setting machine, and then dried after being dipped in the durable soft finishing working solution. The drying room temperature of the setting machine was controlled at 150°C and the drying time was 3 minutes. Among them, the durable soft finishing working solution contained 20g / L of silicone softener, 40g / L of polyurethane softener, 180g / L of modified dimethylol vinyl urea formaldehyde-free resin, 40g / L of magnesium chloride catalyst, and 1g / L of acetic acid.
[0060] i. Baking
[0061] The fabric is baked and finished using a baking machine, the baking room temperature is 160°C, and the baking time is 3 minutes.
[0062] j. Silk protein finishing
[0063] The fabric is subjected to silk protein finishing by using a setting machine, and is dried after being dipped in the silk protein finishing working solution, and the drying room temperature of the setting machine is controlled to be 150-160°C, and the drying time is 2-3 minutes. The silk protein finishing working solution contains 50 g / L silk protein and 20 g / L silicone softener.
[0064] k. Calendering
[0065] The fabric is calendered with a calendering machine, the mirror roller is 100°C, the line pressure is 150N / mm, and the speed is 50m / min.
[0066] 1. Pre-shrinkage
[0067] The preshrinking machine is used to preshrink the fabric. The evenly moistened fabric enters between the rubber blanket and the pressure roller and shrinks as the rubber blanket recovers and shrinks. The fabric is then dried by the blanket drying device to improve the stability of the preshrinking effect. The pressure of the load-bearing roller is 15 kg, the temperature is 80°C, and the speed is 40 m / min. After preshrinking, the shrinkage of the fabric is controlled within 3wt%.
[0068] Example 2
[0069] The method of Example 1 was used to prepare a skin-friendly and soft fabric, except that:
[0070] (h) In the durable softening finishing process, the durable softening finishing working solution includes 20 g / L of silicone softener, 40 g / L of polyurethane softener, 80 g / L of modified dimethylol vinyl urea formaldehyde-free resin, 20 g / L of magnesium chloride catalyst, and 1 g / L of acetic acid.
[0071] Example 3
[0072] The method of Example 1 is used to prepare a skin-friendly and soft fabric, except that:
[0073] (h) In the durable softening finishing process, the durable softening finishing working solution includes 20 g / L of silicone softener, 40 g / L of polyurethane softener, 120 g / L of modified dimethylol vinyl urea formaldehyde-free resin, 30 g / L of magnesium chloride catalyst, and 1 g / L of acetic acid.
[0074] Example 4
[0075] The method of Example 3 was used to prepare a skin-friendly and soft fabric, except that:
[0076] (j) During the silk protein finishing process, the silk protein finishing working solution contains 10 g / L silk protein and 20 g / L silicone softener.
[0077] Example 5
[0078] The method of Example 3 was used to prepare a skin-friendly and soft fabric, except that:
[0079] (j) During the silk protein finishing process, the silk protein finishing working solution contains 30 g / L silk protein and 20 g / L silicone softener.
[0080] Comparative Example 1
[0081] The fabric was prepared by the method of Example 3, except that:
[0082] (h) During the durable softening finishing process, the durable softening finishing working solution contains 20 g / L of silicone softener and 40 g / L of polyurethane softener.
[0083] Comparative Example 2
[0084] The fabric was prepared by the method of Example 3, except that:
[0085] (j) During the silk protein finishing process, the silk protein finishing working solution contains 20 g / L of silicone softener.
[0086] The comprehensive properties of the fabrics prepared in Examples 1 to 5 and Comparative Examples 1 to 2 were tested, and the results are shown in Table 1.
[0087] Table 1
[0088]
[0089] It can be seen from the data results in Table 1 that the skin-friendly and soft fabrics prepared in Examples 1 to 5 of the present invention have excellent air permeability, moisture permeability, softness before washing, smoothness before washing, and good skin feel, and also have good softness and smoothness after washing. In contrast, the moisture permeability, softness after washing, and static friction coefficient of smoothness after washing of the fabrics prepared in Comparative Examples 1 and 2 are significantly reduced.
[0090] Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a skin-friendly and soft fabric, characterized in that: The following steps are included in sequence: Dyeing: The semi-finished fabrics are dyed using continuous reactive dye pad dyeing process; Air softening finishing: Use open width air softening machine to air soften the dyed fabrics; Durable soft finishing: Use a setting machine to perform durable soft finishing on the fabric that has been air softened; Baking: Use a baking machine to bake the durable and soft finished fabrics; Silk protein finishing: Use a setting machine to finish the baked fabric with silk protein; Calendering: Calendering the fabric treated with silk protein using a calendering machine; Pre-shrinkage: Use a pre-shrinkage machine to pre-shrink the calendered fabric.
2. The method for preparing a skin-friendly and soft fabric according to claim 1, characterized in that: The process of durable soft finishing is: the fabric which has been air-softened is dipped into the durable soft finishing working liquid, and then dried and shaped.
3. The method for preparing a skin-friendly and soft fabric according to claim 2, characterized in that: The durable soft finishing working solution comprises an organic silicon softener, a polyurethane softener, a modified dimethylol vinyl urea formaldehyde-free resin, a magnesium chloride catalyst and an acetic acid pH regulator.
4. The method for preparing a skin-friendly and soft fabric according to claim 3, characterized in that: The concentration of the silicone softener is 10 to 20 g / L; The concentration of the polyurethane softener is 20 to 40 g / L; The concentration of the modified dimethylol vinyl urea formaldehyde-free resin is 80 to 180 g / L; The concentration of the magnesium chloride catalyst is 20-40 g / L; The concentration of the acetic acid pH regulator is 1-4 g / L.
5. The method for preparing a skin-friendly and soft fabric according to claim 1, characterized in that: The baking treatment is performed at a temperature of 150° C. to 160° C. and for a time of 2 to 3 minutes.
6. The method for preparing a skin-friendly and soft fabric according to claim 1, characterized in that: The silk protein finishing process is as follows: the baked fabric is dipped into the silk protein finishing working liquid, and then dried and shaped.
7. The method for preparing a skin-friendly and soft fabric according to claim 6, characterized in that: The silk protein finishing working solution comprises a silk protein finishing agent and an organic silicon softener.
8. A method for preparing a skin-friendly and soft fabric according to claim 7, characterized in that: The concentration of the silk protein finishing agent is 10 to 50 g / L; The concentration of the organic silicon softener is 5-20 g / L.
9. The method for preparing a skin-friendly and soft fabric according to claim 1, characterized in that: During the calendering process, the mirror roller temperature is 100-120°C, the line pressure is 60-150N / MM, and the vehicle speed is 30-50m / min; During the preshrinking process, the pressure of the load-bearing roller is 10-15 kg, the temperature is 60-80° C., and the vehicle speed is 30-40 m / min.
10. The method for preparing a skin-friendly and soft fabric according to claim 1, characterized in that: The semi-finished fabric is obtained by sequentially subjecting the original fabric to singeing, desizing, scouring and bleaching, mercerizing and bio-enzyme polishing.