Continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fiber
Through ultrasonic-alkali reduction combined modification treatment and in-situ polymerization, polypyrrole/polyurethane/polyester composite conductive fibers are formed, which solves the problems of conductive layer stability and wear resistance, and achieves high durability and excellent conductive properties. Continuous preparation of pyrrole/polyester conductive fibers.
Patent Information
- Application Number
- CN202411563913.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-05
AI Technical Summary
The prior art is difficult to realize the continuous stabilization treatment of polypyrrole/polyester conductive fibers, resulting in poor stability and wear resistance of the conductive layer.
Polyester fibers treated with ultrasonic-base reduction combined modification were polymerized in situ by soaking in a mixed solution of sodium dodecyl sulfate, aqueous polyurethane and pyrrole monomer and aqueous iron trichloride solution to form polypyrrole/polyurethane. /polyester composite conductive fibers improve the roughness and hydrophilicity of the fiber surface, thereby enhancing the adhesion and firmness of the conductive layer.
The continuous preparation of high-durance polypyrrole/polyurethane/polyester composite conductive fibers is achieved, ensuring the excellent mechanical properties and conductivity of the fibers, and maintaining excellent conductivity after multiple washing and friction.
Smart Images

Figure CN119061691A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional polymer material preparation, and relates to a continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fibers. Background Art
[0002] Polypyrrole is a conductive polymer material with excellent corrosion resistance. Conductive fibers developed from it can be used in sensing, electronic shielding, tissue engineering and other fields. At present, the development of polypyrrole-based conductive fibers is usually carried out by titrating the reaction solution or immersing the fibers and their assemblies in the reaction solution, such as document 1 (Printing and Dyeing, 2023, 49(07): 47-50), document 2 (Journal of Textile Research, 2022, 43(02): 110-115+139) and patent CN103643339A, but these methods are difficult to achieve continuous stabilization of conductive fibers.
[0003] To solve the above problems, some researchers have achieved the continuous preparation of polypyrrole / polyurethane composite fibers through in-situ polymerization, such as reference 3 (npj Flexible Electronics, 2022, 6(1): 42) and reference 4 (Applied Surface Science, 2023, 610: 155515). However, the studies found that the stability of the conductive layer in the prepared composite fibers was poor and the wear resistance needed to be improved.
[0004] In the prior art, the development methods of polymer conductive fibers mainly include co-spinning of conductive materials and polymers or post-finishing of polymer fibers, wherein the latter can impart conductivity to fibers without reducing the mechanical properties of the fibers. For example, Reference 5 (Journal of Textile Research, 2018, 39(02): 20-25) uses an in-situ polymerization method to prepare polyester / polyaniline composite conductive yarns, but the conductive layer is easy to fall off. In order to improve the durability of the conductive layer, Reference 6 (Journal of Textile Research, 2019, 40(08): 95-100) uses plasma to treat polyester fibers, and then prepares polypyrrole / polyester composite conductive yarns by impregnation and in-situ polymerization. However, although this method improves the firmness of polypyrrole, it has the problems of low polymerization uniformity, poor continuity, and serious waste of reaction liquid.
[0005] In summary, the prior art has not yet found a path that can achieve continuous and stable preparation of highly durable polypyrrole / polyester conductive fibers.
[0006] Therefore, it is of great significance to study a continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fibers to solve the above problems. Summary of the invention
[0007] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fibers.
[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fiber, using an in-situ polymerization device, sequentially immersing the polyester fiber after ultrasonic-alkali weight reduction modification in sodium dodecyl sulfate (SDS), a mixed solution of waterborne polyurethane (WPU) and pyrrole monomer (Py) and an aqueous solution of ferric chloride, ferric chloride as an oxidant can induce an in-situ polymerization reaction of pyrrole monomer on the surface of the polyester fiber, followed by drying treatment, the purpose of which is to prevent the fibers from being wound and stacked and adhering to each other, and the steps of immersing in two solutions and drying treatment are repeated multiple times to obtain the polypyrrole / polyurethane / polyester composite conductive fiber;
[0010] The ultrasonic-alkali weight reduction modification of polyester fiber refers to immersing the polyester fiber in a sodium hydroxide solution and performing ultrasonic treatment in a water bath.
[0011] The present invention immerses the polyester fiber modified by ultrasonic-alkali reduction in a polypyrrole in-situ polymerization reaction liquid added with waterborne polyurethane, and realizes the continuous development of highly durable polypyrrole / polyurethane / polyester composite conductive fibers in one step by relying on the viscoelasticity of polyurethane.
[0012] The roughness and hydrophilicity of the fiber surface are improved by ultrasonic-alkali weight reduction combined modification treatment, thereby improving the subsequent adhesion and firmness of conductive polypyrrole; among them, the increase in roughness provides more physical and chemical bonding points for the adhesion of conductive polypyrrole, thereby increasing the adhesion of conductive polypyrrole; the increase in hydrophilicity indicates that there are more hydrophilic groups, which can enhance the hydrogen bonding between the fiber and polypyrrole, thereby improving the firmness.
[0013] As the preferred technical solution:
[0014] According to the continuous preparation method of the polypyrrole / polyurethane / polyester composite conductive fiber as described above, the weight gain rate of the polypyrrole / polyurethane / polyester composite conductive fiber is 27-52 wt.%.
[0015] According to the continuous preparation method of the polypyrrole / polyurethane / polyester composite conductive fiber, the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is above 0.94 S / m, the conductivity retention rate is above 90% after 50 standard washings (the washing refers to the method in the GB / T3921-2008 standard), and the conductivity retention rate is above 85% after 5000 frictions (the friction refers to the method in the GB / T4802.2-2008 standard).
[0016] In the continuous preparation method of the polypyrrole / polyurethane / polyester composite conductive fiber as described above, in the mixed solution of sodium dodecyl sulfate, aqueous polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.4~0.8 mol / L, the concentration of aqueous polyurethane is 2~5 wt.%, and the concentration of pyrrole monomer is 0.5~1.5 mol / L.
[0017] In the continuous preparation method of the polypyrrole / polyurethane / polyester composite conductive fiber as described above, the concentration of the ferric chloride aqueous solution is 0.5-1.5 mol / L.
[0018] In the continuous preparation method of the polypyrrole / polyurethane / polyester composite conductive fiber as described above, the concentration of the sodium hydroxide solution is 50 g / L, and the bath ratio of the immersion is 1:50.
[0019] In the continuous preparation method of a polypyrrole / polyurethane / polyester composite conductive fiber as described above, the water bath temperature is 60°C, the ultrasonic power is 300 W, and the ultrasonic time is 3 h. These parameters are the best hydrophilicity of polyester fiber under the ultrasonic-reduction condition, and the advantage of its conductive treatment is greater. Therefore, the present invention selects these fixed parameters, but it should not be understood as a limitation to the present invention. Other parameter values can still achieve the purpose of the present invention.
[0020] Beneficial effects:
[0021] (1) The present invention improves the roughness and hydrophilicity of the fiber surface through ultrasonic-alkali weight reduction combined modification treatment, thereby improving the subsequent adhesion and firmness of conductive polypyrrole, so that it still has excellent conductivity after multiple washing and friction.
[0022] (2) The present invention immerses the polyester fiber modified by ultrasonic-alkali reduction in the reaction solution of in-situ polymerization of polypyrrole added with water-based polyurethane, thereby realizing the continuous development of highly durable polypyrrole / polyurethane / polyester composite conductive fibers in one step; in addition, the polypyrrole / polyurethane / polyester composite conductive fibers prepared by the present invention have excellent conductivity and high durability while ensuring the excellent mechanical properties of the polyester fiber.
[0023] (3) The present invention provides a reliable technical guarantee for the continuous conductive treatment and high-value utilization of hydrophobic chemical fibers, so that the prepared polypyrrole / polyurethane / polyester composite conductive fibers can be used in the fields of sensing, flexible electronics, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the process flow of preparing conductive fibers based on the in-situ polymerization method of the present invention;
[0025] Figure 2 The surface morphologies of the polyester fiber after the ultrasonic-alkali reduction combined treatment of the present invention, the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Examples 1 to 4 and Comparative Example 2, and the polypyrrole / polyester composite conductive fibers prepared in Comparative Example 1 are shown; in the figure, a is the surface morphology of the polyester fiber after the ultrasonic-alkali reduction combined treatment, b is the surface morphology of the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Example 1, c is the surface morphology of the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Example 2, d is the surface morphology of the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Example 3, e is the surface morphology of the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Example 4, f is the surface morphology of the polypyrrole / polyester composite conductive fibers prepared in Comparative Example 1, and g is the surface morphology of the polypyrrole / polyurethane / polyester composite conductive fibers prepared in Comparative Example 2;
[0026] Figure 3 The conductivity change diagram of the polypyrrole / polyurethane / polyester composite conductive fiber prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 to 2 before and after 50 standard washings; in the figure, before / after washing refers to the composite conductive fiber before / after 50 standard washings. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The testing methods of the relevant performance indicators in the following embodiments and comparative examples are as follows:
[0029] Retention rate of conductivity after 50 standard washes: first measure the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber prepared in each embodiment and use the test sample as sample A, then remove the yarn portion of the plain polyester woven fabric, and then use sample A to embed into the fabric by sewing, and then wash the fabric 50 times as a sample according to the method in GB / T 3921-2008 standard, and finally remove sample A from the fabric to measure its conductivity, and calculate the ratio between the conductivity of sample A after washing and the conductivity of sample A before washing to obtain the retention rate of conductivity after 50 standard washes.
[0030] Retention rate of conductivity after 5000 frictions: first measure the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber prepared in each embodiment and use the test sample as sample B, then remove the yarn portion of the plain polyester woven fabric, and then use sample B to embed into the fabric by sewing, and then refer to the method in GB / T 4802.2-2008 standard to rub the fabric 5000 times as a sample, and finally remove sample B from the fabric to measure its conductivity, and calculate the ratio between the conductivity of sample B after friction and the conductivity of sample B before friction to obtain the retention rate of conductivity after 5000 frictions.
[0031] Strength of polypyrrole / polyurethane / polyester composite conductive fiber: Referring to the method in GB / T 14344-2022 standard, the polypyrrole / polyurethane / polyester composite conductive fiber prepared in each embodiment and comparative example was used as a sample to measure its strength, and each sample was measured 20 times and the average value was calculated.
[0032] Example 1
[0033] A method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fibers, comprising the following steps:
[0034] (1) First, prepare a sodium hydroxide solution with a concentration of 50 g / L in a beaker, and then immerse the polyester fiber (polyester fiber specification is 110 dtex / 36f, single fiber diameter is 19.35 μm, regain is 0.45%, and breaking strength is 4.117 N) washed with detergent in the sodium hydroxide solution. Then, put the beaker into a 60°C warm water bath and use a constant temperature ultrasonic cleaning machine for ultrasonic treatment; the bath ratio of immersion is 1:50, the ultrasonic power is 300 W, and the ultrasonic time is 3 h.
[0035] The linear density of the polyester fiber after ultrasonic-alkali weight reduction modification is 95.29 dtex, the moisture regain is 1.33%, and the breaking strength is 3.41 N. The surface morphology is shown in the figure Figure 2 As shown in (a);
[0036] (2) If Figure 1As shown, the polyester fiber modified by ultrasonic-alkali weight reduction in step (1) is first immersed in a mixed solution of sodium dodecyl sulfate, water-based polyurethane (manufacturer: Shanghai MacLean Biochemical Technology Co., Ltd., solid content of 45%, CAS number NONE8071, item number W909580) and pyrrole monomer (manufacturer: Shanghai Aladdin Biochemical Technology Co., Ltd., purity of 99%, CAS number 109-97-7) through a yarn guide wheel (diameter of 1 mm, material of ceramic), and then squeezed through a rubber roller, and then passed through the hole of a yarn guide needle (the yarn guide needle is a glass tube with a hole, the hole diameter of which is 0.5 mm). Under the action of the yarn guide needle, the polyester fiber passes through the mouth of the titration funnel and makes the fine-mouthed titration funnel (diameter of 2 mm), the ferric chloride aqueous solution in the fiber is dripped drop by drop to ensure that the fiber is in full contact with the ferric chloride solution, and then passes through the rubber pressure roller again, and enters the yarn storage tank under the action of the conveying device, and finally is dried and wound onto the yarn tube; wherein, in the mixed solution of sodium dodecyl sulfate, waterborne polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.6 mol / L, the concentration of waterborne polyurethane is 5wt.%, and the concentration of pyrrole monomer is 1 mol / L; the concentration of ferric chloride aqueous solution is 1.5 mol / L; the winding speed of the yarn is 90m / h, and the conveying device is a rough leather conveyor belt;
[0037] (3) Repeat step (2) for 5 times to obtain polypyrrole / polyurethane / polyester composite conductive fiber.
[0038] The weight gain rate of the final polypyrrole / polyurethane / polyester composite conductive fiber is 51.76 wt.%, and its surface morphology is shown in the figure Figure 2 As shown in (b); the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 1 S / m, the linear density is 144.61 dtex, and the conductivity retention rate after 50 standard washes is 95% (the change in conductivity before and after 50 standard washes is shown in Figure 3 As shown in the figure), after 5000 frictions, the conductivity retention rate is 92%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 4.07 N.
[0039] Comparative Example 1
[0040] A continuous preparation method of polypyrrole / polyester composite conductive fiber is basically the same as Example 1, except that the mixed solution in step (2) is obtained by mixing sodium dodecyl sulfate and pyrrole monomer, and no water-based polyurethane is used.
[0041] The weight gain of the final polypyrrole / polyester composite conductive fiber is 15.42 wt.%, and its surface morphology is shown in the figure below: Figure 2As shown in (f), the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 0.91 S / m, the linear density is 109.98 dtex, and the conductivity retention rate after 50 standard washes is 58.2% (the change in conductivity before and after 50 standard washes is shown in Figure 3 As shown in the figure), after 5000 frictions, the conductivity retention rate is 67%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 3.61 N.
[0042] By comparing Comparative Example 1 with Example 1, it can be seen that the weight gain rate of the polypyrrole / polyester composite conductive fiber prepared in Comparative Example 1 is significantly reduced, and the conductivity retention rate after washing and friction is significantly reduced. This is because the interface effect between the polypyrrole conductive layer and the polyester fiber is weak. During multiple polymerization processes, the polypyrrole that has been polymerized to the fiber surface is very easy to detach from the fiber surface, and it is also easy to detach from the fiber surface during washing and friction.
[0043] Comparative Example 2
[0044] A continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fiber is basically the same as Example 1, except that in step (1), the polyester fiber is simply washed with a detergent, dried at 60° C. for 10 h, and equilibrated under standard conditions for 24 h.
[0045] The weight gain of the final polypyrrole / polyurethane / polyester composite conductive fiber is 30.85 wt.%, and its surface morphology is shown in the figure below: Figure 2 As shown in (g); the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 0.9 S / m, the linear density is 143.94 dtex, and the conductivity retention rate after 50 standard washings is 83.3% (the change in conductivity before and after 50 standard washings is shown in Figure 3 As shown in the figure), after 5000 frictions, the conductivity retention rate is 78%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 4.21 N.
[0046] By comparing Comparative Example 2 with Example 1, it can be seen that the strength of the polypyrrole / polyurethane / polyester composite conductive fiber prepared in Comparative Example 2 is improved, the weight gain rate is reduced, and the conductivity retention rate after washing and friction is significantly reduced. This is because although the initial strength of the polyester fiber that has not been subjected to ultrasonic-alkali weight reduction treatment remains unchanged, the conductive layer will also increase the strength of the composite fiber, but the surface of the initial polyester fiber will also be relatively smooth, resulting in the subsequent adhesion amount and firmness of the conductive polypyrrole. After the polyester fiber of Example 1 is subjected to ultrasonic-alkali weight reduction treatment, the moisture regain, surface roughness and hydrophilicity of the polyester fiber are improved, thereby improving the adhesion amount and adhesion firmness of the conductive polypyrrole.
[0047] Example 2
[0048] A method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fibers, comprising the following steps:
[0049] (1) First, prepare a sodium hydroxide solution with a concentration of 50 g / L in a beaker, and then immerse the polyester fiber (polyester fiber specification is 110 dtex / 36f, single fiber diameter is 19.35 μm, moisture regain is 0.45%, and breaking strength is 4.117N) washed with detergent in the sodium hydroxide solution. Then, put the beaker into a 60 ℃ warm water bath and use a constant temperature ultrasonic cleaning machine for ultrasonic treatment; the bath ratio of immersion is 1:50, the ultrasonic power is 300 W, and the ultrasonic time is 3 h.
[0050] The linear density of the polyester fiber after ultrasonic-alkali weight reduction modification was 95.29 dtex, the moisture regain was 1.33%, and the breaking strength was 3.41 N;
[0051] (2) If Figure 1 As shown, the polyester fiber modified by ultrasonic-alkali weight reduction in step (1) is first immersed in a mixed solution of sodium dodecyl sulfate, water-based polyurethane (manufacturer: Shanghai MacLean Biochemical Technology Co., Ltd., solid content of 45%, CAS number NONE8071, item number W909580) and pyrrole monomer (manufacturer: Shanghai Aladdin Biochemical Technology Co., Ltd., purity of 99%, CAS number 109-97-7) through a yarn guide wheel (diameter 2 mm, material of glass), and then squeezed through a rubber roller, and then passed through the hole of a yarn guide needle (the yarn guide needle is a metal tube with a hole, the hole diameter of which is 1 mm). Under the action of the yarn guide needle, the polyester fiber passes through the mouth of the titration funnel and makes the fine-mouthed titration funnel (diameter 3 mm), the ferric chloride aqueous solution in the fiber is dripped drop by drop to ensure that the fiber is in full contact with the ferric chloride solution, and then passes through the rubber pressure roller again, and enters the yarn storage tank under the action of the conveying device, and finally is dried and wound onto the yarn tube; wherein, in the mixed solution of sodium dodecyl sulfate, waterborne polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.4 mol / L, the concentration of waterborne polyurethane is 4wt.%, and the concentration of pyrrole monomer is 0.5 mol / L; the concentration of ferric chloride aqueous solution is 0.5 mol / L; the winding speed of the yarn is 30 m / h, and the conveying device is a rough leather conveyor belt;
[0052] (3) Repeat step (2) for 5 times to obtain polypyrrole / polyurethane / polyester composite conductive fiber.
[0053] The weight gain of the final polypyrrole / polyurethane / polyester composite conductive fiber is 27.93 wt.%, and its surface morphology is shown in the figure. Figure 2As shown in (c), the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 0.94 S / m, the linear density is 121.9 dtex, and the conductivity retention rate after 50 standard washes is 92.6% (the change in conductivity before and after 50 standard washes is shown in Figure 3 As shown in the figure), the conductivity retention rate after 5000 frictions is 88%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 3.75 N.
[0054] Example 3
[0055] A method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fibers, comprising the following steps:
[0056] (1) First, prepare a sodium hydroxide solution with a concentration of 50 g / L in a beaker, and then immerse the polyester fiber (polyester fiber specification is 110 dtex / 36f, single fiber diameter is 19.35 μm, regain is 0.45%, and breaking strength is 4.117 N) washed with detergent in the sodium hydroxide solution. Then, place the beaker in a 60 ℃ warm water bath and use a constant temperature ultrasonic cleaning machine for ultrasonic treatment; the bath ratio of immersion is 1:50, the ultrasonic power is 300 W, and the ultrasonic time is 3 h.
[0057] The linear density of the polyester fiber after ultrasonic-alkali weight reduction modification was 95.29 dtex, the moisture regain was 1.33%, and the breaking strength was 3.41 N;
[0058] (2) If Figure 1As shown, the polyester fiber modified by ultrasonic-alkali weight reduction in step (1) is first immersed in a mixed solution of sodium dodecyl sulfate, water-based polyurethane (manufacturer: Shanghai MacLean Biochemical Technology Co., Ltd., solid content of 45%, CAS number NONE8071, item number W909580) and pyrrole monomer (manufacturer: Shanghai Aladdin Biochemical Technology Co., Ltd., purity of 99%, CAS number 109-97-7) through a yarn guide wheel (diameter 3 mm, material of glass), and then squeezed through a rubber roller, and then passed through the hole of the yarn guide needle (the yarn guide needle is a ceramic tube with a hole, the hole diameter is 2 mm). Under the action of the yarn guide needle, the polyester fiber passes through the mouth of the titration funnel and makes the fine-mouthed titration funnel (diameter 4 mm), the ferric chloride aqueous solution in the fiber is dripped drop by drop to ensure that the fiber is fully in contact with the ferric chloride solution, and then passes through the rubber pressure roller again, and enters the yarn storage tank under the action of the conveying device, and finally is dried and wound onto the yarn tube; wherein, in the mixed solution of sodium dodecyl sulfate, waterborne polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.8 mol / L, the concentration of waterborne polyurethane is 3wt.%, and the concentration of pyrrole monomer is 1.5 mol / L; the concentration of ferric chloride aqueous solution is 1 mol / L; the winding speed of the yarn is 60m / h, and the conveying device is a rough leather conveyor belt;
[0059] (3) Repeat step (2) for 5 times to obtain polypyrrole / polyurethane / polyester composite conductive fiber.
[0060] The weight gain rate of the final polypyrrole / polyurethane / polyester composite conductive fiber is 44.46 wt.%, and its surface morphology is shown in the figure Figure 2 As shown in (d), the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 0.96 S / m, the linear density is 137.61 dtex, and the conductivity retention rate after 50 standard washes is 91.7% (the change in conductivity before and after 50 standard washes is shown in Figure 3 As shown in the figure), the conductivity retention rate after 5000 frictions is 87%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 3.91 N.
[0061] Example 4
[0062] A method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fibers, comprising the following steps:
[0063] (1) First, prepare a sodium hydroxide solution with a concentration of 50 g / L in a beaker, and then immerse the polyester fiber (polyester fiber specification is 110 dtex / 36f, single fiber diameter is 19.35 μm, regain is 0.45%, and breaking strength is 4.117N) washed with detergent in the sodium hydroxide solution. Then, put the beaker into a 60 ℃ warm water bath and use a constant temperature ultrasonic cleaning machine for ultrasonic treatment; the bath ratio of immersion is 1:50, the ultrasonic power is 300 W, and the ultrasonic time is 3 h;
[0064] The linear density of the polyester fiber after ultrasonic-alkali weight reduction modification was 95.29 dtex, the moisture regain was 1.33%, and the breaking strength was 3.41 N;
[0065] (2) If Figure 1 As shown, the polyester fiber modified by ultrasonic-alkali weight reduction in step (1) is first immersed in a mixed solution of sodium dodecyl sulfate, water-based polyurethane (manufacturer: Shanghai MacLean Biochemical Technology Co., Ltd., solid content of 45%, CAS number NONE8071, item number W909580) and pyrrole monomer (manufacturer: Shanghai Aladdin Biochemical Technology Co., Ltd., purity of 99%, CAS number 109-97-7) through a yarn guide wheel (diameter 4 mm, material of metal), and then squeezed through a rubber roller, and then passed through the hole of the yarn guide needle (the yarn guide needle is a metal tube with a hole, the hole diameter of 1 mm). Under the action of the yarn guide needle, the polyester fiber passes through the mouth of the titration funnel and makes the fine-mouthed titration funnel (diameter 3 mm), the ferric chloride aqueous solution in the fiber is dripped drop by drop to ensure that the fiber is in full contact with the ferric chloride solution, and then passes through the rubber pressure roller again, and enters the yarn storage tank under the action of the conveying device, and finally is dried and wound onto the yarn tube; wherein, in the mixed solution of sodium dodecyl sulfate, waterborne polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.6 mol / L, the concentration of waterborne polyurethane is 2wt.%, and the concentration of pyrrole monomer is 1 mol / L; the concentration of ferric chloride aqueous solution is 1.5 mol / L; the winding speed of the yarn is 120 m / h, and the conveying device is a rough leather conveyor belt;
[0066] (3) Repeating the process of step (2) for 5 times, a polypyrrole / polyurethane / polyester composite conductive fiber is obtained; wherein the polyester fiber from the second cycle of repeated immersion in the two solutions is the polyester fiber wound onto the yarn tube after the previous immersion.
[0067] The weight gain of the final polypyrrole / polyurethane / polyester composite conductive fiber is 38.39 wt.%, and its surface morphology is shown in the figure below: Figure 2As shown in (e); the conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is 0.95 S / m, the linear density is 131.83 dtex, and the conductivity retention rate after 50 standard washes is 90.5% (the change in conductivity before and after 50 standard washes is shown in Figure 3 As shown in the figure), after 5000 frictions, the conductivity retention rate is 85%; the strength of the polypyrrole / polyurethane / polyester composite conductive fiber is 3.87 N.
Claims
1. A continuous preparation method of polypyrrole / polyurethane / polyester composite conductive fiber, characterized in that: Using an in-situ polymerization device, the polyester fiber modified by ultrasonic-alkali weight reduction is sequentially immersed in sodium dodecyl sulfate, a mixed solution of waterborne polyurethane and pyrrole monomer, and an aqueous solution of ferric chloride, and then dried. After multiple cycles, a polypyrrole / polyurethane / polyester composite conductive fiber is obtained. The ultrasonic-alkali weight reduction modification of polyester fiber refers to immersing the polyester fiber in a sodium hydroxide solution and performing ultrasonic treatment in a water bath.
2. The method for continuously preparing a polypyrrole / polyurethane / polyester composite conductive fiber according to claim 1, characterized in that: The weight gain rate of polypyrrole / polyurethane / polyester composite conductive fibers is 27~52 wt.%.
3. The method for continuously preparing a polypyrrole / polyurethane / polyester composite conductive fiber according to claim 2, characterized in that: The conductivity of the polypyrrole / polyurethane / polyester composite conductive fiber is above 0.94 S / m, the conductivity retention rate is above 90% after 50 standard washings, and the conductivity retention rate is above 85% after 5000 frictions.
4. The method for continuously preparing a polypyrrole / polyurethane / polyester composite conductive fiber according to claim 1, characterized in that: In the mixed solution of sodium dodecyl sulfate, waterborne polyurethane and pyrrole monomer, the concentration of sodium dodecyl sulfate is 0.4-0.8 mol / L, the concentration of waterborne polyurethane is 2-5 wt.%, and the concentration of pyrrole monomer is 0.5-1.5 mol / L.
5. The method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fiber according to claim 4, characterized in that: The concentration of ferric chloride aqueous solution is 0.5~1.5 mol / L.
6. The method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fiber according to claim 1, characterized in that: The concentration of the sodium hydroxide solution was 50 g / L, and the bath ratio of the immersion was 1:
50.
7. The method for continuously preparing polypyrrole / polyurethane / polyester composite conductive fiber according to claim 1, characterized in that: The water bath temperature was 60 °C, the ultrasonic power was 300 W, and the ultrasonic time was 3 h.
Citation Information
Patent Citations
Conductive fabric prepared by dip dyeing technology and preparation method and application of conductive fabric
CN102926207A
Method for preparing high-durability polyaniline conductive yarns
CN109162099A
Environment-friendly anti-corrosion luggage cloth fabric and manufacturing method thereof
CN114635278A
Conductive fiber and conductive fabric and preparation method and application thereof
CN115679705A
Antistatic coating composition, preparation method thereof and antistatic textile fabric
CN118360809A
Cited By
Antibacterial fabric and preparation process thereof
CN119682342A