Preparation method of aramid fiber mica paper

Through the combination of CF4 plasma modified meta-aramid fiber and mica, the adhesive roller problem of aramid mica paper in the high-temperature hot pressing process is solved, and its electrical and mechanical properties are improved. It is suitable for high corona resistance and mechanical Insulation material for wind turbines required for strength.

CN119061724AActive Publication Date: 2024-12-03ZHUZHOU TIMES FIBER PIONEER MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411534732.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-12-03
Estimated Expiration
2044-10-31

AI Technical Summary

Technical Problem

Existing aramid mica paper is prone to sticking to rollers in the high-temperature hot pressing process, and its electrical and mechanical properties are insufficient, making it difficult to meet the corona and mechanical strength requirements of wind turbines.

Method used

By modifying the meta-aramid deposition fibers in CF4 plasma, combining meta-aramid chopped fibers and mica, aramid mica paper with high corona resistance, electrical strength and mechanical properties was prepared by releasing and hot pressing processes. .

Benefits of technology

It significantly improves the high temperature resistance, electrical and mechanical strength of aramid mica paper, reduces corona and local discharge phenomena, and extends the service life of wind turbines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an aramid mica paper preparation method, which comprises: (1) carrying out CF4 plasma modification on meta-aramid fibrid, and dispersing the modified meta-aramid fibrid to obtain a slurry A; dispersing meta-position aramid chopped fibers to obtain slurry B; dispersing mica to obtain slurry C; and (2) uniformly mixing the slurry A, the slurry B and the slurry C, and carrying out papermaking and hot pressing to obtain the aramid mica paper. The aramid fiber mica paper is used for a motor insulating material of a wind driven generator, the insulating material is high in electrical strength, good in corona resistance and high in temperature resistance grade, the corona phenomenon and the partial discharge phenomenon in the high-speed operation process of the wind driven generator can be reduced by using the material, and the service life of the wind driven generator is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of papermaking, and in particular relates to a method for preparing insulating paper. Background Art

[0002] When wind turbines are running at high load, corona and partial discharge will inevitably occur. In order to extend the service life of wind turbines and reduce the occurrence of failures, it is necessary to improve the corona resistance and partial discharge starting voltage of the insulating materials in the motor. At the same time, the insulating materials may be stretched and bent during the installation process, and it is necessary to improve the mechanical properties of the insulating materials such as tensile strength, elongation at break and tear strength. Aramid materials have good mechanical properties and certain electrical strength, but their corona resistance is poor. Mica materials have excellent electrical strength and corona resistance, but poor mechanical properties. The combination of the two will make up for each other's shortcomings and enhance the comprehensive performance of the insulating materials.

[0003] For example, patent document CN114214867A discloses a corona-resistant aramid mica insulation paper and a preparation method thereof, the method comprising the following steps: step 1, firstly decomposing aramid chopped fibers, polyethylene oxide and water, and then adding aramid precipitated fibers to decompose to obtain a first slurry; step 2, adding muscovite flakes to the first slurry to decompose to obtain a second slurry, wherein the total mass of aramid chopped fibers, aramid precipitated fibers and muscovite flakes in the second slurry accounts for 0.04-0.07%; step 3, dehydrating, forming, pressing, drying and hot pressing the second slurry in sequence to obtain aramid / mica insulation paper. This patent greatly improves the corona resistance of aramid paper by adding high temperature and corona-resistant muscovite flakes to the manufacturing process of aramid paper, avoids the problem of aramid paper being easily aged due to repeated electric shocks under high temperature and high pressure, and meets the application requirements of equipment for a long life cycle of insulation.

[0004] However, the patent uses polyethylene oxide, which makes the product not resistant to high temperatures. The aramid mica paper product is prone to sticking to the roller in the subsequent high-temperature hot pressing process, which is not conducive to production. At the same time, the electrical and mechanical properties of the product made by this patent also need to be improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method for preparing aramid mica paper with excellent high temperature resistance, mechanical properties and electrical properties.

[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is: A method for preparing aramid mica paper comprises the following steps: (1) The meta-aramid fibrid is modified by CF4 plasma, and the modified meta-aramid fibrid is dispersed to obtain slurry A; the meta-aramid chopped fibers are dispersed to obtain slurry B; and mica is dispersed to obtain slurry C; (2) Slurry A, slurry B and slurry C are mixed evenly, and then paper-made and hot-pressed to obtain aramid mica paper.

[0007] The present invention performs CF4 plasma modification on the meta-aramid fibrid. The CF4 plasma can graft fluoride ions onto the meta-aramid fibrid, and the fluoride ions can provide the meta-aramid fibrid with higher corona resistance. Meanwhile, the CF4 plasma is easy to clean and hardly remains in the meta-aramid fibrid. Therefore, the present invention selects CF4 plasma to perform meta-aramid fibrid modification.

[0008] In the above preparation method, preferably, when the meta-aramid fibrid is subjected to CF4 plasma modification, the volume ratio of CF4 gas to Ar gas is (1-5): (5-30), the flow rate is 0.1-5SLM, and the treatment time is 1-10min. Within the above process parameter range, the fluoride ion grafting rate of CF4 plasma modification can be maximized to ensure economic efficiency. At the same time, the volume ratio of CF4 gas to Ar gas can control the grafting amount of fluoride ions, avoid the modification effect affected by too little grafting, and avoid the mechanical and electrical properties of aramid mica paper products caused by too much grafting.

[0009] In the above preparation method, preferably, when the modified meta-aramid fibrid is dispersed to obtain slurry A, it is dispersed in a deflaker for 5-10 minutes, and the speed of the deflaker is 1500-3000 rpm / min. The modified meta-aramid fibrid should play a bonding role, and after a specific deflaking treatment, it is conducive to uniform dispersion and combination with the meta-aramid chopped fibers and mica.

[0010] In the above preparation method, preferably, the length of the meta-aramid short fibers is 5-7 mm. The meta-aramid short fibers are controlled to be 5-7 mm because the meta-aramid short fibers within this range can have better bonding strength with the modified meta-aramid fibrids and mica, providing higher mechanical properties; if the length is not within this range, the uniformity of the aramid mica paper may be reduced and the mechanical properties may be low.

[0011] In the above preparation method, preferably, when the meta-aramid chopped fibers are dispersed to obtain slurry B, they are dispersed in a deflaker for 2-5 minutes, and the speed of the deflaker is 2000-3500 rpm / min. After the above deflaking treatment, the meta-aramid chopped fibers, the modified meta-aramid fibrids and mica can be mixed evenly, ensuring the effect of their functions.

[0012] In the above preparation method, preferably, the mica is calcined mica and / or synthetic mica, the particle size of the calcined mica is 70-120 μm, the particle size of the synthetic mica is 90-180 μm, and the mass ratio of synthetic mica to calcined mica is (0-50): (50-100). Controlling the mica particle size within the above-mentioned range can make the mica more evenly dispersed, and can provide better uniformity for the aramid mica paper, thereby making the product performance more stable; an appropriate amount of synthetic mica can provide better corona resistance for the aramid mica paper, and the electrical strength retention rate is high, but the surface of the synthetic mica is smoother than that of the calcined mica, and excessive use will deteriorate the mechanical properties of the aramid mica paper. More preferably, the mica must include synthetic mica, that is, the mica is calcined mica and synthetic mica, and the synergistic effect of synthetic mica and fluoride-modified meta-aramid fiber is beneficial to improving the product's corona resistance.

[0013] In the above preparation method, preferably, when the mica is dispersed to obtain slurry C, it is dispersed in a deflaker for 1-5 minutes, and the speed of the deflaker is 1500-3000 rpm / min. After the above deflaking treatment, the mica can be better mixed with the modified meta-aramid fiber and meta-aramid chopped fiber, ensuring better performance of its effect.

[0014] In the above preparation method, preferably, when slurry A, slurry B and slurry C are mixed evenly, a deflaking machine is used to mix them evenly. After slurry A, slurry B and slurry C are mixed evenly, the mass ratio of modified meta-aramid fibrils, meta-aramid chopped fibers and mica is (30-70): (5-25): (30-55). By controlling the above mass ratio, aramid mica paper with both high corona resistance and high mechanical properties can be prepared. Specifically, the modified meta-aramid fibrils should play a bonding role. By controlling its mass content, the meta-aramid chopped fibers and mica can be evenly dispersed and combined; if not processed within this range, the meta-aramid chopped fibers and mica are unevenly dispersed, and the aramid mica paper product cannot be well made, resulting in mica shedding and low surface strength. Meta-aramid chopped fibers provide strength for aramid mica paper. If there are too few meta-aramid chopped fibers, the mechanical properties of the product will be insufficient. If there are too many meta-aramid chopped fibers, the mechanical properties of the product will be affected. If the amount of meta-aramid chopped fibers is too much, the proportion of meta-aramid precipitated fibers will be low, which will affect the bonding of the product, reduce the surface strength of the product, and make the mica easy to fall off. Mica is used to provide aramid mica paper with higher corona resistance. If the amount of mica is too little, the surface uniformity will be reduced and the effect of improving the corona resistance will not be achieved. If the amount is too much, the bonding force of the aramid mica paper will be poor and the mechanical properties will be reduced.

[0015] In the above preparation method, preferably, during papermaking, papermaking is carried out through a PTI Kaiser method rapid paper sheet former, 3-9L of water is injected, the bubbling time is 5-10s, and it is allowed to stand for 5-10s. The aramid mica papermaking can be obtained by dehydration and drying.

[0016] In the above preparation method, preferably, during hot pressing, the hot pressing temperature is 260-320° C., the hot pressing pressure is 0.5-5 MPa, and the hot pressing speed is 2-8 m / min.

[0017] Wind power generation is essential to the use of motors. Early motors will have various problems due to the aging of insulation materials and poor corona resistance, which greatly reduces the power generation efficiency. The aramid mica paper prepared by the present invention can be used as the insulation material of the above motor, greatly improving the electrical strength and corona resistance of the material while ensuring mechanical strength, and is suitable for high-speed wind turbines.

[0018] The aramid mica paper of the present invention comprises modified meta-aramid fibrids, meta-aramid chopped fibers, mixed mica, etc., wherein slurry A mainly comprises meta-aramid fibrids modified by CF4 plasma, slurry B mainly comprises meta-aramid chopped fibers of a certain length, and slurry C mainly comprises one or two of calcined mica and synthetic mica (preferably comprising synthetic mica). By adopting the above three components and adjusting the addition ratio of each component, the prepared aramid mica paper has excellent high temperature resistance, higher corona resistance and electrical strength, and better mechanical strength. The mechanical strength, electrical strength and corona resistance of the produced aramid mica paper are higher than those of the unmodified aramid mica paper, and the service life of the wind turbine can be improved. In addition, the present invention uses domestic aramid and mica raw materials, which can reduce the limitation of raw materials, and the modified aramid mica paper has high temperature resistance, extremely strong electrical performance, high corona resistance grade, good mechanical performance, and can be applied to the motor insulation of the wind turbine.

[0019] In the present invention, the modified meta-aramid fibrid has higher corona resistance due to the grafting of fluoride ions. The modified meta-aramid fibrid provides bonding, electrical strength and partial corona resistance, the meta-aramid chopped fibers provide mechanical strength, and mica can provide high temperature resistance and high corona resistance, especially the high temperature resistance of synthetic mica is higher than that of natural mica. The present invention innovatively utilizes CF4 plasma to modify and optimize the meta-aramid fibrid that mainly provides bonding. This specific modification method is conducive to mutual coordination with other components, which is conducive to better improving the corona resistance of the product, especially after coordination with mica containing synthetic mica, the electrical resistance is more excellent and the electrical strength retention rate is higher. The present invention uses the synergistic coordination of the above three components to make the improved aramid mica paper have better electrical strength, corona resistance, mechanical properties and high temperature resistance.

[0020] The motor produced by the aramid mica paper of the present invention can avoid corona phenomenon and partial discharge phenomenon during operation, and can be applied to the motor insulation material of the wind power generator which needs high corona partial discharge voltage resistance performance and frequency conversion function.

[0021] Compared with the prior art, the advantages of the present invention are: 1. The aramid mica paper produced by the preparation method of the present invention uses slurry A (CF4 plasma modified meta-aramid fibrils), slurry B (meta-aramid chopped fibers) and slurry C (mica) as raw materials, and can combine the dual advantages of high strength, good dielectric properties and chemical stability of pure aramid paper and good corona resistance of pure mica paper, thereby improving the corona resistance of aramid mica paper, reducing the amount of local discharge, and improving the mechanical strength and electrical strength of aramid mica composite materials.

[0022] 2. The aramid mica paper of the present invention is used as the insulation material of the motor of the wind turbine. The insulation material has high electrical strength, good corona resistance and high temperature resistance. The use of the material can reduce the corona phenomenon and partial discharge phenomenon during the high-speed operation of the wind turbine, thereby increasing the service life of the wind turbine. DETAILED DESCRIPTION

[0023] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0024] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0026] Embodiment 1: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:10 (v / v), the flow rate was 3 SLM, and the treatment time was 5 min. By weight, 30% of the modified meta-aramid fibrid (the modified meta-aramid fibrid accounted for 30% of the mass of the aramid mica paper, and the following embodiments were the same as those in the comparative examples) was deflaked in a deflaker at a speed of 3000 rpm / min for 10 min and set aside.

[0027] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers (meta-aramid chopped fibers account for 15% of the mass of aramid mica paper, the same as in the following embodiments and comparative examples) with a length of 5 mm were added and stirred at a speed of 3000 rpm / min for 2 min for standby use.

[0028] 3. Preparation of component C: Component C is composed of calcined mica and synthetic mica, the particle size of calcined mica is 70-120 μm (D50 is about 100 μm, the same in the following examples and comparative examples), the particle size of synthetic mica is 90-180 μm (D50 is about 100 μm, the same in the following examples and comparative examples), and the ratio of synthetic mica to calcined mica is 1:10 (w / w). Take 55% of mica by weight (mica accounts for 55% of the mass of aramid mica paper, the same in the following examples and comparative examples), deflake in a deflaking machine at 3000 rpm / min, the deflaking time is 1 min, and set aside.

[0029] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 30:15:55), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 5L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 280℃, pressure: 3MPa, and vehicle speed of 4m / min.

[0030] The performance test results of the above aramid mica paper are as follows: The electrical strength is 31.37 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 13.5 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.76 kV, and the aging retention rate and mechanical properties are shown in Table 1. Among them, the electrical properties are tested using the national standard GB / T 1408.1-2006, and the mechanical properties are tested using the national standard: GB / T 12914-2008, the same below.

[0031] Comparative Example 1: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: 30% by weight of unmodified meta-aramid fibrils were deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0032] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 5 mm were added and stirred at a speed of 3000 rpm / min for 2 min for standby use.

[0033] 3. Preparation of component C: Component C is composed of calcined mica and synthetic mica. The particle size of calcined mica is 70-120μm, the particle size of synthetic mica is 90-180μm, and the ratio of synthetic mica to calcined mica is 1:10 (w / w). Take 55% of the mica by weight and deflake it in a deflaking machine at 3000rpm / min for 1min, and set aside.

[0034] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 30:15:55), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 5L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 280℃, pressure: 3MPa, and vehicle speed of 4m / min.

[0035] The performance test results of the above aramid mica paper are as follows: The electrical strength is 21.62 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 6.5 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.52 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0036] Embodiment 2: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 3:17 (v / v), the flow rate was 3SLM, and the treatment time was 5 minutes. By weight, 40% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0037] 2. Preparation of component B: 10% by weight of meta-aramid chopped fibers with a length of 7 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0038] 3. Preparation of component C: Component C is calcined mica, and the particle size of the calcined mica is 70-120 μm. 50% of the calcined mica is taken by weight and deflaked in a deflaking machine at 3000 rpm / min for 1 minute, and then set aside.

[0039] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 40:10:50), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 4L of water injected, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 300℃, pressure: 3MPa, and vehicle speed of 5m / min.

[0040] The performance test results of the above aramid mica paper are as follows: The electrical strength is 41.18 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 21.5 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.64 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0041] Comparative Example 2: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: 40% by weight of unmodified meta-aramid fibrils were deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0042] 2. Preparation of component B: 10% by weight of meta-aramid chopped fibers with a length of 7 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0043] 3. Preparation of component C: Component C is calcined mica, and the particle size of the calcined mica is 70-120 μm. 50% of the calcined mica is taken by weight and deflaked in a deflaking machine at 3000 rpm / min for 1 minute, and then set aside.

[0044] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 40:10:50), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 4L of water injected, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 300℃, pressure: 3MPa, and vehicle speed of 5m / min.

[0045] The performance test results of the above aramid mica paper are as follows: The electrical strength is 26.79 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 10.1 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.55 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0046] Embodiment 3: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:19 (v / v), the flow rate was 0.5 SLM, and the treatment time was 5 min. By weight, 45% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 min and set aside.

[0047] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 7 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0048] 3. Preparation of component C: Component C consists of calcined mica and synthetic mica. The particle size of calcined mica is 70-120μm, the particle size of synthetic mica is 90-180μm, and the ratio of synthetic mica to calcined mica is 1:5 (w / w). Take 40% of the mica by weight and deflake it in a deflaking machine at 3000rpm / min for 1min, and set aside.

[0049] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 45:15:40), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 9L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 310℃, pressure: 4MPa, and vehicle speed of 5m / min.

[0050] The performance test results of the above aramid mica paper are as follows: The electrical strength is 42.61 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 17 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.67 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0051] Embodiment 4: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:19 (v / v), the flow rate was 0.5 SLM, and the treatment time was 5 min. By weight, 45% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 min and set aside.

[0052] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 7 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0053] 3. Preparation of component C: Component C is calcined mica, the particle size of the calcined mica is 70-120 μm, and only calcined mica is used. 40% of the calcined mica is taken by weight and deflaked in a deflaking machine at 3000 rpm / min for 1 minute, and then set aside.

[0054] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 45:15:40), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 9L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 310℃, pressure: 4MPa, and vehicle speed of 5m / min.

[0055] The performance test results of the above aramid mica paper are as follows: The electrical strength is 42.75 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 20 h, the initial partial discharge voltage with a discharge amount of 10 pC is 0.74 kV, and the aging retention rate and mechanical properties are shown in Table 1. In this embodiment, synthetic mica is not used. Although the mechanical properties and electrical properties are slightly higher than those in Example 3, the aging electrical strength retention rate is low and the high temperature resistance will be reduced.

[0056] Embodiment 5: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:10 (v / v), the flow rate was 2SLM, and the treatment time was 5 minutes. By weight, 45% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0057] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 6 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0058] 3. Preparation of component C: Component C is composed of calcined mica and synthetic mica. The particle size of calcined mica is 70-120μm, the particle size of synthetic mica is 90-180μm, and the ratio of synthetic mica to calcined mica is 1:4 (w / w). Take 40% of the mica by weight and deflake it in a deflaking machine at 3000rpm / min for 1min, and set aside.

[0059] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 45:15:40), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 9L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 310℃, pressure: 4MPa, and vehicle speed of 5m / min.

[0060] The performance test results of the above aramid mica paper are as follows: The electrical strength is 42.76 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 17.2 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.71 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0061] Embodiment 6: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:10 (v / v), the flow rate was 2SLM, and the treatment time was 5 minutes. By weight, 45% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0062] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 6 mm were stirred at a speed of 3000 rpm / min for 2 min and set aside.

[0063] 3. Preparation of component C: Component C is calcined mica, and the particle size of the calcined mica is 70-120 μm. 40% of the calcined mica is taken by weight and deflaked in a deflaking machine at 3000 rpm / min for 1 minute for standby use.

[0064] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 45:15:40), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 9L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 310℃, pressure: 4MPa, and vehicle speed of 5m / min.

[0065] The performance test results of the above aramid mica paper are as follows: The electrical strength is 41.53 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 15 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.72 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0066] Embodiment 7: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 1:25 (v / v), the flow rate was 5 SLM, and the treatment time was 5 min. By weight, 50% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 min and set aside.

[0067] 2. Preparation of component B: 10% by weight of meta-aramid chopped fibers with a length of 5 mm were added and stirred at a speed of 3000 rpm / min for 2 min for standby use.

[0068] 3. Preparation of component C: Component C is composed of calcined mica and synthetic mica. The particle size of calcined mica is 70-120μm, the particle size of synthetic mica is 90-180μm, and the ratio of synthetic mica to calcined mica is 1:15 (w / w). Take 40% of the mica by weight and deflake it in a deflaking machine at 3000rpm / min for 1min, and set aside.

[0069] 4. Preparation of aramid mica paper: Mix the above three components A, B and C (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 50:10:40), use a deflaker to mix them evenly, and make paper in a PTI Kaiser rapid paper former, inject 5L of water, bubbling time 10s, stand for 5s, dehydrate and dry to obtain aramid mica paper. Hot press the paper to obtain aramid mica paper, and the hot pressing conditions are temperature: 300℃, pressure: 4MPa, and vehicle speed 4m / min; The performance test results of the above aramid mica paper are as follows: The electrical strength is 43.09 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 22.5 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.81 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0070] Comparative Example 3: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: 50% by weight of unmodified meta-aramid fibrils were deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0071] 2. Preparation of component B: 10% by weight of meta-aramid chopped fibers with a length of 5 mm were added and stirred at a speed of 3000 rpm / min for 2 min for standby use.

[0072] 3. Preparation of component C: Component C is calcined mica, and the particle size of the calcined mica is 70-120 μm. 40% of the calcined mica is taken by weight and deflaked in a deflaking machine at 3000 rpm / min for 1 minute for standby use.

[0073] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 50:10:40), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 5L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 300℃, pressure: 4MPa, and vehicle speed of 4m / min.

[0074] The performance test results of the above aramid mica paper are as follows: The electrical strength is 43.27 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 18.3 h, the initial partial discharge voltage with a discharge capacity of 10 pC is 0.78 kV, and the aging retention rate and mechanical properties are shown in Table 1.

[0075] Embodiment 8: A method for preparing aramid mica paper, the aramid mica paper comprising components A, B and C, comprising the following steps: 1. Preparation of Component A: The meta-aramid fibrid was modified by CF4 plasma, and the modification conditions were as follows: the addition ratio of CF4 gas to Ar gas was 10:1 (v / v), the flow rate was 3SLM, and the treatment time was 5 minutes. By weight, 30% of the modified meta-aramid fibrid was deflaked in a deflaker at a speed of 3000 rpm / min for 10 minutes and set aside.

[0076] 2. Preparation of component B: 15% by weight of meta-aramid chopped fibers with a length of 5 mm were added and stirred at a speed of 3000 rpm / min for 2 min for standby use.

[0077] 3. Preparation of component C: Component C is composed of calcined mica and synthetic mica. The particle size of calcined mica is 70-120μm, the particle size of synthetic mica is 90-180μm, and the ratio of synthetic mica to calcined mica is 1:10 (w / w). Take 55% of the mica by weight and deflake it in a deflaking machine at 3000rpm / min for 1min, and set aside.

[0078] 4. Preparation of aramid mica paper: The above three components A, B and C are mixed (that is, the mass ratio of the modified meta-aramid fiber, meta-aramid short fiber and mica is 30:15:55), mixed evenly using a deflaker, and papered in a PTI Kaiser rapid paper former, with 5L of water, bubbling time of 10s, standing for 5s, dehydration and drying to obtain aramid mica paper. Aramid mica paper is obtained by hot pressing the paper, and the hot pressing conditions are temperature: 300℃, pressure: 4MPa, and vehicle speed of 4m / min.

[0079] The performance test results of the above aramid mica paper are as follows: The electrical strength is 25.22 kV / mm, the corona resistance time under the test voltage of 1.8 kV can reach 10.9 h, the initial partial discharge voltage with a discharge amount of 10 pC is 0.49 kV, and the aging retention rate and mechanical properties are shown in Table 1. In this embodiment, plasma modification is performed using gas with too high a CF4 gas content, and too much fluorine ions are grafted, which will affect the electrical and mechanical properties of the aramid mica paper.

[0080] Table 1: Aging retention rate and mechanical properties of Examples 1-8 and Comparative Examples 1-3

[0081] Note: Aging retention rate refers to the retention rate of electrical strength.

Claims

1. A method for preparing aramid mica paper, characterized in that: The following steps are involved: (1) subjecting meta-aramid fibrids to CF4 plasma modification, and then dispersing the modified meta-aramid fibrids to obtain slurry A; Dispersing meta-aramid chopped fibers to obtain slurry B; dispersing mica to obtain slurry C; (2) Slurry A, slurry B and slurry C are mixed evenly, and then paper-made and hot-pressed to obtain aramid mica paper.

2. The preparation method according to claim 1, characterized in that: When the meta-aramid fiber is modified by CF4 plasma, the volume ratio of CF4 gas to Ar gas is (1-5): (5-30), the flow rate is 0.1-5 SLM, and the treatment time is 1-10 min.

3. The preparation method according to claim 1, characterized in that: When the modified meta-aramid fibrils are dispersed to obtain slurry A, the slurry is dispersed in a deflaker for 5-10 minutes at a speed of 1500-3000 rpm / min.

4. The preparation method according to claim 1, characterized in that: The length of the meta-aramid chopped fibers is 5-7 mm.

5. The preparation method according to claim 1, characterized in that: When the meta-aramid chopped fibers are dispersed to obtain slurry B, the slurry is dispersed in a deflaker for 2-5 minutes at a rotation speed of 2000-3500 rpm / min.

6. The preparation method according to claim 1, characterized in that: The mica is calcined mica and / or synthetic mica. The particle size of the calcined mica is 70-120 μm, the particle size of the synthetic mica is 90-180 μm, and the mass ratio of the synthetic mica to the calcined mica is (0-50):(50-100).

7. The preparation method according to claim 6, characterized in that: The mica is calcined mica and synthetic mica.

8. The preparation method according to claim 1, characterized in that: When the mica is dispersed to obtain slurry C, it is dispersed in a deflaker for 1-5 minutes, and the rotation speed of the deflaker is 1500-3000 rpm / min.

9. The preparation method according to claim 1, characterized in that: When slurry A, slurry B and slurry C are mixed evenly, a deflaking machine is used to mix them evenly. After slurry A, slurry B and slurry C are mixed evenly, the mass ratio of modified meta-aramid fibrils, meta-aramid chopped fibers and mica is (30-70): (5-25): (30-55).

10. The preparation method according to claim 1, characterized in that: During papermaking, papermaking is carried out through a PTI Kaiser method rapid paper sheet former, 3-9 L of water is injected, the bubbling time is 5-10 s, and the paper is left to stand for 5-10 s. After dehydration and drying, aramid mica papermaking can be obtained. During hot pressing, the hot pressing temperature is 260-320°C, the hot pressing pressure is 0.5-5 MPa, and the hot pressing vehicle speed is 2-8 m / min.

Citation Information

Patent Citations

  • Preparation method of aramid fiber nano-mica insulation paper modified by plasma treatment

    CN111945478A

  • High-corona-resistance aramid mica insulation paper

    CN112746514A

  • Powder material plasma surface modification method based on fiber carrier

    CN116943568A

  • Method for plasma treating paper and cardboards

    WO2004101891A1

Cited By

  • High-performance meta-position aramid fiber / mica composite insulation paper, preparation method and application