Preparation method of corn straw nanocellulose

A combined chemical and mechanical process for preparing corn straw nanocellulose addresses inefficiencies and environmental issues in existing methods, achieving high yield and quality nanocellulose with reduced costs and pollution.

CN119061716AInactive Publication Date: 2024-12-03HEBEI AGRICULTURAL UNIV. +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202487.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing nanocellulose preparation methods are inefficient, costly, environmentally harmful, and difficult to scale due to high energy consumption, chemical pollution, and long production cycles.

Method used

A method combining chemical and mechanical processes to prepare corn straw nanocellulose, involving steps like ultrasonic cleaning, acid washing, alkali boiling, bleaching, and TEMPO oxidation, using fewer chemicals and optimizing conditions for high yield and quality.

Benefits of technology

The method reduces production costs, environmental impact, and improves efficiency while maintaining high-quality nanocellulose properties, achieving yields up to 60.33% with uniform nanoscale fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061716A_ABST
    Figure CN119061716A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of green biomass refining, in particular to a preparation method of corn straw nanocellulose, which comprises the following steps: crushing and sieving corn straw, repeatedly washing and filtering corn straw powder with ultrapure water under ultrasonic conditions, and drying for later use; mixing the dried powder with ultrapure water, carrying out acid pickling treatment, and then filtering, washing and drying to obtain an acid pickling product; carrying out soda boiling treatment on the acid pickling product, and then filtering, washing and drying to obtain a soda boiling product; bleaching the soda boiling product, and then filtering, washing and drying to obtain a bleached product; under the condition of room temperature, performing TEMPO oxidation on the bleaching product, and then filtering, washing and drying to obtain an oxidation product; and carrying out ultrasonic treatment on the oxidation product by using an ultrasonic cell disruptor to obtain a nanocellulose suspension, and carrying out vacuum freeze drying for 48 hours to obtain the nanocellulose. Compared with some traditional chemical treatment methods, the method has the advantage that the pollution to the environment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of green biomass refining, and in particular to a method for preparing corn straw nanocellulose. Background Art

[0002] Nanocellulose, as a new type of cellulose material, has a wide range of applications, including biomedicine, textiles, food industry, environmental protection, and paper manufacturing. In the biomedical field, nanocellulose can be used to prepare various biodegradable medical products due to its high specific surface area and good biocompatibility. It can also be used as a carrier for drug delivery systems to effectively load drugs and achieve controlled release of drugs, thereby improving the bioavailability and efficacy of drugs. In the field of textiles, nanocellulose can be used to prepare high-performance textiles such as sportswear, waterproof coatings, and antibacterial textiles. In the food industry, nanocellulose can be used as a food additive to improve the texture, taste, and stability of food. At the same time, it can also be used in the preparation of food packaging materials because it has good barrier properties and can effectively extend the shelf life of food. In the field of environmental protection, nanocellulose can be used to prepare nanocellulose membranes for filtration and separation in water treatment processes to effectively remove suspended solids and microorganisms in water. In paper manufacturing, it can improve the hygroscopicity and water resistance of paper, improve the optical properties of paper, reduce the amount of pulp used, and reduce the pressure on forest resources. Therefore, the method of preparing nanocellulose has also become one of the research hotspots.

[0003] With the continuous development of nanotechnology and the improvement of application requirements, the existing nanocellulose preparation method has been difficult to meet the urgent needs of the market. Therefore, it is of great theoretical and practical significance to develop a new nanocellulose preparation method that can not only maintain the excellent properties of nanocellulose, but also improve production efficiency, reduce costs and reduce environmental pollution. Traditional nanocellulose preparation methods mainly include mechanical methods, chemical methods and biological methods. Mechanical methods such as high-pressure homogenization methods can obtain nanocellulose of a certain particle size, but the equipment cost is high, the energy consumption is large, and the natural structure of cellulose may be destroyed. Chemical methods such as acid hydrolysis methods have high production efficiency, but the use of strong acids will cause environmental pollution and may produce harmful by-products. Biological methods such as microbial fermentation methods are environmentally friendly, but they have long cycles and low yields, which are difficult to meet the needs of large-scale production. Summary of the invention

[0004] In order to overcome the deficiencies and shortcomings of the prior art, the object of the present invention is to provide a method for preparing nanofibers, which combines chemical and mechanical methods to improve the yield, reduce environmental pollution, and improve the performance of nanocellulose.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing corn straw nanocellulose comprises the following steps:

[0007] Step 1, after the corn stalks are crushed and sieved, the corn stalk powder is repeatedly washed and filtered with ultrapure water under ultrasonic conditions, and dried for later use;

[0008] Step 2, mixing the powder dried in step 1 with ultrapure water, performing an acid wash treatment, and then filtering, washing, and drying to obtain an acid wash product;

[0009] Step 3, subjecting the acid-washed product obtained in step 2 to alkali boiling treatment, and then filtering, washing, and drying to obtain an alkali boiling product;

[0010] Step 4, bleaching the alkali-boiling product obtained in step 3, and then filtering, washing and drying to obtain a bleached product;

[0011] Step 5, at room temperature, subjecting the bleaching product obtained by the pretreatment in step 4 to TEMPO oxidation, and then filtering, washing, and drying to obtain an oxidation product;

[0012] Step 6: The oxidation product obtained in step 5 is subjected to ultrasonic treatment with an ultrasonic cell crusher to obtain a nanocellulose suspension, and then vacuum freeze-dried for 48 hours to obtain nanocellulose.

[0013] Furthermore, in step 1, the mesh size of the sieve after crushing is 40 to 60 meshes.

[0014] Furthermore, in step 2, the pickling treatment is hydrochloric acid treatment, wherein the material-liquid ratio is 1: (10-15) g / ml, the solution pH is adjusted to 1.3-1.7, the hydrochloric acid content in the solution is 0.4%-2%, the water bath temperature is 70-75°C, and the magnetic stirring time is 2-3h.

[0015] Furthermore, in step 3, the alkali boiling treatment is a sodium hydroxide treatment, wherein the solid-liquid ratio is 1: (10-15) g / ml, the solution pH is adjusted to 12.4-12.7, the sodium hydroxide content in the solution is 3%-5%, the water bath temperature is 75-80°C, and the magnetic stirring time is 4-6h.

[0016] Furthermore, in step 4, the bleaching treatment is a sodium hypochlorite treatment, wherein the solid-liquid ratio is 1:(10-15) g / ml, the sodium hypochlorite content in the solution is 0.5%-1%, the reaction is carried out at room temperature, and the magnetic stirring time is 8-12 hours.

[0017] Furthermore, in step 5, a TEMPO / NaBr / NaClO oxidation method is used, wherein the material-liquid ratio is 1:(80-120) g / ml, the mass ratio of cellulose to NaBr in the solution is 1:(0.1-0.2), the mass ratio of cellulose to TEMPO in the solution is 1:(0.01-0.02), a sodium hypochlorite solution with an effective chlorine content of 10% is added to make its mass molar concentration 5-30 mmol / g, 0.5 mol / L of sodium hydroxide is added during the reaction to adjust the pH of the solution to 9.8-10.2, and the pH is measured every half an hour to keep the pH constant.

[0018] Furthermore, in step 6, the material-liquid ratio is 1: (80-120) g / ml, the rated power is 400w, and the time is 20-30min.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention uses corn cobs as raw materials, which are agricultural and sideline products with a wide range of sources and low prices, thus greatly reducing production costs.

[0021] (2) Compared with some traditional chemical treatment methods, the present invention uses relatively fewer chemical reagents and can be recovered and reused through subsequent treatment, thereby reducing pollution to the environment.

[0022] (3) The entire preparation process of the present invention includes steps such as ultrasonic cleaning, pickling, alkali boiling, bleaching and oxidation treatment. These steps are relatively simple, do not require special instruments, and are easy to operate and control.

[0023] (4) The nanocellulose prepared by the present invention has a high yield. By precisely controlling the oxidation and ultrasonic treatment conditions, high-quality nanocellulose with excellent physical and chemical properties is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a flow chart of preparing nanocellulose according to the present invention.

[0025] Figure 2 Figure 1 is the FTIR spectra of corn stover (CS) and corn stover nanocellulose (CNF); the characteristic peak at 3340 cm-1 is due to -OH stretching vibration. The stretching at 1735 cm-1, mainly from the carbonyl group in hemicellulose, shows a relatively weak signal in the treated sample compared to corn stover. The relatively low band at 1509 cm-1 in the treated sample is attributed to the aromatic skeleton vibration of lignin. The vibration of the characteristic peaks at 1160 and 897 cm-1 means that the cellulose crystal structure is still retained after ultrasound, preserving its chemical characteristics.

[0026] Figure 3 This is a TEM image of corn straw nanocellulose (CNF); from the TEM image of CNF, it can be seen that the prepared cellulose has reached the nanoscale, with a length in the range of 200-1000nm and a width in the range of 5-20nm, with a very uniform size distribution and good dispersibility.

[0027] Figure 4 is a SEM image of corn stover (CS); untreated corn stover appears smooth, intact, and non-porous.

[0028] Figure 5 This is a SEM image of corn straw nanocellulose (CNF); after a series of treatments, the surface structure of cellulose is destroyed and appears loose, indicating that lignin and hemicellulose are removed.

[0029] Figure 6 is a TG image of corn stover nanocellulose. The initial weight loss of CNF occurs at 50-200°C, mainly due to the evaporation of bound water molecules. The second significant weight loss between 200 and 300°C is due to the degradation of hemicellulose and the decomposition of glycosidic bonds of cellulose. From 300°C to 600°C, cellulose further degrades. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A method for preparing corn straw nanocellulose comprises the following steps:

[0033] (1) Ultrasonic cleaning: Under ultrasonic conditions, the corn stalk powder is repeatedly washed and filtered with ultrapure water, and then dried for later use.

[0034] (2) Acid washing: dried corn stalk powder was mixed with ultrapure water at a solid-liquid ratio of 1:10 g / ml, hydrochloric acid was added to adjust the pH value (1.5±0.2), magnetic stirring was performed at 70°C for 2 h, and after cooling, the mixture was filtered and washed until the pH value of the filtrate was neutral, and then dried for later use.

[0035] (3) Alkali cooking: The acid-washed corn stalk powder is mixed with ultrapure water at a material-liquid ratio of 1:10 g / ml, the NaOH content in the solution is 4%, and the alkali cooking is carried out in a constant temperature water bath at 80°C for 4 hours. After cooling, the precipitate is filtered and rinsed until the pH is neutral. Dry and set aside.

[0036] (4) Bleaching: Mix the raw material obtained in step (3) with ultrapure water at a material-liquid ratio of 1:10 g / ml, add sodium hypochlorite solution to make the sodium hypochlorite content in the solution 0.5%, stir magnetically at room temperature until complete bleaching, filter out the precipitate, rinse the precipitate with ultrapure water until the pH value is neutral, and dry and store for later use.

[0037] (5) Prepare corncob nanocellulose fibers by TEMPO / NaBr / NaClO oxidation method. At room temperature, 1.00 g of the above-mentioned pretreated corncob fibers were dispersed in 100 ml of ultrapure water. After sufficient stirring and dispersion, NaBr (0.16 g) and TEMPO (0.016 g) were added under magnetic stirring. After dissolution, sodium hypochlorite solution with an effective chlorine content of 10% was added to make its mass molar concentration 5 mmol / g, and oxidation was started. During the reaction, the pH value of the suspension was adjusted to (10±0.2) by adding 0.5 mol / L NaOH solution. The pH value was measured every half an hour until it was almost unchanged, and the reaction was terminated. The corncob fibers were filtered and washed until the pH value was neutral. Put it at 4°C for use.

[0038] (6) 1.00 g of oxidized corncob fiber was dispersed in 100 ml of ultrapure water and ultrasonically treated with an ultrasonic cell crusher at a rated power of 400 W for 20 min. A corncob nanocellulose suspension was obtained, and corncob nanocellulose was obtained after vacuum freeze drying for 48 h. The nanocellulose yield was 60.33%.

[0039] Example 2

[0040] A method for preparing corn straw nanocellulose comprises the following steps:

[0041] (1) Ultrasonic cleaning: Under ultrasonic conditions, the corn stalk powder is repeatedly washed and filtered with ultrapure water, and then dried for later use.

[0042] (2) Acid washing: The dried corn stalk powder was mixed with ultrapure water at a solid-liquid ratio of 1:10 g / ml, and hydrochloric acid was added to adjust the pH value (1.5±0.2). The mixture was stirred magnetically at 75°C for 2 h. After cooling, the mixture was filtered and washed until the pH value of the filtrate was neutral, and then dried for later use.

[0043] (3) Alkali cooking: The acid-washed corn stalk powder is mixed with ultrapure water at a material-liquid ratio of 1:10 g / ml, the NaOH content in the solution is 4%, and the alkali cooking is carried out in a constant temperature water bath at 80°C for 4 hours. After cooling, the precipitate is filtered and rinsed until the pH is neutral. Dry and set aside.

[0044] (4) Bleaching: Mix the raw material obtained in step (3) with ultrapure water at a material-liquid ratio of 1:10 g / ml, add sodium hypochlorite solution to make the sodium hypochlorite content in the solution 0.5%, stir magnetically at room temperature until complete bleaching, filter out the precipitate, rinse the precipitate with ultrapure water until the pH value is neutral, and dry and store for later use.

[0045] (5) Prepare corncob nanocellulose fibers by TEMPO / NaBr / NaClO oxidation method. At room temperature, 1.00 g of the above-mentioned pretreated corncob fibers were dispersed in 100 ml of ultrapure water. After sufficient stirring and dispersion, NaBr (0.16 g) and TEMPO (0.016 g) were added under magnetic stirring. After dissolution, sodium hypochlorite solution with an effective chlorine content of 10% was added to make its mass molar concentration 5 mmol / g, and oxidation was started. During the reaction, the pH value of the suspension was adjusted to (10±0.2) by adding 0.5 mol / L NaOH solution. The pH value was measured every half an hour until it was almost unchanged, and the reaction was terminated. The corncob fibers were filtered and washed until the pH value was neutral. Put it at 4°C for use.

[0046] (6) 1.00 g of oxidized corncob fiber was dispersed in 100 ml of ultrapure water and ultrasonically treated with an ultrasonic cell crusher at a rated power of 400 W for 30 min. A corncob nanocellulose suspension was obtained, and corncob nanocellulose was obtained after vacuum freeze drying for 48 h. The nanocellulose yield was 49.58%.

[0047] Example 3

[0048] A method for preparing corn straw nanocellulose comprises the following steps:

[0049] (1) Ultrasonic cleaning: Under ultrasonic conditions, the corn stalk powder is repeatedly washed and filtered with ultrapure water, and then dried for later use.

[0050] (2) Acid washing: The dried corn stalk powder was mixed with ultrapure water at a solid-liquid ratio of 1:10 g / ml, and hydrochloric acid was added to adjust the pH value (1.5±0.2). The mixture was stirred magnetically at 75°C for 2 h. After cooling, the mixture was filtered and washed until the pH value of the filtrate was neutral, and then dried for later use.

[0051] (3) Alkali cooking: The acid-washed corn stalk powder is mixed with ultrapure water at a material-liquid ratio of 1:10 g / ml, the NaOH content in the solution is 4%, and the alkali cooking is carried out in a constant temperature water bath at 80°C for 4 hours. After cooling, the precipitate is filtered and rinsed until the pH is neutral. Dry and set aside.

[0052] (4) Bleaching: Mix the raw material obtained in step (3) with ultrapure water at a material-liquid ratio of 1:10 g / ml, add sodium hypochlorite solution to make the sodium hypochlorite content in the solution 0.5%, stir magnetically at room temperature until complete bleaching, filter out the precipitate, rinse the precipitate with ultrapure water until the pH value is neutral, and dry and store for later use.

[0053] (5) Prepare corncob nanocellulose fibers by TEMPO / NaBr / NaClO oxidation method. At room temperature, 1.00 g of the above-mentioned pretreated corncob fibers were dispersed in 100 ml of ultrapure water. After sufficient stirring and dispersion, NaBr (0.16 g) and TEMPO (0.016 g) were added under magnetic stirring. After dissolution, sodium hypochlorite solution with an effective chlorine content of 10% was added to make its mass molar concentration 15 mmol / g, and oxidation was started. During the reaction, the pH value of the suspension was adjusted to (10±0.2) by adding 0.5 mol / L NaOH solution. The pH value was measured every half an hour until it was almost unchanged, and the reaction was terminated. The corncob fibers were filtered and washed until the pH value was neutral. Put it at 4°C for use.

[0054] (6) 1.00 g of oxidized corncob fiber was dispersed in 100 ml of ultrapure water and ultrasonically treated with an ultrasonic cell crusher at a rated power of 400 W for 20 min. A corncob nanocellulose suspension was obtained, and corncob nanocellulose was obtained after vacuum freeze drying for 48 h. The yield of nanocellulose was 53.74%.

[0055] Example 4

[0056] A method for preparing corn straw nanocellulose comprises the following steps:

[0057] (1) Ultrasonic cleaning: Under ultrasonic conditions, the corn stalk powder is repeatedly washed and filtered with ultrapure water, and then dried for later use.

[0058] (2) Acid washing: The dried corn stalk powder was mixed with ultrapure water at a solid-liquid ratio of 1:10 g / ml, and hydrochloric acid was added to adjust the pH value (1.5±0.2). The mixture was stirred magnetically at 75°C for 2 h. After cooling, the mixture was filtered and washed until the pH value of the filtrate was neutral, and then dried for later use.

[0059] (3) Alkali cooking: The acid-washed corn stalk powder is mixed with ultrapure water at a material-liquid ratio of 1:10 g / ml, the NaOH content in the solution is 4%, and the alkali cooking is carried out in a constant temperature water bath at 80°C for 4 hours. After cooling, the precipitate is filtered and rinsed until the pH is neutral. Dry and set aside.

[0060] (4) Bleaching: Mix the raw material obtained in step (3) with ultrapure water at a material-liquid ratio of 1:10 g / ml, add sodium hypochlorite solution to make the sodium hypochlorite content in the solution 0.5%, stir magnetically at room temperature until complete bleaching, filter out the precipitate, rinse the precipitate with ultrapure water until the pH value is neutral, and dry and store for later use.

[0061] (5) Prepare corncob nanocellulose fibers by TEMPO / NaBr / NaClO oxidation method. At room temperature, 1.00 g of the above-mentioned pretreated corncob fibers were dispersed in 100 ml of ultrapure water. After sufficient stirring and dispersion, NaBr (0.16 g) and TEMPO (0.016 g) were added under magnetic stirring. After dissolution, sodium hypochlorite solution with an effective chlorine content of 10% was added to make its mass molar concentration 25 mmol / g, and oxidation was started. During the reaction, the pH value of the suspension was adjusted to (10±0.2) by adding 0.5 mol / L NaOH solution. The pH value was measured every half an hour until it was almost unchanged, and the reaction was terminated. The corncob fibers were filtered and washed until the pH value was neutral. Put it at 4°C for use.

[0062] (6) 1.00 g of oxidized corncob fiber was dispersed in 100 ml of ultrapure water and ultrasonically treated with an ultrasonic cell crusher at a rated power of 400 W for 20 min. A corncob nanocellulose suspension was obtained, and corncob nanocellulose was obtained after vacuum freeze drying for 48 h. The yield of nanofibers was 49.54%.

[0063] From the yield of nanocellulose obtained in Comparative Examples 1-4, it can be seen that when TEMPO oxidation is used, the mass molar concentration of sodium hypochlorite in the solution is 5 mmol / g, and the ultrasonic crushing time is 20 min, the yield of nanocellulose obtained is the highest.

[0064] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. A method for preparing corn straw nanocellulose, comprising the following steps: Step 1: After the corn stalks are crushed and sieved, the corn stalk powder is repeatedly washed and filtered with ultrapure water under ultrasonic conditions, and dried for later use; Step 2: mixing the powder dried in step 1 with ultrapure water, performing an acid wash treatment, and then filtering, washing, and drying to obtain an acid wash product; Step 3, alkali-boiling the acid-washed product obtained in step 2, and then filtering, washing, and drying to obtain an alkali-boiling product; Step 4: bleaching the alkali-boiling product obtained in step 3, and then filtering, washing, and drying to obtain a bleached product; Step 5: Under room temperature, the bleached product obtained by the pretreatment in Step 4 is subjected to TEMPO oxidation, and then filtered, washed, and dried to obtain an oxidized product; Step 6: The oxidation product obtained in step 5 is ultrasonically treated with an ultrasonic cell disruptor to obtain a nanocellulose suspension, which is then freeze-dried in vacuum for 48 hours to obtain nanocellulose.

2. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 1, the mesh size of the sieve after crushing is 40 to 60 meshes.

3. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 2, the pickling treatment is hydrochloric acid treatment, wherein the material-liquid ratio is 1:(10-15) g / ml, the pH of the solution is adjusted to 1.3-1.7, the hydrochloric acid content in the solution is 0.4%-2%, the water bath temperature is 70-75°C, and the magnetic stirring time is 2-3h.

4. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 3, the alkali boiling treatment is a sodium hydroxide treatment, wherein the material-liquid ratio is 1:(10-15) g / ml, the sodium hydroxide content in the solution is 3%-5%, the solution pH is adjusted to 12.4-12.7, the water bath temperature is 75-80° C., and the magnetic stirring time is 4-6 hours.

5. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 4, the bleaching treatment is sodium hypochlorite treatment, wherein the material-liquid ratio is 1:(10-15) g / ml, the sodium hypochlorite content in the solution is 0.5%-1%, the reaction is carried out at room temperature, and the magnetic stirring time is 8-12 hours.

6. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 5, a TEMPO / NaBr / NaClO oxidation method is used, wherein the material-liquid ratio is 1:(80-120) g / ml, the mass ratio of cellulose to NaBr in the solution is 1:(0.1-0.2), the mass ratio of cellulose to TEMPO in the solution is 1:(0.01-0.02), and a sodium hypochlorite solution with an available chlorine content of 10% is added to have a mass molar concentration of 5-30 mmol / g. During the reaction, 0.5 mol / L of sodium hydroxide is added to adjust the pH of the solution to 9.8-10.2, and the pH is measured every half hour to keep it constant.

7. The method for preparing corn straw nanocellulose according to claim 1, wherein: In step 6, the material-liquid ratio is 1: (80-120) g / ml, the rated power is 400 W, and the time is 20-30 min.