Method for testing compression modulus of paper-based material impregnated with resin
By laying the paper-based material sample after impregnating the resin in the same direction, pressing and curing, and cutting it into standard samples, directly measuring the compression modulus of the paper-based material, it is solved that the inability to measure the paper-based material impregnated resin in the prior art is solved. The problem of post-compression modulus improves data accuracy and management capabilities of the production process.
Patent Information
- Application Number
- CN202411208742.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot directly measure the compression modulus in the direction of paper length or paper width after paper-based materials are impregnated with resin, and due to the brittleness of the material, there is a large data error in using tensile modulus instead of compression modulus.
By laying multiple paper-based material samples with the same size impregnated resin in the same direction, pressing and curing, cutting them into standard samples, and performing compression modulus tests according to the test standards, and directly measuring the paper-based material after impregnated resin The compression modulus avoids the impact of material brittleness.
Accurate measurement of the compression modulus of paper length or paper width direction after paper-based materials are impregnated with resin, improve data accuracy, avoid errors caused by material brittleness, provide more accurate process data, and enhance production process Control capability and product quality.
Smart Images

Figure CN119064104A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of material compression modulus testing, and in particular to a method for testing the compression modulus of a paper-based material after it is impregnated with resin. Background Art
[0002] High-performance new materials are the foundation and support for the development of high-end equipment such as aerospace and rail transit. Aramid honeycomb core materials have excellent characteristics such as high specific strength, high specific stiffness, wave transparency, good impact resistance and strong designability. They are one of the key lightweight materials in the fields of high-end equipment such as aerospace and rail transit. Aramid paper is one of the key raw materials for the preparation of aramid honeycomb core materials, which has excellent properties such as high tensile strength, good tear resistance, flame retardancy and high temperature resistance.
[0003] Dipping is a key step in preparing honeycombs from aramid paper. This step involves soaking the white honeycombs made from aramid paper in phenolic resin through equipment. For aramid paper, this is equivalent to coating the surface of the aramid paper with resin evenly, which is called aramid impregnated paper. The white honeycomb obtains a certain amount of glue during the dipping process, and the aramid paper increases quantitatively. After the curing process, the honeycomb pore wall is equivalent to an elastic thin plate, which is a brittle material with different tensile and compressive properties. At present, for aramid paper materials, most of them use tensile modulus instead of compression modulus. This method uses tensile modulus instead of compression modulus, but most paper-based materials are materials with different tensile and compressive properties, and direct substitution results in large data errors. Summary of the invention
[0004] (1) Technical issues to be solved
[0005] The present application provides a method for testing the compression modulus of a paper-based material after being impregnated with resin, which solves the current problem that the compression modulus of the paper length or paper width direction cannot be directly measured after the paper-based material is impregnated with resin.
[0006] (2) Technical solution
[0007] The present application provides a method for testing the compression modulus of a paper-based material after being impregnated with resin, comprising:
[0008] Laying down a plurality of paper-based material samples impregnated with resin and having the same size in the same direction to obtain a paper-based material impregnated board;
[0009] Pressing and curing the paper-based material impregnated board, and cutting the cured paper-based material impregnated board into standard samples;
[0010] The compression modulus test is performed on the standard sample according to the test standard to obtain the compression modulus of the paper-based material after being impregnated with resin.
[0011] Furthermore, before stacking a plurality of paper-based material samples impregnated with resin of the same size in the same direction to obtain a paper-based material impregnated board, the method further comprises:
[0012] The paper-based material is cut into a plurality of paper-based material samples of the same size, directions of the paper-based material samples are marked, and the paper-based material samples are impregnated with resin in the same direction.
[0013] Furthermore, the method of cutting the paper-based material into a plurality of paper-based material samples of the same size comprises:
[0014] Determining the number of sheets of the paper-based material sample to be cut according to the thickness of the paper-based material and the thickness of the standard sample;
[0015] The size of the paper-based material sample to be cut is determined according to the length and width of the standard sample.
[0016] Furthermore, the method of cutting the paper-based material into a plurality of paper-based material samples of the same size, marking the directions of the paper-based material samples, and impregnating the paper-based material samples with resin in the same direction, further comprises:
[0017] The paper-based material sample impregnated with resin is placed in a ventilated environment to remove the solvent in the paper-based material sample.
[0018] Furthermore, the ambient temperature for airing the paper-based material sample is 25°C±10°C, and the airing time is 24±6 hours.
[0019] Furthermore, the pressing and curing of the paper-based material impregnated board comprises:
[0020] Release material and air-permeable felt are respectively laid on the upper and lower surfaces of the paper-based material impregnated plate, and then the plate is put into a press for pressing and curing.
[0021] Furthermore, the pressure of the press is 0.3±0.1 MPa, the temperature is 180°C±5°C, and the insulation time is 2±0.5 hours.
[0022] Furthermore, the step of cutting the cured paper-based material impregnated board into standard samples comprises:
[0023] The cured paper-based material impregnated board is cut into standard samples after removing a certain size from the edge in the marked direction.
[0024] Furthermore, the paper-based material is any one of aramid paper, kraft paper, and insulating paper.
[0025] Furthermore, the resin is a solution of a uniform mixture of resin base and a dilution solvent, the dilution solvent is one or more of alcohol, ethyl acetate, DMSO, DMAC, and DMF, and the resin base is one or more of phenolic resin, epoxy resin, polyimide resin, and bismaleimide resin.
[0026] (3) Beneficial effects
[0027] The above technical solution of the present application has the following advantages:
[0028] The present application provides a method for testing the compression modulus of a paper-based material after being impregnated with resin. The method comprises the following steps: stacking a plurality of paper-based material samples impregnated with resin of the same size in the same direction to obtain a paper-based material impregnated board, and then pressing and curing the paper-based material impregnated board. The cured paper-based material impregnated board has a certain thickness, and its strength is improved relative to that of a single paper-based material. The cured paper-based material impregnated board is cut into standard samples, and then a compression modulus test is performed on the standard samples according to the test standard. The compression modulus of the paper-based material in the length or width direction of the paper after being impregnated with resin can be directly measured, and the influence caused by the brittleness of the material can be effectively avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0030] Figure 1 A flow chart of a method for testing the compression modulus of a paper-based material after being impregnated with resin provided in the present application;
[0031] Figure 2 A schematic diagram of paper-based material samples provided in this application being stacked in the same direction;
[0032] Figure 3 This is a schematic diagram of cutting the impregnated board of the paper-based material after curing provided in the present application. DETAILED DESCRIPTION
[0033] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present application.
[0034] It should be understood that when used in the present specification and the appended claims, the term "comprising" indicates the presence of described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.
[0035] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.
[0036] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways. "Multiple" means "two or more".
[0037] At present, the methods for testing the compression modulus of thin sheet materials mainly include macro measurement method, pressure plate method, and elastic film method. For aramid paper materials, most of them use tensile modulus instead of compression modulus. The tensile modulus substitution method uses tensile modulus to replace compression modulus, but most paper-based materials are materials with different properties in tension and compression, and direct substitution has large data errors. The pressure plate method and elastic film method measure the compression modulus of the film in the z direction (height direction), and cannot complete the compression modulus test in the length or width direction. The macro measurement method places the material sample in a tension-compression testing machine, first applies a certain tensile force, then applies a certain compressive force, measures the strain and stress of the material, and thus calculates the compression modulus, but some paper-based materials such as aramid paper and kraft paper are brittle materials after being impregnated with resin, which is not suitable for this method.
[0038] In response to the above problems, the present application provides a method for testing the compression modulus of a paper-based material after being impregnated with resin, which can be used for paper-based and paper-based composite materials to help obtain the accurate compression modulus of the paper-based material after being impregnated with resin. The compression modulus of the paper-based material in the length or width direction of the paper after being impregnated with resin can be directly measured, and the influence of the brittleness of the material can be effectively avoided.
[0039] The specific implementation methods of the present application are further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present application but are not intended to limit the scope of the present application.
[0040] like Figure 1 As shown, the method for testing the compression modulus of a paper-based material after being impregnated with resin provided in an embodiment of the present application specifically comprises the following steps: stacking a plurality of paper-based material samples impregnated with resin of the same size in the same direction to obtain a paper-based material impregnated board; pressing and curing the paper-based material impregnated board, and cutting the cured paper-based material impregnated board into standard specimens; and performing a compression modulus test on the standard specimens according to the test standard to obtain the compression modulus of the paper-based material after being impregnated with resin.
[0041] The test method for the compression modulus of a paper-based material after being impregnated with resin provided in an embodiment of the present application is that a plurality of paper-based material samples impregnated with resin of the same size are stacked in the same direction to obtain a paper-based material impregnated board, and the paper-based material impregnated board is then pressed and solidified. The solidified paper-based material impregnated board has a certain thickness, and its strength is improved compared to a single paper-based material. The solidified paper-based material impregnated board is cut into standard samples, and then a compression modulus test is performed on the standard samples according to the test standard. The compression modulus of the paper-based material in the length or width direction of the paper after being impregnated with resin can be directly measured, and the influence caused by the brittleness of the material is effectively avoided.
[0042] This application can accurately obtain the compression modulus of thin paper-based materials, which greatly improves data accuracy compared to using tensile modulus instead, and provides more accurate process data for honeycomb production and manufacturing. This test method is simple and practical, and can effectively improve the production process control capabilities and enhance product quality.
[0043] In some embodiments, before stacking multiple resin-impregnated paper-based material samples of the same size in the same direction to obtain a paper-based material impregnated board, the process further includes: cutting the paper-based material into multiple paper-based material samples of the same size, marking directions of the paper-based material samples, and impregnating resin in the same direction.
[0044] In some embodiments, cutting the paper-based material into multiple paper-based material samples of the same size includes: determining the number of paper-based material samples to be cut according to the thickness of the paper-based material and the thickness of the standard sample; and determining the size of the paper-based material samples to be cut according to the length and width of the standard sample.
[0045] In some embodiments, the method of cutting the paper-based material into multiple paper-based material samples of the same size, marking the directions of the paper-based material samples, and impregnating the paper-based material samples with resin in the same direction also includes: placing the paper-based material samples impregnated with resin in a ventilated environment to remove the solvent in the paper-based material samples.
[0046] In some embodiments, the ambient temperature for airing the paper-based material sample is 25° C.±10° C., and the airing time is 24±6 hours.
[0047] In some embodiments, pressing and curing the paper-based material impregnated board includes: laying a demoulding material and a breathable felt on the upper and lower surfaces of the paper-based material impregnated board respectively, and then placing the board in a press for pressing and curing.
[0048] In some embodiments, the pressure of the press is 0.3±0.1 MPa, the temperature is 180°C±5°C, and the holding time is 2±0.5 hours.
[0049] In some embodiments, cutting the cured paper-based material impregnated board into standard samples includes: removing a certain size from the edge of the cured paper-based material impregnated board in a marked direction and then cutting the board into standard samples.
[0050] In some embodiments, the paper-based material is any one of aramid paper, kraft paper, and insulating paper.
[0051] In some embodiments, the resin is a solution of a uniform mixture of a resin base and a dilution solvent, the dilution solvent is one or more of alcohol, ethyl acetate, DMSO, DMAC, and DMF, and the resin base is one or more of a phenolic resin, an epoxy resin, a polyimide resin, and a bismaleimide resin.
[0052] The method for testing the compression modulus of a paper-based material after being impregnated with resin provided in an embodiment of the present application mainly comprises the following steps: impregnating the paper-based material with resin, airing, stacking, pressing and curing, cutting, and testing.
[0053] Taking 0.05mm thick aramid paper impregnated with phenolic resin as an example, the specific operation is as follows: Impregnation of paper-based material with resin: Cut 40 100mm*100mm size samples from the aramid paper, mark the direction, and impregnate the phenolic resin in the same direction. Airing: Hang the impregnated aramid paper at room temperature or less than 40℃ to remove the solvent in the aramid paper. Stacking: Stack the aired aramid paper layer by layer according to the direction, such as Figure 2 Pressing and curing: Place release material and breathable felt on the upper and lower surfaces of the stacked aramid impregnated boards, respectively, and place them in a press for pressing and curing. Cutting: Remove 15mm from the edge of the pressed aramid impregnated boards in the marked direction and cut them into standard specimens of 50.8mm*12.7mm*3mm, as shown in the figure below. Figure 3 Test: Test according to material testing standards to obtain the compression modulus of aramid impregnated paper.
[0054] The minimum number of cut samples can be calculated based on the thickness of the paper-based material and the thickness of the standard sample. The number of cut samples ≥ the standard sample thickness / (paper-based material thickness + 0.05mm); the size of the cut sample is calculated based on the length and width of the standard sample. The length of the cut sample ≥ the length of the standard sample + 25mm, and the width of the cut sample ≥ the width of the standard sample + 25mm. The paper-based material can be aramid paper, kraft paper, insulation paper or other paper structure materials. The impregnated resin can be one or more of liquid phenolic resin, epoxy resin, polyimide resin, and bismaleimide resin. Determine the appropriate curing parameters according to the selected resin type, and choose to cut different test sizes according to different test standards.
[0055] The test method for the compression modulus of the paper-based material after impregnation with resin provided in the embodiment of the present application can be used to measure the compression modulus of the paper-based material in the length or width direction of the paper after impregnation with resin, helping to obtain the accurate compression modulus of the paper-based material after impregnation with resin, and effectively avoiding the influence of the brittleness of the material.
[0056] The following is an explanation through specific embodiments.
[0057] Example 1
[0058] Cut 20 aramid paper samples of 100mm*100mm size, impregnate them with alcohol-soluble phenolic resin after marking the direction, hang them in a ventilated environment at 25℃±5℃ for 24 hours after impregnation, take them out after air-drying, and stack them in the marked direction. After stacking, cover the upper and lower surfaces with demoulding materials and breathable felt respectively. According to the characteristics of phenolic resin, set the press pressure to 0.3MPa, the temperature to 180℃±5℃, and the insulation time to 2 hours. Remove 15mm from the edge of the pressed aramid impregnated board in the marked direction and cut it into 50.8mm*12.7mm*3mm standard specimens for testing. The compression modulus data of the aramid impregnated paper is 4.10MPa.
[0059] Example 2
[0060] Cut 30 aramid paper samples of 100mm*100mm size, impregnate them with alcohol-soluble phenolic resin after marking the direction, hang them in a ventilated environment at 25℃±5℃ for 24 hours after impregnation, take them out after air-drying, and stack them in the marked direction. After stacking, cover the upper and lower surfaces with demoulding materials and breathable felt respectively. According to the characteristics of phenolic resin, set the press pressure to 0.3MPa, the temperature to 180℃±5℃, and the insulation time to 2 hours. Remove 15mm from the edge of the pressed aramid impregnated board in the marked direction and cut it into 50.8mm*12.7mm*3mm standard specimens for testing. The compression modulus data of the aramid impregnated paper is 4.30MPa.
[0061] Example 3
[0062] Cut 40 aramid paper samples of 100mm*100mm size, impregnate them with alcohol-soluble phenolic resin after marking the direction, hang them in a ventilated environment at 25℃±5℃ for 24 hours after impregnation, take them out after air-drying, and stack them in the marked direction. After stacking, cover the upper and lower surfaces with demoulding materials and breathable felt respectively. According to the characteristics of phenolic resin, set the press pressure to 0.3MPa, the temperature to 180℃±5℃, and the insulation time to 2 hours. Remove 15mm from the edge of the pressed aramid impregnated board in the marked direction and cut it into 50.8mm*12.7mm*3mm standard specimens for testing. The compression modulus data of the aramid impregnated paper is 4.35MPa.
[0063] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for testing the compression modulus of a paper-based material after being impregnated with resin, characterized in that: include: Laying down a plurality of paper-based material samples impregnated with resin and having the same size in the same direction to obtain a paper-based material impregnated board; Pressing and curing the paper-based material impregnated board, and cutting the cured paper-based material impregnated board into standard samples; The compression modulus test is performed on the standard sample according to the test standard to obtain the compression modulus of the paper-based material after being impregnated with resin.
2. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 1, characterized in that: Before stacking a plurality of paper-based material samples impregnated with resin of the same size in the same direction to obtain a paper-based material impregnated board, the method further comprises: The paper-based material is cut into a plurality of paper-based material samples of the same size, directions of the paper-based material samples are marked, and the paper-based material samples are impregnated with resin in the same direction.
3. The method for testing the compression modulus of a paper-based material after being impregnated with resin as claimed in claim 2, characterized in that: The method of cutting the paper-based material into a plurality of paper-based material samples of the same size comprises: Determining the number of sheets of the paper-based material sample to be cut according to the thickness of the paper-based material and the thickness of the standard sample; The size of the paper-based material sample to be cut is determined according to the length and width of the standard sample.
4. The method for testing the compression modulus of a paper-based material after being impregnated with resin as claimed in claim 2, characterized in that: The method further comprises: cutting the paper-based material into a plurality of paper-based material samples of the same size, marking directions of the paper-based material samples, and impregnating the paper-based material samples with resin in the same direction; The paper-based material sample impregnated with resin is placed in a ventilated environment to remove the solvent in the paper-based material sample.
5. The method for testing the compression modulus of a paper-based material after being impregnated with resin as claimed in claim 4, characterized in that: The ambient temperature for airing the paper-based material sample is 25° C.±10° C., and the airing time is 24±6 hours.
6. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 1, characterized in that: The pressing and curing of the paper-based material impregnated board comprises: Release material and air-permeable felt are respectively laid on the upper and lower surfaces of the paper-based material impregnated plate, and then the plate is put into a press for pressing and curing.
7. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 6, characterized in that: The pressure of the press is 0.3±0.1 MPa, the temperature is 180°C±5°C, and the insulation time is 2±0.5 hours.
8. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 1, characterized in that: The method of cutting the cured paper-based material impregnated board into standard samples comprises: The cured paper-based material impregnated board is cut into standard samples after removing a certain size from the edge in the marked direction.
9. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 1, characterized in that: The paper-based material is any one of aramid paper, kraft paper and insulating paper.
10. The method for testing the compression modulus of a paper-based material after being impregnated with resin according to claim 1, characterized in that: The resin is a uniformly mixed solution of resin base and dilution solvent, the dilution solvent is one or more of alcohol, ethyl acetate, DMSO, DMAC, and DMF, and the resin base is one or more of phenolic resin, epoxy resin, polyimide resin, and bismaleimide resin.
Citation Information
Patent Citations
Sample preparation method for testing inter-laminar shear performance of carbon fiber composite material
CN101968409A
Preparation method of high-strength lightweight composite honeycomb panel
CN107718849A
Testing method of in-plane compression mechanical properties of aramid paper
CN109855968A
Special aramid paper for aramid paper honeycomb and preparation method of special aramid paper
CN114211847A
Method, device and equipment for testing in-plane compression modulus and storage medium
CN117804903A