Method for preparing low-interception temperature-resistant hollow paper rod for heating cigarette
By using diatomaceous earth and phase change cooling materials in the heating cigarette hollow paper rod to construct a rapid cooling ternary network structure, the problems of aerosol retention, high sidewall temperature and 'paper baking' atmosphere are solved, and efficient cooling and High temperature deformation performance improves the sensory quality of the heated cigarette.
Patent Information
- Application Number
- CN202411149486.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Most of the aerosol release amount in the hollow paper rod of the heating cigarette is intercepted, the high side wall temperature leads to lip burning, and the 'paper baking' smell during the suction process, affecting the sensory quality.
The large number of interconnected heat conduction channels inside diatomaceous earth are combined with a variety of phase change cooling materials to build a fast cooling ternary network structure, and two multi-gradient cooling transmission channels are designed to improve the low retention rate and temperature resistance of hollow paper rods. performance.
It realizes the efficient cooling and high-temperature deformation performance of the hollow paper rod of heated cigarettes, reduces aerosol retention, avoids lip burning and the 'paper baking' atmosphere, and improves the suction quality.
Smart Images

Figure CN119061726A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a low-entrapment temperature-resistant hollow paper rod for heating cigarettes, and belongs to the field of papermaking. Background Art
[0002] The harm of traditional cigarettes to smokers, passive smokers and the environment has been proven many times, and quitting smoking is a long and difficult process. Therefore, relatively low-harm cigarette substitutes can serve as a more effective transition. Heated cigarettes have attracted widespread attention due to their characteristics of not requiring combustion. Heated cigarettes refer to tobacco products that heat tobacco materials through heating elements to produce inhalable aerosols from tobacco or reconstituted tobacco leaves at a lower temperature. Compared with traditional cigarettes, the harmful substances inhaled are significantly reduced.
[0003] The cooling section of heated cigarettes refers to heated cigarette paper that has the characteristics of heat conduction and cooling, high toughness and high strength, and can well connect the cigarette section and the filter section and intercept the cooling aerosol. The earliest cooling section with pleated polylactic acid (PLA) as the base is to fold it to form multiple longitudinally extending channels and then wrap it in the wrapping material to form a columnar filter rod. When the high-temperature smoke passes through the PLA polymer, it will reach the glass transition temperature, and the heat energy of the smoke will be consumed by absorbing heat to achieve a cooling of 14 to 23°C. However, the use of polylactic acid (PLA) for cooling will not only intercept a large amount of aerosol, but also melt and stack to block the transmission channel, thereby reducing the cooling efficiency and affecting the smoking quality. This technology was developed and industrialized by tobacco giant Philip Morris International (PMI). Among them, the most well-known application is the iQOS series of heated cigarettes. At present, the iQOS heatstick cigarette can reduce the smoke temperature to 40°C.
[0004] At present, major tobacco companies at home and abroad have also launched corresponding heated cigarette products. Through a lot of research, it can be found that the current research on the cooling performance of heated cigarette paper sticks mainly focuses on the following three aspects:
[0005] (1) Cooling of smoke from heated cigarettes is achieved by adding cooling materials, such as heat absorbing materials, heat storage materials, and heat conductive materials, to cigarettes. British American Tobacco Group (BAT) uses perforated cardboard empty tube filter rods to reduce smoke temperature. Patent publication number CN110372916A discloses a heat-not-burn cigarette filter rod that uses a starch empty tube as a cooling section. The patent uses starch, phase change material and polyol to prepare a starch-based cooling material. The phase change material has the effect of absorbing and storing heat, which can significantly reduce the temperature of the smoke flow and achieve a rapid and strong cooling effect. The cooling effect can reach 70-120°C. The raw materials used in the preparation are all biodegradable materials. At the same time, the retention of aroma components in cigarette smoke is effectively reduced. However, this patent does not mention the obvious "paper baking" smell of the empty paper rod during the heating and smoking process, which affects the sensory quality of the heated cigarette. Patent publication number CN109700 The invention patent of 070A discloses a cooling type acetate fiber particle, which uses hydroxypropyl methylcellulose as the outer coating layer to form a dense and leak-proof film on the surface of active particles or inactive particles, which can greatly reduce the temperature of cigarette smoke, but this patent does not mention the method for improving the smoking quality; the invention patent of patent CN106235403A discloses a slow-release flavor filter rod, which mixes low, medium and high molecular weight PEG in a certain proportion and sprays it on the filter tip tow. PEG can also be mixed with propylene glycol and hexadecyl alcohol to make a granular, round ribbon or coating-like heat-absorbing gel and added to the filter rod, which can reduce the smoke temperature by 1 to 8°C. Although this patent can improve the smoking quality, it has a poor effect on reducing the smoke temperature.
[0006] (2) Improve the heat loss of smoke through cooling structure design, such as using cavity buffering to store heat, lengthening the smoke channel, and strengthening the heat exchange between smoke and the external environment. A multi-segment cavity structure can be used in the cigarette structure, combined with highly transparent or perforated forming paper to improve the contact between ambient air and high-temperature smoke. A column with multiple longitudinal straight channels can be regarded as a multi-cavity cooling structure. The invention patent with patent publication number WO2017102633A1 discloses a method of using a spiral curved channel coiled parallel to the cross section as a smoke cooling channel. The channel surface is also provided with a periodically raised protruding portion, which is more conducive to smoke collision heat exchange and increases the smoke cooling amplitude. However, although the spiral curved channel is conducive to reducing the smoke temperature, it will have an adverse effect on the suction quality; the invention patent with patent publication number CN207604513U discloses an aerosol generating article, which is combined with an aerosol generating device to form an aerosol, and uses woven PLA fiber bundles for cooling. However, the biggest problem with using polylactic acid (PLA) is that it will collapse, soften and melt after contacting high-temperature smoke, resulting in blockage of the smoke channel, affecting the cooling effect of the cooling material, and aerosol retention should be a problem caused by it, affecting the suction quality.
[0007] (3) Composite cooling and heating cigarette filter rods are constructed by designing cooling structures and adding cooling materials. The early "Kuanzhai" cigarettes of Sichuan China Tobacco Industry Co., Ltd. used 18mm embossed gathered aluminum foil composite paper for cooling; Hubei China Tobacco Industry Co., Ltd.'s "MOK" cigarettes used perforated embossed gathered PLA materials for cooling; the invention patent with patent publication number CN207519612U discloses a flavoring and cooling base rod, which uses 10mm embossed gathered PLA film to achieve the purpose of cooling. The use of embossed gathered polylactic acid film is currently the most commonly used cooling method.
[0008] Studies have shown that most current heated cigarettes use three sections, namely, the cigarette section, the cooling section, and the filtering section. When the cigarette reaches the atomization temperature under heating conditions of 250-350°C, the atomizer and flavor substances in the cigarette section material vaporize and condense to form an aerosol. Since the cooling section of the cigarette is short and the cigarette section is completely heated, the inlet smoke temperature is too high, and its smoking experience is significantly different from that of traditional cigarettes, which directly affects product quality and user experience. The hollow paper rod of heated cigarettes is the cooling element and smoke transmission channel of heated cigarettes, and has good aerosol conduction and cooling performance. However, the development of hollow paper rods for heated cigarettes has the following bottleneck problems: (1) Most of the aerosol release is intercepted by the hollow section, affecting the sensory quality; (2) Due to the thin wall thickness of the hollow paper rod, the temperature of the side wall of the heated cigarette is high, which is prone to lip burning; (3) During the heated smoking process, the hollow paper rod has an obvious "paper baking" smell, which affects the sensory quality of the heated cigarette. Summary of the invention
[0009] This patent intends to build a ternary network structure of rapid cooling and high mobility coating interface for the heated cigarette hollow paper stick, so as to achieve simultaneous improvement of cooling performance and high temperature deformation resistance, and maintain and regulate its low interception and high toughness and hardness characteristics. This patent will provide a theoretical basis and technical support for the development of heated cigarette hollow paper sticks, and provide new ideas for the transformation and upgrading of the heated cigarette industry.
[0010] Problems existing in the prior art: (1) Most of the aerosol release is intercepted by the hollow section, affecting the sensory quality;
[0011] (2) Since the hollow paper stick has a thin wall thickness, the temperature of the heated cigarette side wall is high, which can easily burn the lips;
[0012] (3) During the heating and smoking process, the empty paper stick has a distinct "paper baking" smell, which affects the sensory quality of the heated cigarette.
[0013] [Technical solution]
[0014] In order to solve at least one of the above problems, the present invention provides a low-retention heat-resistant hollow paper stick for heating cigarettes and a preparation method thereof. For the first time, the extremely large number of interconnected heat-conducting channels inside diatomite are combined with its two major advantages of making paper smooth, light, strong, and reducing the shrinkage caused by humidity changes during papermaking. A variety of phase-change cooling materials are loaded to construct a multi-gradient rapid cooling ternary network structure to achieve rapid and efficient cooling. At the same time, a new design idea of two-section multi-gradient cooling transmission channels is proposed, that is, the first section is designed as a hollow paper stick channel for rapid cooling by composite synergy of multiple phase-change materials, and the second section is designed as a stable and high-strength hollow paper stick transmission channel with excellent high-temperature deformation resistance. The two sections of gradient cooling transmission channels with different functions are connected in sequence and at different length ratios, so as to achieve the simultaneous improvement of the low interception rate and temperature resistance of the hollow paper stick as a whole.
[0015] The first object of the present invention is to solve the "easy lip burning" phenomenon caused by the high temperature of the side wall of the heated cigarette, and provide a method for preparing a high-strength, high-toughness, and high-heat-resistance hollow paper stick, the method comprising the following steps:
[0016] (1) First, plant fiber and regenerated cellulose fiber raw materials are obtained by beating and refining, and regenerated cellulose fiber and a high temperature resistant additive are added into a reaction container and stirred evenly to obtain a modified fiber raw material.
[0017] (2) The plant fiber of step (1) and the regenerated cellulose fiber raw material modified with a high temperature resistant additive are mixed in a certain proportion to make a hollow paper stick base paper for the second stage.
[0018] (3) Adding a phase-change temperature-resistant material and charge-reversal treated diatomaceous earth into a reaction container, stirring the mixture evenly at room temperature to obtain a mixed solution.
[0019] (4) The mixed solution of step (3) is used for preparing hollow paper stick base paper with plant fiber and regenerated cellulose fiber in step (1) as raw materials through two processes: in-slurry addition and surface coating, for use in the first stage.
[0020] (5) The base paper of steps (4) and (2) is prepared into a hollow paper rod, which is connected and combined with an adhesive to obtain a low-retention temperature-resistant hollow paper rod for heating cigarettes.
[0021] In one embodiment of the present invention, the steps are as follows:
[0022] (1) Plant fibers or regenerated cellulose fibers are added to a Wall-E pulper for decomposition, and then the concentration is adjusted for pulping to obtain initial fiber raw materials.
[0023] (2) The regenerated cellulose fiber in step (1) is mixed with a high temperature resistant additive, and stirred evenly at room temperature of 25° C. to obtain a modified regenerated cellulose fiber raw material.
[0024] (3) The plant fiber suspension obtained in steps (1) and (2) and the modified regenerated cellulose fiber suspension are mixed and then subjected to web-making, pressing and dehydration, and drying in different proportions to obtain hollow paper rod base paper with high strength, high toughness, and high heat resistance.
[0025] In one embodiment of the present invention, the plant fiber described in step (1) is one or more of bleached chemical hardwood pulp fiber, bleached chemical coniferous pulp fiber, bleached chemical bamboo pulp fiber, hemp pulp fiber, and natural chemical mechanical pulp fiber, and the beating degree is 30-60°SR; the regenerated cellulose fiber is one or more of viscose fiber, tencel fiber, modal fiber, bamboo fiber, chitin fiber, and cuprammonia fiber, and the beating degree is 18-50°SR.
[0026] In one embodiment of the present invention, the Walle beater deflaking concentration in step (1) is 1.57%.
[0027] In one embodiment of the present invention, the refining concentration of the PFI refiner in step (1) is 10%.
[0028] In one embodiment of the present invention, the refining speed of the PFI refiner in step (1) is 10000r-60000r.
[0029] In one embodiment of the present invention, the high temperature resistant auxiliary agent in step (2) is one or more polymer materials containing phosphorus, boron, silicon, and halogen element groups.
[0030] In one embodiment of the present invention, in step (2), the mass ratio of the modified regenerated cellulose fiber raw material to the high temperature resistant additive is 1:1-4; the mass percentage concentration of the high temperature resistant additive is 1%-5%; stirring at 50-80°C and 300-600rpm for 3-6h, keeping warm for 1-2h, and washing with water three times to obtain a fiber suspension.
[0031] In one embodiment of the present invention, the papermaking decomposition process in step (3) is decomposition at a speed of 3000r / min for 5-10min, a pressing pressure of 0.4Mpa, a pressing time of 3min, and a drying time of 105°C for 10min.
[0032] In one embodiment of the present invention, the ratio of plant fiber to modified regenerated cellulose fiber in step (3) is 6-8:4-2. Paper weight 60-100 g / m 2 .
[0033] The second purpose of the present invention is to solve the problem of obvious "paper baking" smell of hollow paper sticks during smoking of heated cigarettes, and provide a method for preparing a high-efficiency cooling composite phase change material and a fast and high-efficiency cooling hollow paper stick, comprising the following steps:
[0034] (1) Add diatomaceous earth, water, and a cationic auxiliary agent into a reaction container, stir evenly at room temperature of 25° C., react for a period of time, and wash three times to obtain charge-reversed diatomaceous earth.
[0035] (2) Adding a phase change temperature-resistant material and charge reversal treated diatomaceous earth into a reaction container, stirring evenly at room temperature of 25° C., reacting for 1-3 hours, and washing three times to obtain a composite phase change material.
[0036] (3) The composite phase change material of step (2) is prepared by three processes: in-slurry addition, surface coating, and in-slurry addition combined with surface coating to prepare a first section of hollow paper stick base paper with plant fiber and regenerated cellulose fiber as raw materials.
[0037] In one embodiment of the present invention, the diatomaceous earth in step (1) has a negative charge on its surface and a particle size of 5-250 mm; the cationic adjuvant is one or more of polyethyleneimine, chitosan, cationic polyacrylamide, sodium carboxymethyl cellulose, and cationic starch.
[0038] In one embodiment of the present invention, the mass ratio of diatomaceous earth to water in step (1) is 1:50-100.
[0039] In one embodiment of the present invention, the mass ratio of diatomaceous earth to cationic auxiliary agent in step (1) is 1:4-10.
[0040] In one embodiment of the present invention, the uniform mixing in step (1) specifically comprises: stirring at 400 rpm for 1-2 hours.
[0041] In one embodiment of the present invention, the uniform mixing in step (2) specifically comprises: stirring at 600 rpm for 1-3 hours.
[0042] In one embodiment of the present invention, the phase change temperature-resistant material described in step (2) is one or more of polyethylene glycol with a molecular weight of 600, 1000, 2000, 6000, and 10000; the crystalline hydrated salt is one or more of magnesium chloride hexahydrate, magnesium nitrate hexahydrate, sodium thiosulfate pentahydrate, palladium hydroxide octahydrate, sodium sulfate decahydrate, calcium chloride hexahydrate, lithium perchlorate trihydrate, and disodium hydrogen phosphate dodecahydrate; the fatty acid is one or more of octadecanoic acid, hexadecanoic acid, tetradecanoic acid, and dodecanoic acid; and the fatty alcohol is one or more of dodecanol, tetradecanol, hexadecanol, pentaerythritol, and neopentyl glycol.
[0043] In one embodiment of the present invention, in step (2), the mass ratio of the phase change temperature resistant material to the charge reversal diatomaceous earth is 1:1-4, and the reaction time is 1-3h.
[0044] In one embodiment of the present invention, the mass ratio of the phase change temperature resistant material to water in step (2) is 1-5:50-100.
[0045] In one embodiment of the present invention, the amount of the composite phase change material added to the pulp in step (3) is 5%-20%, relative to the absolute dry raw material, and the paper weight is 60-100g / m 2 .
[0046] In one embodiment of the present invention, the coating method described in step (3) is roller pressing; the coating liquid is one or more of starch, alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), and sodium carboxymethyl cellulose; and the mass ratio of the coating liquid to the composite phase change material is 10-20:1.
[0047] The third object of the present invention is to solve the problem that most of the aerosol release is intercepted by the hollow section, and provide a method for constructing a hollow paper stick multi-gradient with two sections, namely a rapid cooling channel and a stable high-strength transmission channel, comprising the following steps:
[0048] (1) The first section of hollow paper stick base paper and the second section of hollow paper stick base paper are prepared into a hollow paper stick.
[0049] (2) The two hollow paper sticks are connected and combined by an adhesive to obtain a low-retention temperature-resistant hollow paper stick for heating cigarettes.
[0050] In one embodiment of the present invention, the hollow paper stick in step (1) is prepared by machine or manual curling.
[0051] In one embodiment of the present invention, the binder in step (2) is one or more of starch, sodium carboxymethyl cellulose, and guar gum.
[0052] In one embodiment of the present invention, in step (2), the ratio of the first section of hollow paper rods (rapid cooling section) to the second section of hollow paper rods (high-strength transmission section) is 3-7:7-3.
[0053] The fourth purpose of the present invention is to combine two hollow paper sticks, connect them with a filter section and a cigarette stick section, and apply them to the field of heated cigarettes.
[0054] In one embodiment of the present invention, the charge-reversed diatomaceous earth in step (3) is cationic polymer-modified diatomaceous earth with a positively charged surface.
[0055] In one embodiment of the present invention, the step (4) of mixing and adding the composite phase change material into the slurry comprises the following steps:
[0056] (1) The plant fibers are deflated using a fiber deflation device to obtain a uniformly dispersed fiber suspension.
[0057] (2) The regenerated cellulose fibers are deflated using a fiber deflation device to obtain a uniformly dispersed fiber suspension.
[0058] (3) The fiber suspensions obtained in step (1) and step (2) are mixed and dispersed using a fiber dispersing device to obtain a uniformly dispersed fiber suspension. At the same time, the composite phase change material is added.
[0059] (4) The fiber suspension obtained in step (3) is placed on a screen for papermaking, squeezed for dehydration, and dried to obtain a first section of hollow paper stick base paper.
[0060] The addition amount of the composite phase change material is 5%-20% relative to the absolute dry raw material.
[0061] In one embodiment of the present invention, the hollow paper stick in step (5) is prepared by machine or manual curling; the binder is one or more of starch, sodium carboxymethyl cellulose, and guar gum. The ratio of the first hollow paper stick (rapid cooling section) to the second hollow paper stick (high-strength transmission section) is 3-7:7-3.
[0062] The rapid cooling section and the high-strength transmission section are connected to form a low-retention / heat-resistant hollow paper rod, which is used as a cooling total section and is combined with the cigarette section and the filtering section in sequence before and after and applied to heating cigarettes.
[0063] Beneficial Effects
[0064] (1) The hollow paper rod for heating cigarettes of the present invention is modified for temperature resistance of regenerated cellulose fibers, and the ratio of plant fibers to regenerated cellulose fibers is adjusted to achieve simultaneous improvement of high hardness, high strength and high heat resistance, thereby solving the problem of "easy lip burns" caused by the high temperature of the side wall of the heating cigarette.
[0065] (2) The hollow paper stick for heating cigarettes of the present invention utilizes the numerous interconnected heat-conducting channels inside diatomite, reverses its surface charge to positive charge through grafting, and then mixes it with a variety of phase-change cooling materials. Through hydrogen bonding, hydroxylamine reaction and electrostatic adsorption, a multi-layer synergistic cooling composite material is constructed, which gives the paper high-temperature deformation resistance while rapidly cooling. By constructing a composite phase-change polymer network, a "bridge" is built to enhance the interaction between the fiber raw material and the high-temperature aerosol. The obvious "paper baking" smell of the empty paper stick during the heating and smoking process is solved.
[0066] (3) The hollow paper rod of the heated cigarette of the present invention adopts segmented cooling. Without increasing the length of the cooling section, the cooling section is designed as two sections of multi-gradient cooling transmission channels, namely, a rapid cooling section and a high-strength transmission section. The two sections of the hollow paper rods are connected at different length ratios. The different cooling and temperature resistance characteristics of the composite phase change polymer material and the high-strength and high-resistance thermal paper rod are utilized to compare their overall interception effects, thereby achieving an overall low interception rate and excellent high-temperature deformation resistance, which effectively solves the problem that most of the aerosol release is intercepted by the hollow section.
[0067] (4) The various raw materials used in the hollow paper stick for heating cigarettes of the present invention are matched and synergistic with each other to form a product with excellent performance. Since diatomaceous earth is commonly used in the papermaking process, it has the effect of making the paper smooth and light in weight. At the same time, the special internal extremely interconnected heat conduction channels of diatomaceous earth provide abundant retention points for various phase change cooling materials, which can achieve the effect of "killing two birds with one stone". On the other hand, the major bulk materials and polymer materials are low-priced and easy to obtain, and the use of the present invention has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 It is a rapid cooling section and a high-strength transmission section with different length ratios (unit: mm). DETAILED DESCRIPTION
[0069] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explanation of the present invention and are not intended to limit the present invention. The solutions described in the embodiments that do not specifically specify solvents are all water-based. All fractions are calculated by mass fraction.
[0070] The test methods involved in the following embodiments are:
[0071] Performance testing method:
[0072] The tobacco segment of the cigarette sample is inserted into the HnB cigarette heater for heating, and the generated smoke is sucked into the T-type three-way structure by the smoking machine. The HCI mode is used for puffing, with a puff time of 2s, a puff interval of 30s, a puff volume of 55mL per puff, and a bell-shaped puff curve. The other two ends of the three-way structure are connected to the smoking machine and the smoke temperature measuring device respectively, and the temperature recorder records the dynamic temperature of the smoke flowing out of the filter tip measured by the thermocouple. (Refer to Patent Publication No. CN110411597A—Tipstick Temperature Measuring Device).
[0073] Phase change material loading test:
[0074] The mass of diatomaceous earth loaded with phase change material before and after drying to a certain dryness (dryness: 3.0%) was weighed, and the loading amount was characterized by the change in mass.
[0075] Sensory evaluation:
[0076] It is carried out in accordance with "YC / T415-2011 Sensory Evaluation Method for Tobacco Products".
[0077] The raw materials used in the following examples are:
[0078] The high temperature resistant additive described in the present invention is one or more polymer materials containing phosphorus, boron, silicon, and halogen element groups: it can be prepared by itself or a commercially available product. The high temperature resistant additive involved in the following embodiments is purchased from Guangzhou Dongfugui Chemical Raw Materials Co., Ltd., item number: organic high temperature resistant additive SRE-5250.
[0079] The Tencel fiber and viscose fiber involved in the following embodiments were purchased from Hubei Aoyuan Meigu Company; the diatomaceous earth was purchased from Sinopharm Chemical Reagents, item number: XW688555499, with a median particle size of 3.5 μm; the polyethyleneimine was purchased from Shanghai Aladeng Biochemical Technology Co., Ltd., item number: E107078, with a molecular weight of 1800; the starch was purchased from Hangzhou Zhiyou Technology Co., Ltd.
[0080] The raw material preparation method used in the following examples:
[0081] Preparation method of 18°SR broadleaf pulp and 18°SR coniferous pulp: use a 5kg heavy weight on a Wall-E pulper to beat the pulp for about 15-20 minutes, from the initial 12.5°SR to 18°SR; and prepare the above-mentioned 18°SR broadleaf pulp and 18°SR coniferous pulp respectively.
[0082] Preparation method of 18°SR heat-resistant additive modified Tencel fiber, 18°SR Tencel fiber, 18°SR viscose fiber, and 18°SR heat-resistant additive modified viscose fiber: Because the above-mentioned pulps are in small amounts and are not suitable for large-scale pulping with a Wall-E pulper, a PFI pulper is used for pulping. The initial beating degree is 9-12°SR, so the knife distance is 0.2mm, and the pulping is about 5000-7500r, to prepare 18°SR heat-resistant additive modified Tencel fiber, 18°SR Tencel fiber, 18°SR viscose fiber, and 18°SR heat-resistant additive modified viscose fiber, respectively.
[0083] Example 1: Preparation of low-retention high-temperature resistant hollow paper stick for heating cigarettes
[0084] The specific steps are as follows: (1) adding 12 g of a high temperature resistant additive to 388 ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 3%, adding 12 g of 18°SR Tencel fiber thereto, stirring at 300 rpm at 50°C for 3 h, keeping warm for 1 h, and then washing with water three times to obtain a 10% 18°SR heat resistant additive modified Tencel fiber suspension;
[0085] Adding 18°SR hardwood pulp and 18°SR softwood pulp into water respectively to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR softwood pulp suspension;
[0086] (2) grinding the obtained 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR heat-resistant additive modified Tencel fiber suspension, all of which have a mass percentage concentration of 10%, respectively using a PFI refiner for 15000r, 15000r and 20000r, to a final beating degree of 43°SR for the hardwood pulp, 45°SR for the softwood pulp, and 48°SR for the heat-resistant additive modified Tencel fiber;
[0087] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive modified Tencel fiber = 4:4:2 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0088] (3) Add 2 g of diatomaceous earth with a particle size of 20 mm to 98 ml of water, add 8 g of cationic auxiliary polyethyleneimine with a molecular weight of 1800, stir at 400 rpm for 1 hour at room temperature of 25°C, wash three times and then dry at 60°C for 6 hours to obtain charge reversal diatomaceous earth. According to the above method, in order to obtain more charge reversal diatomaceous earth, it can be prepared multiple times.
[0089] (4) Add 5 g of disodium hydrogen phosphate dodecahydrate to 95 ml of water, and add 5 g of the charge reversal diatomaceous earth obtained in step (3) at the same time, stir at 600 rpm for 1 h at room temperature 25 ° C, wash three times and then dry. The drying conditions are: 60 ° C, 6 h, to obtain a temperature-resistant composite phase change material.
[0090] (5) Raw material processing:
[0091] 18°SR Tencel fiber is added into water, stirred at 300 rpm for 3 hours at 50°C, kept warm for 1 hour, and then washed with water three times to obtain a 10% 18°SR Tencel fiber suspension; 18°SR hardwood pulp and 18°SR coniferous pulp are respectively added into water to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR coniferous pulp suspension;
[0092] The 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR Tencel fiber suspension prepared according to the above method with a mass percentage concentration of 10% were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final hardwood pulp beating degree was 43°SR, the softwood pulp beating degree was 45°SR, and the Tencel fiber was 48°SR;
[0093] After refining, a pulp suspension is prepared according to the ratio of broadleaf pulp: coniferous pulp: tencel fiber = 4:4:2 (absolute dry mass ratio), and after mixing, the composite phase change material prepared in step (4) is added in an amount of 10%. The papermaking deflaking process is 3000r / min speed for 5-10min, pressing pressure of 0.4Mpa, pressing time of 3min, drying temperature of 105°C, drying time of 10min, and paper weight of 60g / m 2 , and obtain the first section of hollow paper stick base paper.
[0094] (6) Using a paper stick forming machine, the first section of hollow paper stick base paper and the second section of hollow paper stick base paper are prepared into paper sticks.
[0095] First, a starch binder was prepared: 1 g of starch was added to 99 ml of water, stirred at 500 rpm for 1 h at 80° C., and kept warm at 60° C. to obtain a starch binder with a mass percentage concentration of 1%;
[0096] Secondly, a starch adhesive is applied to the interface of two hollow paper sticks connected at a length ratio of 5:5, and finally a low-retention high-temperature resistant hollow paper stick that can be used for heating cigarettes is obtained.
[0097] In this example, the first section of the hollow paper stick maintains high strength and hardness while also taking into account the cooling effect on the smoke. The second section of the hollow paper stick achieves high moisture absorption rate and high cooling efficiency while maintaining its high temperature resistance deformation effect.
[0098] Example 2: Effect of the amount of high temperature resistant modification additive
[0099] The specific implementation method is the same as Example 1, except that only step (1) in Example 1 is adjusted to add 4g of high temperature resistant additive to 396ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 1%. The specific adjustment step (1) is:
[0100] (1) 4 g of a high temperature resistant additive was added to 396 ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 1%; 12 g of 18°SR Tencel fiber was added thereto, stirred at 300 rpm at 50°C for 3 h, kept warm for 1 h, and then washed three times with water to obtain a 10% 18°SR heat resistant additive modified Tencel fiber suspension.
[0101] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0102] Example 3: Effect of the amount of high temperature resistant modification additive
[0103] The specific implementation method is the same as Example 1, except that only step (1) in Example 1 is adjusted to add 20g of high temperature resistant additive to 380ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 5%. The specific adjustment step (1) is:
[0104] (1) Add 20 g of a high temperature resistant additive to 380 ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 5%; add 12 g of 18°SR Tencel fiber thereto, stir at 300 rpm at 50°C for 3 h, keep warm for 1 h, and then wash three times with water to obtain a 10% 18°SR heat resistant additive modified Tencel fiber suspension.
[0105] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0106] Example 4: Effect of the ratio of plant fiber and high temperature resistant additive modified regenerated fiber
[0107] The specific implementation method is the same as Example 1, except that step (2) in Example 1 is adjusted to prepare a pulp suspension according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive-modified tencel fiber = 4:5:1 (absolute dry weight ratio) after grinding. At the same time, step (5) is also changed according to this ratio.
[0108] The specific adjustment steps (2) are:
[0109] 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR heat-resistant additive modified Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final hardwood pulp beating degree was 43°SR, the softwood pulp beating degree was 45°SR, and the heat-resistant additive modified Tencel fiber was to a beating degree of 48°SR;
[0110] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive modified Tencel fiber = 4:5:1 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0111] Adjust step (5) to:
[0112] 18°SR Tencel fiber is added into water, stirred at 300 rpm for 3 hours at 50°C, kept warm for 1 hour, and then washed with water three times to obtain a 10% 18°SR Tencel fiber suspension; 18°SR hardwood pulp and 18°SR coniferous pulp are respectively added into water to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR coniferous pulp suspension;
[0113] 18°SR hardwood pulp suspension, 18°SR coniferous wood pulp suspension and 18°SR Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final beating degree of the hardwood pulp was 43°SR, the coniferous wood pulp was 45°SR, and the Tencel fiber was 48°SR;
[0114] After refining, a pulp suspension is prepared according to the ratio of broadleaf pulp: coniferous pulp: tencel fiber = 4:5:1 (absolute dry mass ratio), and the composite phase change material prepared in step (4) is added into the pulp in an amount of 10%. The papermaking deflaking process is 3000r / min speed for 5-10min, pressing pressure of 0.4Mpa, pressing time of 3min, drying temperature of 105°C, drying time of 10min, and paper weight of 60g / m 2 , and obtain the first section of hollow paper stick base paper.
[0115] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0116] Example 5: Effect of the ratio of plant fiber and high temperature resistant additive modified regenerated fiber
[0117] Specific implementation method The same as Example 1, except that (2) in Example 1 is changed to prepare pulp suspension according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive modified tencel fiber = 3:4:3 (absolute dry weight ratio) after grinding. Meanwhile, step (5) is also changed according to this ratio.
[0118] Adjustment step (2) is:
[0119] 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR heat-resistant additive modified Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final hardwood pulp beating degree was 43°SR, the softwood pulp beating degree was 45°SR, and the heat-resistant additive modified Tencel fiber was to a beating degree of 48°SR;
[0120] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive modified Tencel fiber = 3:4:3 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0121] Adjust step (5) to:
[0122] 18°SR Tencel fiber is added into water, stirred at 300 rpm for 3 hours at 50°C, kept warm for 1 hour, and then washed with water three times to obtain a 10% 18°SR Tencel fiber suspension; 18°SR hardwood pulp and 18°SR coniferous pulp are respectively added into water to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR coniferous pulp suspension;
[0123] 18°SR hardwood pulp suspension, 18°SR coniferous wood pulp suspension and 18°SR Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final beating degree of the hardwood pulp was 43°SR, the coniferous wood pulp was 45°SR, and the Tencel fiber was 48°SR;
[0124] After refining, a pulp suspension is prepared according to the ratio of broadleaf pulp: coniferous pulp: tencel fiber = 3:4:3 (absolute dry mass ratio), and the composite phase change material prepared in step (4) is added into the pulp in an amount of 10%. The papermaking deflaking process is 3000r / min speed for 5-10min, pressing pressure of 0.4Mpa, pressing time of 3min, drying temperature of 105°C, drying time of 10min, and paper weight of 60g / m 2 , and obtain the first section of hollow paper stick base paper.
[0125] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0126] Example 6: Influence of the ratio of plant fiber and regenerated fiber modified with a high temperature resistant additive. The specific implementation method is the same as that of Example 1, except that step (2) in Example 1 is adjusted to prepare the pulp suspension after grinding according to the ratio of broadleaf pulp: coniferous pulp: heat resistant additive modified Tencel fiber = 3:3:4 (absolute dry mass ratio), and step (5) is also changed according to this ratio.
[0127] Adjustment step (2) is:
[0128] 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR heat-resistant additive modified Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final hardwood pulp beating degree was 43°SR, the softwood pulp beating degree was 45°SR, and the heat-resistant additive modified Tencel fiber was to a beating degree of 48°SR;
[0129] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: heat-resistant additive modified Tencel fiber = 3:4:3 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0130] Adjust step (5) to:
[0131] 18°SR Tencel fiber is added into water, stirred at 300 rpm for 3 hours at 50°C, kept warm for 1 hour, and then washed with water three times to obtain a 10% 18°SR Tencel fiber suspension; 18°SR hardwood pulp and 18°SR coniferous pulp are respectively added into water to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR coniferous pulp suspension;
[0132] 18°SR hardwood pulp suspension, 18°SR coniferous wood pulp suspension and 18°SR Tencel fiber suspension, all with a mass percentage concentration of 10%, were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final beating degree of the hardwood pulp was 43°SR, the coniferous wood pulp was 45°SR, and the Tencel fiber was 48°SR;
[0133] After refining, a pulp suspension is prepared according to the ratio of broadleaf pulp: coniferous pulp: tencel fiber = 3:4:3 (absolute dry mass ratio), and the composite phase change material prepared in step (4) is added into the pulp in an amount of 10%. The papermaking deflaking process is 3000r / min speed for 5-10min, pressing pressure of 0.4Mpa, pressing time of 3min, drying temperature of 105°C, drying time of 10min, and paper weight of 60g / m 2 , and obtain the first section of hollow paper stick base paper.
[0134] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0135] Example 7: Effect of the amount of charge reversal diatomaceous earth added
[0136] The specific implementation method is the same as that of Example 1, except that the 5g charge-reversal diatomaceous earth in step (4) of Example 1 is adjusted to 10g. Specifically:
[0137] (4) Add 5 g of disodium hydrogen phosphate dodecahydrate to 95 ml of water, and add 10 g of the charge reversal diatomaceous earth obtained in step (3), stir at 600 rpm at 25° C. for 1 h, wash three times and then dry at 60° C. for 6 h to obtain a temperature-resistant composite phase change material.
[0138] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0139] Example 8: Effect of the amount of charge reversal diatomaceous earth added
[0140] The specific implementation method is the same as that of Example 1, except that the 5g charge-reversed diatomaceous earth in step (4) of Example 1 is adjusted to 15g. Specifically:
[0141] (4) Add 5 g of disodium hydrogen phosphate dodecahydrate to 95 ml of water, and add 15 g of charge reversal diatomaceous earth at the same time, stir at 600 rpm at 25° C. for 1 h, wash three times and then dry at 60° C. for 6 h to obtain a temperature-resistant composite phase change material.
[0142] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0143] Example 9: Influence of Preparation Conditions of Heat-Resistant Composite Phase Change Materials
[0144] The specific implementation is the same as in Example 1, except that the stirring at 600 rpm for 1 h at 25°C in (4) of Example 1 is adjusted to stirring at 600 rpm for 2 h at 25°C. Specifically:
[0145] (4) Add 5 g of disodium hydrogen phosphate dodecahydrate to 95 ml of water, and add 5 g of charge reversal diatomaceous earth at the same time, stir at 600 rpm at 25° C. for 2 h, wash three times and then dry at 60° C. for 6 h to obtain a temperature-resistant composite phase change material.
[0146] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0147] Example 10: Influence of Preparation Conditions of Heat-Resistant Composite Phase Change Materials
[0148] The specific implementation is the same as in Example 1, except that the stirring at 600 rpm for 1 h at room temperature 25°C in (4) of Example 1 is adjusted to stirring at 600 rpm for 3 h at 25°C. Specifically:
[0149] (4) Add 5 g of disodium hydrogen phosphate dodecahydrate to 95 ml of water, and add 5 g of charge reversal diatomaceous earth at the same time, stir at 600 rpm at 25° C. for 3 h, wash three times and then dry at 60° C. for 6 h to obtain a temperature-resistant composite phase change material.
[0150] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0151] Example 11: Effect of the ratio of two paper sticks
[0152] The specific implementation method is the same as that of Example 1, except that the starch adhesive is applied to the interface of the hollow paper sticks connected at a length ratio of 5:5 in (6) of Example 1 instead of applying the starch adhesive to the interface of the hollow paper sticks connected at a length ratio of 3:7. Specifically:
[0153] (6) Using a paper stick forming machine, the first section of hollow paper stick base paper and the second section of hollow paper stick base paper are prepared into paper sticks.
[0154] First, a starch binder was prepared: 1 g of starch was added to 99 ml of water, stirred at 500 rpm at 80° C. for 1 h, and kept warm at 60° C. to obtain a starch binder with a mass percentage concentration of 1%;
[0155] Secondly, a starch adhesive is applied to the interfaces of the hollow paper rods connected at a length ratio of 3:7, and finally a low-retention high-temperature-resistant hollow paper rod that can be used for heating cigarettes is obtained.
[0156] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0157] Example 12: Effect of the ratio of two paper sticks
[0158] The specific implementation method is the same as that of Example 1, except that the starch adhesive is applied to the interface of the hollow paper sticks connected at a ratio of 5:5 in (6) of Example 1 instead of applying the starch adhesive to the interface of the hollow paper sticks connected at a length ratio of 7:3. Specifically:
[0159] (6) Using a paper stick forming machine, the first section of hollow paper stick base paper and the second section of hollow paper stick base paper are prepared into paper sticks.
[0160] First, a starch binder was prepared: 1 g of starch was added to 99 ml of water, stirred at 500 rpm at 80° C. for 1 h, and kept warm at 60° C. to obtain a starch binder with a mass percentage concentration of 1%;
[0161] Secondly, a starch adhesive is applied to the interfaces of the hollow paper rods connected at a length ratio of 7:3, and finally a low-retention high-temperature-resistant hollow paper rod that can be used for heating cigarettes is obtained.
[0162] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0163] Comparative Example 1: Effect of not adding high temperature resistant additives
[0164] The specific implementation method is the same as Example 1, except that in Example 1, no high temperature resistant additive is added, and unmodified Tencel fiber is used to prepare the second hollow paper stick base paper. The specific adjustment step (1) is:
[0165] (1) Add 12 g of 18° SR Tencel fiber to 400 ml of water, stir at 300 rpm at 50° C. for 3 h, keep warm for 1 h, and then wash with water three times to obtain a 10% 18° SR Tencel fiber suspension;
[0166] Adding 18°SR hardwood pulp and 18°SR softwood pulp into water respectively to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR softwood pulp suspension;
[0167] Adjustment step (2) is:
[0168] The 18°SR hardwood pulp suspension, 18°SR softwood pulp suspension and 18°SR Tencel fiber suspension prepared according to the above method with a mass percentage concentration of 10% were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final hardwood pulp beating degree was 43°SR, the softwood pulp beating degree was 45°SR, and the Tencel fiber was 48°SR;
[0169] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: tencel fiber = 4:4:2 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0170] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0171] Comparative Example 2: Effect of Different Fibers
[0172] The specific implementation is the same as in Example 1, except that the Tencel fiber in Example 1 is changed into viscose fiber.
[0173] The specific adjustment steps (1) are:
[0174] (1) 12 g of a high temperature resistant additive was added to 388 ml of water to prepare a high temperature resistant modified additive with a mass percentage concentration of 3%, 12 g of 18°SR viscose fiber was added thereto, and the mixture was stirred at 300 rpm at 50°C for 3 h. After keeping the mixture warm for 1 h, the mixture was washed three times with water to obtain a 10% 18°SR viscose fiber suspension.
[0175] Adding 18°SR hardwood pulp and 18°SR softwood pulp into water respectively to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR softwood pulp suspension;
[0176] (2) grinding a 18°SR hardwood pulp suspension, a 18°SR softwood pulp suspension, and a 18°SR heat-resistant additive modified viscose fiber suspension, all of which have a mass percentage concentration of 10%, at 15,000 r, 15,000 r, and 20,000 r, respectively, using a PFI refiner to grind the hardwood pulp to a beating degree of 43°SR, the softwood pulp to a beating degree of 45°SR, and the heat-resistant additive modified viscose fiber to a beating degree of 50°SR;
[0177] After refining, the pulp suspension is prepared according to the ratio of hardwood pulp: coniferous pulp: heat-resistant additive modified viscose fiber = 4:4:2 (absolute dry mass ratio). The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0178] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0179] Comparative Example 3: Effect of Phase Change Heat Resistant Materials
[0180] The specific implementation method is the same as Example 1, except that the 5g of disodium hydrogen phosphate dodecahydrate in step (4) of Example 1 is adjusted to 2g of disodium hydrogen phosphate dodecahydrate, 1g of polyethylene glycol with a molecular weight of 600, 1g of polyethylene glycol with a molecular weight of 6000, and 1g of polyethylene glycol with a molecular weight of 10000.
[0181] Specifically:
[0182] (4) Add 2 g of disodium hydrogen phosphate dodecahydrate, 1 g of polyethylene glycol with a molecular weight of 600, 1 g of polyethylene glycol with a molecular weight of 6000, and 1 g of polyethylene glycol with a molecular weight of 10000 to 95 ml of water, add 5 g of charge reversal diatomaceous earth, stir at 600 rpm for 1 h at room temperature 25 ° C, wash three times and then dry. The drying conditions are: 60 ° C, 6 h, and temperature-resistant composite phase change materials are obtained.
[0183] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0184] Comparative Example 4: Effect of simultaneous high temperature modification of hardwood pulp, softwood pulp and Tencel fiber
[0185] The specific implementation is the same as that of Example 1, except that the adjustment steps (1) and (2) are as follows:
[0186] (1) adding 18°SR Tencel fiber into water, stirring at 300 rpm for 3 h at 50°C, keeping warm for 1 h, and washing with water three times to obtain a 10% 18°SR Tencel fiber suspension; adding 18°SR hardwood pulp and 18°SR coniferous pulp into water respectively to obtain a 10% 18°SR hardwood pulp suspension and a 10% 18°SR coniferous pulp suspension;
[0187] (2) The 18°SR hardwood pulp suspension, 18°SR coniferous pulp suspension and 18°SR Tencel fiber suspension prepared according to the above method with a mass percentage concentration of 10% were respectively ground by a PFI refiner at 15000r, 15000r and 20000r, and the final beating degree of the hardwood pulp was 43°SR, the coniferous pulp was 45°SR, and the Tencel fiber was 48°SR;
[0188] After refining, a pulp suspension is prepared according to the ratio of hardwood pulp: softwood pulp: tencel fiber = 4:4:2 (absolute dry mass ratio), and 3% of a high temperature resistant modification aid is added to the suspension. The 3% of the high temperature resistant modification aid is: 12g of the high temperature resistant aid is added to 388ml of water;
[0189] The papermaking process is 3000r / min speed for 5-10min, pressing pressure 0.4Mpa, pressing time 3min, drying temperature: 105℃, drying time 10min, paper weight 100g / m 2 , and obtain the second section of hollow paper stick base paper.
[0190] The other steps are carried out according to the method of Example 1 to prepare a low-retention high-temperature resistant hollow paper stick that can be used to heat cigarettes.
[0191] Example 13: Preparation of heated cigarettes
[0192] The tobacco segment, the self-made combined cooling segment, and the filter segment are connected in sequence by starch bonding to obtain a self-made heated cigarette; the self-made combined cooling segment is prepared by wrapping the low-retention and high-temperature-resistant hollow paper stick for heating cigarettes prepared in the embodiments and comparative examples on the outside of a spiral model with a thread spacing of 1.5 mm to obtain the self-made combined cooling segment.
[0193] Test results:
[0194] (1) Test results of Examples 1 to 3, Comparative Examples 1 to 2, and 4:
[0195] The flue gas temperature was tested respectively, and the specific data are shown in Table 1:
[0196] Table 1: Effect of reducing flue gas temperature
[0197] sample Flue gas temperature / ℃ iQOS e-cigarette sample (commercially available) 65 Example 1 53 Example 2 48 Example 3 42 Comparative Example 1 63 Comparative Example 2 56
[0198] It can be seen from Table 1 that as the amount of high temperature resistant additive increases, the effect of reducing flue gas temperature becomes better. At the same time, Tencel, as a regenerated cellulose fiber with good strength and hygroscopicity, has certain advantages over other regenerated cellulose fibers. It is worth noting that the hydrogen bonding effect of the modified paper in Comparative Example 4 is very poor, which leads to poor uniformity of the paper after papermaking, so no subsequent flue gas temperature test was performed, which also shows that the pulp cannot be modified as a whole, which will destroy the molding uniformity and paper strength.
[0199] (2) Test results of Examples 4 to 6:
[0200] Test flue gas temperature, see Table 2 for specific data:
[0201] Table 2: Effect of reducing flue gas temperature
[0202] sample Flue gas temperature / ℃ iQOS e-cigarette sample (commercially available) 65 Example 4 55 Example 5 50 Example 6 47
[0203] It can be seen from Table 2 that with the increase of the content of modified Tencel fiber, the effect of reducing the flue gas temperature is more obvious.
[0204] (3) The loading amount of phase change material on charge reversal diatomaceous earth and the flue gas temperature were tested. The specific data are shown in Table 3:
[0205] Table 3: Phase change material loading and flue gas temperature reduction effect
[0206]
[0207]
[0208] It can be seen from Table 3 that the increase in the amount of diatomite will increase the loading amount of the phase change material, which is conducive to reducing the flue gas temperature, but the stirring time has little effect on the loading amount of the phase change material. Therefore, under the premise that the total mass of the phase change material remains unchanged, increasing the type of phase change material will slightly increase the loading amount of the phase change material, and at the same time will significantly reduce the flue gas temperature.
[0209] (4) Test flue gas temperature. See Table 4 for specific data:
[0210] Table 4: Effect of reducing flue gas temperature
[0211] sample Flue gas temperature / ℃ iQOS e-cigarette sample (commercially available) 65 Embodiment 11 55 Example 12 46
[0212] It can be seen from Table 4 that the higher the proportion of the rapid cooling section of the hollow paper stick, the better the cooling effect.
[0213] (5) The above examples and comparative examples were subjected to sensory evaluation, and the evaluation criteria were based on the "YC / T415-2011 Sensory Evaluation Method for Tobacco Products":
[0214] Table 5: Sensory evaluation table of cigarette smoking quality
[0215]
[0216]
[0217] It can be seen from Table 5 that Example 12 and Comparative Example 3 have better effects, which proves that increasing the proportion of the rapid cooling section and mixing multiple types of phase change materials are not only beneficial to the cooling effect, but also improve the sensory quality of smoking cigarettes.
[0218] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a low-entrapment temperature-resistant hollow paper rod for heating cigarettes, It is characterized in that The method comprises the following steps: (1) mixing Tencel fiber with a beating degree of 18-50° SR and a high temperature resistant additive to obtain modified Tencel fiber; (2) mixing hardwood pulp with a beating degree of 30-60° SR, softwood pulp with a beating degree of 30-60° SR and the modified tencel fiber obtained in step (1) in a mass ratio of 3-4:3-5:4-1, and then making hollow paper stick base paper on a net to obtain a second section of hollow paper stick base paper; (3) adding water and a cationic auxiliary agent to diatomaceous earth and stirring to obtain charge-reversed diatomaceous earth; mixing the phase-change temperature-resistant material, water, and the charge-reversed diatomaceous earth to obtain a composite phase-change material; (4) mixing hardwood pulp with a beating degree of 30-60°SR, softwood pulp with a beating degree of 30-60°SR, and tencel fiber with a beating degree of 18-50°SR in a mass ratio of 3-4:3-5:4-1, adding the composite phase change material obtained in step (3), and making hollow paper stick base paper on a screen to obtain the first section of hollow paper stick base paper; (5) The first section of hollow paper stick base paper and the second section of hollow paper stick base paper are connected and combined by an adhesive to obtain a low-retention temperature-resistant hollow paper stick for heating cigarettes.
2. The method according to claim 1, It is characterized in that The high temperature resistant additive is one or more polymer materials containing phosphorus, boron, silicon and halogen element groups.
3. The method according to claim 1 or 2, It is characterized in that In step (1), the mass ratio of the tencel fiber to the high temperature resistant additive is 1:1-4; the mass percentage concentration of the high temperature resistant additive is 1%-5%; after mixing, stirring at 50-80°C and 300-600rpm for 3-6h, keeping warm for 1-2h, washing with water three times to obtain a modified tencel fiber suspension.
4. The method according to any one of claims 1 to 3, It is characterized in that In step (2) and step (4), the papermaking decomposition process is 3000r / min rotation speed for 5-10min, pressing pressure for 0.4Mpa, pressing time for 3min, and drying time at 105℃ for 10min.
5. The method according to any one of claims 1 to 4, It is characterized in that In step (3), the surface of the charge-reversed diatomaceous earth is positively charged, and the particle size is 5-250 mm; the cationic auxiliary agent is one or more of polyethylene imine, chitosan, cationic polyacrylamide, sodium carboxymethyl cellulose, and cationic starch; the mass ratio of the diatomaceous earth to water is 1:50-100; the mass ratio of the diatomaceous earth to the cationic auxiliary agent is 1:4-10; and the mixing is specifically: stirring at 600 rpm for 1-3 hours.
6. The method according to any one of claims 1 to 5, It is characterized in that In step (3), the phase-change heat-resistant material is one or more of polyethylene glycol with a molecular weight of 600, 1000, 2000, 6000, and 10000; the crystalline hydrated salt is one or more of magnesium chloride hexahydrate, magnesium nitrate hexahydrate, sodium thiosulfate pentahydrate, palladium hydroxide octahydrate, sodium sulfate decahydrate, calcium chloride hexahydrate, lithium perchlorate trihydrate, and disodium hydrogen phosphate dodecahydrate; the fatty acid is one or more of octadecanoic acid, hexadecanoic acid, tetradecanoic acid, and dodecanoic acid, and the fatty alcohol is one or more of dodecanol, tetradecanol, hexadecanol, pentaerythritol, and neopentyl glycol; the mass ratio of the phase-change heat-resistant material to the charge reversal diatomaceous earth is 1:1-4, and the reaction time is 1-3h; the mass ratio of the phase-change heat-resistant material to water is 1-5:50-100.
7. The method according to any one of claims 1 to 6, It is characterized in that In step (4), the amount of composite phase change material added is 5%-20%.
8. The method according to any one of claims 1 to 7, It is characterized in that In step (5), the first section of the hollow paper stick and the second section of the hollow paper stick are bonded at a length ratio of 3-7:7-3.
9. A low-retention, heat-resistant hollow paper rod for heating cigarettes prepared by the method according to any one of claims 1 to 8.
10. Use of the method according to any one of claims 1 to 8 or the low-entrapment heat-resistant hollow paper rod for heated cigarettes according to claim 9 in the preparation of heated cigarettes.
Citation Information
Patent Citations
Method for preparing tipping base paper containing tencel fibers
CN104294700A
Cigarette filter stick containing controlled-release spice core wire
CN106387994A
Flame-retardant lyocell filaments and preparation method thereof
CN113862807A
Silica gel cooling section for a product that heats tobacco without combustion
EA202300036A1
Compound phosphorus-nitrogen flame retardant, flame-retardant regenerated cellulose fiber, and preparation method
WO2024130910A1