Non-woven fabric for antibacterial mask and mask prepared from non-woven fabric
By using PET, carboxymethyl cellulose and hydroxypropyl cellulose in nonwoven fabrics, and vinylation treatment and ultraviolet curing, the antibacterial and water absorption properties of nonwoven fabrics are improved, and the existing nonwoven fabrics are solved. The problems of poor water absorption and water retention and insufficient antibacterial performance have achieved better mask liquid loading and skin care effects.
Patent Information
- Application Number
- CN202411239278.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
AI Technical Summary
Existing non-woven fabrics are poor in water absorption and water retention and antibacterial properties, and are susceptible to bacterial infestation, making it difficult to meet the load of mask liquid and skin care needs.
Non-woven fabrics are prepared using materials such as PET, carboxymethyl cellulose, hydroxypropyl cellulose, and other materials, and non-wovens are improved through 3,3'-diaminobenzophenone, vinyl treatment and ultraviolet curing agents. The antibacterial and hydrophilic properties of the cloth improve the effectiveness of the mask.
It significantly improves the skin-friendly, antibacterial and water-retaining properties of non-woven fabrics, enhances the use effect of the mask, ensures uniform coverage of the mask liquid and long-term antibacterial effect.
Smart Images

Figure BDA0005028729300000091 
Figure BDA0005028729300000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-woven fabric preparation, in particular to a non-woven fabric for an antibacterial facial mask and a facial mask prepared using the non-woven fabric. Background Art
[0002] A facial mask is usually composed of a base fabric and a mask liquid, wherein the base fabric plays the role of carrying and dispersing the mask liquid, so that the mask liquid can be evenly covered on the face to care for the skin; existing mask base fabrics are usually made of non-woven fabrics, which are low in cost and soft in texture compared to conventional textile fabrics. However, existing non-woven fabrics are mostly made of artificial polymer fibers. Compared with cotton fabrics, this type of non-woven fabric has poor water absorption and water retention properties, low mask liquid loading performance, and weak antibacterial properties. It is easy to be invaded by bacteria after being placed for a long time or disassembled for use. Therefore, it is necessary to improve the defects here. Summary of the invention
[0003] The object of the present invention is to provide an antibacterial non-woven fabric for facial mask and a facial mask prepared therefrom, so as to solve the problems raised in the above-mentioned background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0005] S1. Preparing nonwoven fabric;
[0006] S11. PET, carboxymethyl cellulose, hydroxypropyl cellulose and methylene succinic acid are mixed and melted, the mixed melt is filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric;
[0007] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0008] S21. 3,3'-diaminobenzophenone is dispersed in methanol, stirred and mixed for 0.5-1h under nitrogen environment, triethylamine is added, and stirring and mixing is continued for 5-10min, and then cooled to 2-4°C in an ice-water bath, and ether solution of di-tert-butyl dicarbonate is slowly added thereto, and the mixture is stirred and reacted for 8-12h. After removing excess solvent by rotary evaporation, the reaction product is washed with ether for 2-3 times to obtain amino-protected benzophenone;
[0009] S22. The amino-protected benzophenone prepared in step S21 is dispersed in DMF, 4-vinylbenzoic acid and N,N'-dicyclohexylcarbodiimide are added thereto, the temperature is raised to 80-90°C under a nitrogen atmosphere, the reaction is carried out for 2-5 hours, and then the excess solvent is removed by rotary evaporation. The reaction product is dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 5-15°C, stirred for reaction for 6-12 hours, and the excess solvent is evaporated in vacuo, and then washed with deionized water for 3-5 times, and evaporated in vacuo to constant weight to obtain vinylated benzophenone;
[0010] S23. Disperse vinyl benzophenone in methanol, add sodium hydroxide, heat to 55-64°C, stir and disperse for 25-40 minutes, add 1,4-dibromobutane, continue to stir and react for 24-48 hours, remove excess solvent by rotary evaporation, wash the reaction product with deionized water 3-5 times, and disperse it again in a mixed solvent of ethanol and tetrahydrofuran with a volume ratio of 1:4, continue to stir and mix for 1-4 hours, add N,N-dimethyldodecylamine, heat to 40-60°C, stir and react for 12-48 hours, and evaporate in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0011] S24. Disperse the vinylated benzophenone quaternary ammonium salt into pure DMF, heat to 45-60°C, disperse and mix by ultrasonic vibration for 2-4h, add non-woven fabric thereto, irradiate with ultraviolet light for 5-15min, remove, take out the non-woven fabric, wash with deionized water for 3-8 times, and obtain a quaternary ammonium salt modified non-woven fabric;
[0012] S3. Preparation of antibacterial nonwoven fabric for facial mask;
[0013] Disperse sericin in deionized water, heat to 35-45°C, stir and disperse for 8-12 hours, add methacrylic anhydride, cool to 2-5°C, adjust the pH value to 7.5-8, react for 6-8 hours, add ultraviolet curing agent, stir and mix for 0.5-2 minutes, add quaternary ammonium salt modified non-woven fabric, take out after ultraviolet irradiation for 10-15 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
[0014] Furthermore, in step S1, the non-woven fabric comprises the following components by weight: 75-85 parts of PET, 3-5 parts of carboxymethyl cellulose, 8-12 parts of hydroxypropyl cellulose, and 0.5-1 part of methylene succinic acid.
[0015] Furthermore, in step S21, the mass ratio of the 3,3'-diaminobenzophenone, triethylamine and di-tert-butyl dicarbonate is 10:(0.05-0.1):(9-10.5).
[0016] Furthermore, in step S22, the mass ratio of the amino-protected benzophenone, 4-vinylbenzoic acid and N,N'-dicyclohexylcarbodiimide is 10:(2.7-3.5):(0.02-0.04).
[0017] Furthermore, in step S23, the mass ratio of vinylated benzophenone, sodium hydroxide, 1,4-dibromobutane, and N,N-dimethyldodecylamine (213) is 10:(2-4):(3.2-3.7):(3.2-3.8).
[0018] Furthermore, in step S24, the mass ratio of the vinylated benzophenone quaternary ammonium salt to the non-woven fabric is (0.5-5):10.
[0019] Furthermore, in step S3, the mass ratio of the sericin, methacrylic anhydride, ultraviolet curing agent, and quaternary ammonium salt modified non-woven fabric is (1-4): (1-3): (0.05-0.1): 10.
[0020] Furthermore, in step S3, the ultraviolet curing agent is ultraviolet curing agent 2959; and the molecular weight of the sericin is 2000-5000.
[0021] The present application also provides a facial mask, comprising the antibacterial non-woven fabric for the facial mask and the facial mask liquid adsorbed on the non-woven fabric.
[0022] Furthermore, the facial mask liquid comprises the following components by weight: 80-90 parts of water, 0.05-0.15 parts of salicylic acid, 1-3 parts of Centella asiatica extract, 2-3 parts of sodium hyaluronate, and 1-2 parts of hydrolyzed sodium hyaluronate.
[0023] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0024] 1. In order to improve the skin-friendly performance of the non-woven fabric, the present invention uses natural polysaccharide raw materials with bio-affinity such as hydroxypropyl cellulose and carboxymethyl cellulose to blend with PET fiber when preparing the non-woven fabric, which can effectively reduce and improve the bio-affinity of the non-woven fabric;
[0025] 2. In order to further improve the antibacterial and hydrophilic properties of the non-woven fabric, the present invention also performs a modification treatment on the non-woven fabric;
[0026] The present invention first uses 3,3'-diaminobenzophenone as a raw material, and after using di-tert-butyl dicarbonate to protect part of the amino groups therein, it is reacted with 4-vinylbenzoic acid, thereby introducing a vinyl group into the benzophenone, and then the protected amino group is released in an acidic environment, and further reacted with 1,4-dibromobutane, and the substitution reaction between the amino group and the bromine element is used to graft the 1,4-dibromobutane into the vinylated benzophenone. On this basis, the present invention further uses N,N-dimethyldodecylamine to react with it, thereby finally preparing a quaternary ammonium salt with vinyl and benzophenone groups, and then under ultraviolet light irradiation, the benzophenone group reacts with the methylene group in PET, thereby introducing the quaternary ammonium salt into the surface of the non-woven fabric, thereby improving the antibacterial performance of the non-woven fabric; at the same time, because the reaction activity of the vinyl group is poor, it cannot react and cross-link with PET under simple ultraviolet light irradiation, so in this reaction process, the vinyl structure is simultaneously introduced into the surface of the non-woven fabric;
[0027] Afterwards, the present invention uses methacrylic anhydride to modify the sericin and introduces a vinyl structure on its surface. After adding an ultraviolet curing agent, the sericin with a vinyl structure will react and cross-link with the vinyl on the surface of the non-woven fabric, thereby curing the sericin on the surface of the non-woven fabric. The introduction of sericin can effectively improve the hydrophilicity of the non-woven fabric, improve the liquid extraction rate and water retention performance of the facial mask, and achieve improved performance of the facial mask. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The sericin used in this application is Wei's reagent sericin powder with a molecular weight of 3000-4000;
[0030] Embodiment 1. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0031] S1. Preparing nonwoven fabric;
[0032] S11. By weight, 75 parts of PET, 3 parts of carboxymethyl cellulose, 8 parts of hydroxypropyl cellulose, and 0.5 parts of methylene succinic acid were mixed and melted, and the mixed melt was filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric;
[0033] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0034] S21. Disperse 10 parts of 3,3'-diaminobenzophenone in methanol by weight, stir and mix for 0.5 h under nitrogen environment, add 0.05 parts of triethylamine, continue to stir and mix for 5 min, cool to 2 ° C in an ice-water bath, slowly add 9 parts of ether solution of di-tert-butyl dicarbonate thereto, stir and react for 8 h, remove excess solvent by rotary evaporation, wash the reaction product with ether twice to obtain amino-protected benzophenone;
[0035] S22. By weight, 10 parts of the amino-protected benzophenone prepared in step S21 were dispersed in DMF, 2.7 parts of 4-vinylbenzoic acid and 0.04 parts of N,N'-dicyclohexylcarbodiimide were added thereto, the temperature was raised to 80°C under a nitrogen atmosphere, the reaction was continued for 4 hours, and the excess solvent was removed by rotary evaporation. The reaction product was dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 8°C, stirred for 6 hours, and the excess solvent was evaporated in vacuo. The product was washed with deionized water 3 times and evaporated in vacuo to constant weight to obtain vinylated benzophenone.
[0036] S23. By weight, 10 parts of vinyl benzophenone were dispersed in methanol, 2 parts of sodium hydroxide were added, the temperature was raised to 55 ° C, and the mixture was stirred and dispersed for 25 minutes. Then, 3.2 parts of 1,4-dibromobutane were added, and the reaction was continued to stir for 24 hours. The excess solvent was removed by rotary evaporation, and the reaction product was washed with deionized water 3 times. Then, the mixture was dispersed again in a mixed solvent of ethanol and tetrahydrofuran in a volume ratio of 1:4, and the mixture was stirred and mixed for 3 hours. Then, 3.2 parts of N,N-dimethyldodecylamine were added, the temperature was raised to 40 ° C, the reaction was stirred for 36 hours, and the mixture was evaporated in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0037] S24. Disperse 0.5 parts of vinyl benzophenone quaternary ammonium salt in pure DMF by weight, heat to 55 ° C, disperse and mix by ultrasonic vibration for 2 hours, add 10 parts of non-woven fabric, irradiate with ultraviolet light for 8 minutes, remove, take out the non-woven fabric, wash it with deionized water 5 times, and obtain a quaternary ammonium salt modified non-woven fabric;
[0038] S3. Preparation of antibacterial nonwoven fabric for facial mask;
[0039] Disperse 1 part of sericin in deionized water, heat to 35°C, stir and disperse for 8 hours, add 1 part of methacrylic anhydride, cool to 2°C, adjust the pH value to 7.5, react for 6 hours, add 0.08 parts of UV curing agent 2959, stir and mix for 0.5 minutes, add 10 parts of quaternary ammonium salt modified non-woven fabric, take out after ultraviolet irradiation for 10 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
[0040] Embodiment 2. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0041] Compared with Example 1, the amount of 4-vinylbenzoic acid added in step S22 is increased in this example, and the other steps remain unchanged;
[0042] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0043] S21. Disperse 10 parts of 3,3'-diaminobenzophenone in methanol by weight, stir and mix for 0.5 h under nitrogen environment, add 0.05 parts of triethylamine, continue to stir and mix for 5 min, cool to 2 ° C in an ice-water bath, slowly add 9 parts of ether solution of di-tert-butyl dicarbonate thereto, stir and react for 8 h, remove excess solvent by rotary evaporation, wash the reaction product with ether twice to obtain amino-protected benzophenone;
[0044] S22. By weight, 10 parts of the amino-protected benzophenone prepared in step S21 were dispersed in DMF, 3.5 parts of 4-vinylbenzoic acid and 0.04 parts of N,N'-dicyclohexylcarbodiimide were added thereto, the temperature was raised to 80°C under a nitrogen atmosphere, the reaction was continued for 4 hours, and the excess solvent was removed by rotary evaporation. The reaction product was dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 8°C, stirred for 6 hours, and the excess solvent was evaporated in vacuo. The product was washed with deionized water 3 times and evaporated in vacuo to constant weight to obtain vinylated benzophenone;
[0045] S23. By weight, 10 parts of vinyl benzophenone were dispersed in methanol, 2 parts of sodium hydroxide were added, the temperature was raised to 55 ° C, and the mixture was stirred and dispersed for 25 minutes. Then, 3.2 parts of 1,4-dibromobutane were added, and the reaction was continued to stir for 24 hours. The excess solvent was removed by rotary evaporation, and the reaction product was washed with deionized water 3 times. Then, the mixture was dispersed again in a mixed solvent of ethanol and tetrahydrofuran in a volume ratio of 1:4, and the mixture was stirred and mixed for 3 hours. Then, 3.2 parts of N,N-dimethyldodecylamine were added, the temperature was raised to 40 ° C, the reaction was stirred for 36 hours, and the mixture was evaporated in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0046] S24. Disperse 0.5 parts of vinylated benzophenone quaternary ammonium salt into pure DMF by weight, heat to 55°C, disperse and mix by ultrasonic vibration for 2 hours, add 10 parts of non-woven fabric, irradiate with ultraviolet light for 8 minutes, remove the non-woven fabric, take out the non-woven fabric, wash it with deionized water 5 times, and obtain quaternary ammonium salt modified non-woven fabric.
[0047] Embodiment 3. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0048] Compared with Example 1, the present embodiment increases the amount of vinylated benzophenone quaternary ammonium salt added in step S24, and the other steps remain unchanged;
[0049] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0050] S21. Disperse 10 parts of 3,3'-diaminobenzophenone in methanol by weight, stir and mix for 0.5 h under nitrogen environment, add 0.05 parts of triethylamine, continue to stir and mix for 5 min, cool to 2 ° C in an ice-water bath, slowly add 9 parts of ether solution of di-tert-butyl dicarbonate thereto, stir and react for 8 h, remove excess solvent by rotary evaporation, wash the reaction product with ether twice to obtain amino-protected benzophenone;
[0051] S22. By weight, 10 parts of the amino-protected benzophenone prepared in step S21 were dispersed in DMF, 2.7 parts of 4-vinylbenzoic acid and 0.04 parts of N,N'-dicyclohexylcarbodiimide were added thereto, the temperature was raised to 80°C under a nitrogen atmosphere, the reaction was continued for 4 hours, and the excess solvent was removed by rotary evaporation. The reaction product was dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 8°C, stirred for 6 hours, and the excess solvent was evaporated in vacuo. The product was washed with deionized water 3 times and evaporated in vacuo to constant weight to obtain vinylated benzophenone.
[0052] S23. By weight, 10 parts of vinyl benzophenone were dispersed in methanol, 2 parts of sodium hydroxide were added, the temperature was raised to 55 ° C, and the mixture was stirred and dispersed for 25 minutes. Then, 3.2 parts of 1,4-dibromobutane were added, and the reaction was continued to stir for 24 hours. The excess solvent was removed by rotary evaporation, and the reaction product was washed with deionized water 3 times. Then, the mixture was dispersed again in a mixed solvent of ethanol and tetrahydrofuran in a volume ratio of 1:4, and the mixture was stirred and mixed for 3 hours. Then, 3.2 parts of N,N-dimethyldodecylamine were added, the temperature was raised to 40 ° C, the reaction was stirred for 36 hours, and the mixture was evaporated in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0053] S24. Disperse 5 parts of vinylated benzophenone quaternary ammonium salt into pure DMF by weight, heat to 55°C, disperse and mix by ultrasonic vibration for 2 hours, add 10 parts of non-woven fabric, irradiate with ultraviolet light for 8 minutes, remove the non-woven fabric, take out the non-woven fabric, wash it with deionized water 5 times, and obtain quaternary ammonium salt modified non-woven fabric.
[0054] Embodiment 4. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0055] Compared with Example 1, the amount of sericin added in step S3 is increased in this example, and the other steps remain unchanged;
[0056] S3. Preparation of antibacterial nonwoven fabric for facial mask;
[0057] Disperse 4 parts of sericin into deionized water, heat to 35°C, stir and disperse for 8 hours, add 1 part of methacrylic anhydride, cool to 2°C, adjust the pH value to 7.5, react for 6 hours, add 0.08 parts of UV curing agent 2959, stir and mix for 0.5 minutes, add 10 parts of quaternary ammonium salt modified non-woven fabric, take out after ultraviolet irradiation for 10 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
[0058] Embodiment 5. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0059] S1. Preparing nonwoven fabric;
[0060] S11. By weight, 75 parts of PET, 3 parts of carboxymethyl cellulose, 8 parts of hydroxypropyl cellulose, and 0.5 parts of methylene succinic acid were mixed and melted, and the mixed melt was filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric;
[0061] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0062] S21. Disperse 10 parts of 3,3'-diaminobenzophenone in methanol by weight, stir and mix for 0.5 h under nitrogen environment, add 0.1 parts of triethylamine, continue to stir and mix for 5 min, cool to 2 ° C in an ice-water bath, slowly add 10.5 parts of ether solution of di-tert-butyl dicarbonate thereto, stir and react for 8 h, remove excess solvent by rotary evaporation, wash the reaction product with ether twice to obtain amino-protected benzophenone;
[0063] S22. By weight, 10 parts of the amino-protected benzophenone prepared in step S21 were dispersed in DMF, 3.5 parts of 4-vinylbenzoic acid and 0.04 parts of N,N'-dicyclohexylcarbodiimide were added thereto, the temperature was raised to 80°C under a nitrogen atmosphere, the reaction was continued for 4 hours, and the excess solvent was removed by rotary evaporation. The reaction product was dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 8°C, stirred for 6 hours, and the excess solvent was evaporated in vacuo. The product was washed with deionized water 3 times and evaporated in vacuo to constant weight to obtain vinylated benzophenone;
[0064] S23. By weight, 10 parts of vinyl benzophenone were dispersed in methanol, 4 parts of sodium hydroxide were added, the temperature was raised to 55 ° C, and the mixture was stirred and dispersed for 25 minutes. Then, 3.7 parts of 1,4-dibromobutane were added, and the reaction was continued to stir for 24 hours. The excess solvent was removed by rotary evaporation, and the reaction product was washed with deionized water 3 times. Then, the mixture was dispersed again in a mixed solvent of ethanol and tetrahydrofuran in a volume ratio of 1:4, and the mixture was stirred and mixed for 3 hours. Then, 3.8 parts of N,N-dimethyldodecylamine were added, the temperature was raised to 40 ° C, the reaction was stirred for 36 hours, and the mixture was evaporated in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0065] S24. Disperse 5 parts of vinyl benzophenone quaternary ammonium salt in pure DMF by weight, heat to 55 ° C, disperse and mix by ultrasonic vibration for 2 hours, add 10 parts of non-woven fabric, irradiate with ultraviolet light for 8 minutes, remove, take out the non-woven fabric, wash it with deionized water 5 times, and obtain a quaternary ammonium salt modified non-woven fabric;
[0066] S3. Preparation of antibacterial nonwoven fabric for facial mask;
[0067] Disperse 4 parts of sericin into deionized water, heat to 35°C, stir and disperse for 8 hours, then add 3 parts of methacrylic anhydride, cool to 2°C, adjust the pH value to 7.5, react for 6 hours, add 0.08 parts of UV curing agent 2959, stir and mix for 0.5 minutes, add 10 parts of quaternary ammonium salt modified non-woven fabric, take out after ultraviolet irradiation for 10 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
[0068] Embodiment 6. A mask made of non-woven fabric for antibacterial facial mask, the preparation method of which comprises the following steps:
[0069] Compared with Example 1, this embodiment adds a process of impregnating the antibacterial mask nonwoven fabric with mask liquid;
[0070] The antibacterial mask non-woven fabric is immersed in the mask liquid, and after being immersed for 2 hours at a temperature of 45° C., the mask is taken out and packaged to obtain a mask;
[0071] Wherein, the facial mask liquid includes the following components by weight: 80 parts of water, 0.15 parts of salicylic acid, 3 parts of Centella asiatica extract, 3 parts of sodium hyaluronate, and 1 part of hydrolyzed sodium hyaluronate.
[0072] Comparative Example 1. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0073] Compared with Example 1, this comparative example did not prepare a quaternary ammonium salt-modified nonwoven fabric;
[0074] S1. Preparing nonwoven fabric;
[0075] S11. By weight, 75 parts of PET, 3 parts of carboxymethyl cellulose, 8 parts of hydroxypropyl cellulose, and 0.5 parts of methylene succinic acid were mixed and melted, and the mixed melt was filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric;
[0076] S3. Preparation of antibacterial nonwoven fabric for facial mask;
[0077] Disperse 1 part of sericin in deionized water, heat to 35°C, stir and disperse for 8 hours, add 1 part of methacrylic anhydride, cool to 2°C, adjust the pH value to 7.5, react for 6 hours, add 0.08 parts of UV curing agent 2959, stir and mix for 0.5 minutes, add 10 parts of non-woven fabrics, take out after ultraviolet irradiation for 10 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
[0078] Comparative Example 2. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0079] Compared with Example 1, this comparative example only prepared a quaternary ammonium salt-modified nonwoven fabric;
[0080] S1. Preparing nonwoven fabric;
[0081] S11. By weight, 75 parts of PET, 3 parts of carboxymethyl cellulose, 8 parts of hydroxypropyl cellulose, and 0.5 parts of methylene succinic acid were mixed and melted, and the mixed melt was filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric;
[0082] S2. Preparation of quaternary ammonium salt modified nonwoven fabric;
[0083] S21. Disperse 10 parts of 3,3'-diaminobenzophenone in methanol by weight, stir and mix for 0.5 h under nitrogen environment, add 0.05 parts of triethylamine, continue to stir and mix for 5 min, cool to 2 ° C in an ice-water bath, slowly add 9 parts of ether solution of di-tert-butyl dicarbonate thereto, stir and react for 8 h, remove excess solvent by rotary evaporation, wash the reaction product with ether twice to obtain amino-protected benzophenone;
[0084] S22. By weight, 10 parts of the amino-protected benzophenone prepared in step S21 were dispersed in DMF, 2.7 parts of 4-vinylbenzoic acid and 0.04 parts of N,N'-dicyclohexylcarbodiimide were added thereto, the temperature was raised to 80°C under a nitrogen atmosphere, the reaction was continued for 4 hours, and the excess solvent was removed by rotary evaporation. The reaction product was dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 8°C, stirred for 6 hours, and the excess solvent was evaporated in vacuo. The product was washed with deionized water 3 times and evaporated in vacuo to constant weight to obtain vinylated benzophenone.
[0085] S23. By weight, 10 parts of vinyl benzophenone were dispersed in methanol, 2 parts of sodium hydroxide were added, the temperature was raised to 55 ° C, and the mixture was stirred and dispersed for 25 minutes. Then, 3.2 parts of 1,4-dibromobutane were added, and the reaction was continued to stir for 24 hours. The excess solvent was removed by rotary evaporation, and the reaction product was washed with deionized water 3 times. Then, the mixture was dispersed again in a mixed solvent of ethanol and tetrahydrofuran in a volume ratio of 1:4, and the mixture was stirred and mixed for 3 hours. Then, 3.2 parts of N,N-dimethyldodecylamine were added, the temperature was raised to 40 ° C, the reaction was stirred for 36 hours, and the mixture was evaporated in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt;
[0086] S24. Disperse 0.5 parts of vinylated benzophenone quaternary ammonium salt into pure DMF by weight, heat to 55°C, disperse and mix by ultrasonic vibration for 2 hours, add 10 parts of non-woven fabric, irradiate with ultraviolet light for 8 minutes, remove the non-woven fabric, take out the non-woven fabric, wash it with deionized water 5 times, and obtain quaternary ammonium salt modified non-woven fabric.
[0087] Comparative Example 3. A method for preparing a non-woven fabric for an antibacterial facial mask, comprising the following steps:
[0088] Compared with Example 1, this comparative example only prepared non-woven fabric;
[0089] S1. Preparing nonwoven fabric;
[0090] S11. According to weight proportions, 75 parts of PET, 3 parts of carboxymethyl cellulose, 8 parts of hydroxypropyl cellulose and 0.5 parts of methylene succinic acid are mixed and melted, the mixed melt is filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric.
[0091] Test: The nonwoven fabrics prepared in Examples 1-5 and Comparative Examples 1-3 were prepared to have a gram weight of 65±2 g / m 2 Fabrics;
[0092] The nonwoven fabrics prepared in the above Examples 1-5 and Comparative Examples 1-3 were immersed in deionized water for two hours, then removed, and the squeeze rate was calculated according to the formula of squeeze rate = (fabric weight after squeeze - fabric weight before squeeze) / fabric weight before squeeze;
[0093] According to GB / T 20944.3-2008, the samples prepared in Examples 1-5 and Comparative Examples 1-3 were tested for antibacterial properties. The test results are shown in the following table;
[0094]
[0095]
[0096] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a non-woven fabric for an antibacterial facial mask, characterized in that: The following steps are involved: S1. Preparing nonwoven fabric; S11. PET, carboxymethyl cellulose, hydroxypropyl cellulose and methylene succinic acid are mixed and melted, the mixed melt is filtered through a melt filter, extruded and spun, and hot-rolled to form a non-woven fabric; S2. Preparation of quaternary ammonium salt modified nonwoven fabric; S21. 3,3'-diaminobenzophenone is dispersed in methanol, stirred and mixed for 0.5-1h under nitrogen environment, triethylamine is added, stirring and mixing is continued for 5-10min, and then cooled to 2-4°C in an ice-water bath, and ether solution containing di-tert-butyl dicarbonate is slowly added thereto, stirred and reacted for 8-12h, excess solvent is removed by rotary evaporation, and the reaction product is washed with ether for 2-3 times to obtain amino-protected benzophenone; S22. The amino-protected benzophenone prepared in step S21 is dispersed in DMF, 4-vinylbenzoic acid and N,N'-dicyclohexylcarbodiimide are added thereto, the temperature is raised to 80-90°C under a nitrogen atmosphere, the reaction is carried out for 2-5 hours, and then the excess solvent is removed by rotary evaporation. The reaction product is dispersed in a saturated hydrogen chloride solution of tetrahydrofuran, cooled to 5-15°C, stirred for reaction for 6-12 hours, and the excess solvent is evaporated in vacuo, and then washed with deionized water for 3-5 times, and evaporated in vacuo to constant weight to obtain vinylated benzophenone; S23. Disperse vinyl benzophenone in methanol, add sodium hydroxide, heat to 55-64°C, stir and disperse for 25-40 minutes, add 1,4-dibromobutane, continue to stir and react for 24-48 hours, remove excess solvent by rotary evaporation, wash the reaction product with deionized water 3-5 times, and disperse it again in a mixed solvent of ethanol and tetrahydrofuran with a volume ratio of 1:4, continue to stir and mix for 1-4 hours, add N,N-dimethyldodecylamine, heat to 40-60°C, stir and react for 12-48 hours, and evaporate in vacuo to constant weight to obtain vinyl benzophenone quaternary ammonium salt; S24. Disperse the vinylated benzophenone quaternary ammonium salt into pure DMF, heat to 45-60°C, disperse and mix by ultrasonic vibration for 2-4h, add non-woven fabric thereto, irradiate with ultraviolet light for 5-15min, remove, take out the non-woven fabric, wash with deionized water for 3-8 times, and obtain a quaternary ammonium salt modified non-woven fabric; S3. Preparation of antibacterial nonwoven fabric for facial mask; Disperse sericin in deionized water, heat to 35-45°C, stir and disperse for 8-12 hours, add methacrylic anhydride, cool to 2-5°C, adjust the pH value to 7.5-8, react for 6-8 hours, add ultraviolet curing agent, stir and mix for 0.5-2 minutes, add quaternary ammonium salt modified non-woven fabric, take out after ultraviolet irradiation for 10-15 minutes, wash the non-woven fabric with hot water at a temperature of 65-70°C, and obtain antibacterial non-woven fabric for facial mask after drying.
2. The method for preparing a nonwoven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S1, the non-woven fabric comprises the following components by weight: 75-85 parts of PET, 3-5 parts of carboxymethyl cellulose, 8-12 parts of hydroxypropyl cellulose, and 0.5-1 part of methylene succinic acid.
3. The method for preparing a nonwoven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S21, the mass ratio of 3,3'-diaminobenzophenone, triethylamine and di-tert-butyl dicarbonate is 10:(0.05-0.1):(9-10.5).
4. The method for preparing a nonwoven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S22, the mass ratio of the amino-protected benzophenone, 4-vinylbenzoic acid and N,N'-dicyclohexylcarbodiimide is 10:(2.7-3.5):(0.02-0.04).
5. The method for preparing a non-woven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S23, the mass ratio of vinylated benzophenone, sodium hydroxide, 1,4-dibromobutane and N,N-dimethyldodecylamine (213) is 10:(2-4):(3.2-3.7):(3.2-3.8).
6. The method for preparing a nonwoven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S24, the mass ratio of the vinylated benzophenone quaternary ammonium salt to the non-woven fabric is (0.5-5):
10.
7. The method for preparing a nonwoven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S3, the mass ratio of the sericin, methacrylic anhydride, ultraviolet curing agent, and quaternary ammonium salt modified non-woven fabric is (1-4): (1-3): (0.05-0.1):
10.
8. The method for preparing a non-woven fabric for an antibacterial facial mask according to claim 1, characterized in that: In step S3, the ultraviolet curing agent is ultraviolet curing agent 2959; the molecular weight of the sericin is 2000-5000.
9. A facial mask, characterized in that: It comprises the antibacterial nonwoven fabric for facial mask as described in any one of claims 1 to 8, and the facial mask liquid adsorbed on the antibacterial nonwoven fabric for facial mask.