Method for testing fracture toughness of fiber reinforced ceramic matrix composite material

Through the combination of in-situ three-point bending test and finite element simulation, the problem of fracture toughness prediction of fiber-reinforced ceramic matrix composite materials is solved, and the impact of crack deflection and microstructure is considered, which improves the accuracy of fracture toughness testing. and effectiveness.

CN119064180AActive Publication Date: 2024-12-03SUN YAT SEN UNIV

Patent Information

Application Number
CN202411166138.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The prior art is difficult to accurately predict the fracture toughness of fiber-reinforced ceramic matrix composites, especially because crack deflection increases the difficulty of testing, and conventional testing methods cannot fully consider the influence of microstructure and interlayer lateral cracking behavior, resulting in fracture toughness. The prediction accuracy is low.

Method used

In-situ three-point bending test combined with finite element simulation method, load-head displacement curve is recorded in real time through fixed displacement control, lateral crack initiation and expansion are observed, finite element model with prefabricated cracks is established, appropriate boundary conditions are set and Mesh division, calculate the energy release rate and stress intensity factor, draw the stress intensity factor-displacement load curve, and obtain fracture toughness data.

Benefits of technology

Through the method of combining in-situ mechanical testing with finite element simulation, the microstructure and interlayer lateral cracking behavior are fully considered, and the fracture toughness of ceramic matrix composite materials is more accurately predicted, which improves the effectiveness and rationality of fracture toughness testing. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064180A_ABST
    Figure CN119064180A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material fracture toughness testing, in particular to a method for testing fracture toughness of a fiber-reinforced ceramic-based composite material. According to the invention, the fact observation of the whole crack initiation and propagation process of the ceramic-based composite material under the action of external load is realized through an in-situ mechanical test technology, and microscopic test data is provided for the test of fracture toughness; then in-situ test and finite element simulation are combined, the influence of a microstructure and interlayer transverse cracking behaviors on the overall fracture toughness of the ceramic matrix composite is fully considered, and the effectiveness and rationality of fracture toughness prediction are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material fracture toughness testing, and in particular to a method for testing the fracture toughness of a fiber-reinforced ceramic-based composite material. Background Art

[0002] Ceramic matrix composites refer to composite materials with continuous fibers as reinforcement and ceramic materials as matrix. Ceramic matrix composites have excellent properties such as high specific strength, high temperature resistance, oxidation resistance, and corrosion resistance. They have been widely used in high temperature extreme environments such as aerospace hot end components and hypersonic aircraft. The mechanical properties and cracking behavior of fiber-reinforced ceramic matrix composites under external loads are closely related to their microstructures. The volume proportion and distribution of fibers, the interfacial bonding between fibers and the matrix, the porosity of the preform, and the residual stress will affect the crack propagation path of ceramic matrix composites, thus increasing the difficulty of fracture toughness testing of ceramic matrix composites. Unlike general ceramic materials where the main cracks extend in the direction perpendicular to the load, the two-dimensional woven fiber-reinforced ceramic matrix composites have weak interfacial bonding between the fibers and the matrix, so the vertical main crack extension is prone to deflection under external loads, and will extend laterally along the interface when reaching the fiber-matrix interface. For three-dimensional piercing fiber reinforced ceramic matrix composites, when the main crack deflects and expands along the fiber-matrix interface under external load, its longitudinal fibers will hinder the further expansion of the interface crack, causing the crack to deflect again and expand along the longitudinal fiber and matrix interface. It can be seen that the deflection phenomenon of the main crack brings technical difficulties to the prediction of the overall fracture toughness of two-dimensional and three-dimensional fiber reinforced ceramic matrix composites. However, conventional fracture toughness test methods for ceramic matrix composites include double cantilever beam method, three-point bending method, single-sided notch beam method, indentation method, etc., which are more suitable for ceramic or metal materials with isotropic microstructures, and cannot fully consider the influence of microstructure and interlayer transverse cracking behavior on the overall fracture toughness of ceramic matrix composites, resulting in low fracture toughness prediction accuracy. At present, there is no effective experimental method and mathematical model that can reasonably consider the influence of crack deflection on the overall fracture toughness of ceramic matrix composites. Summary of the invention

[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for testing the fracture toughness of fiber-reinforced ceramic matrix composites, which takes into account the influence of crack deflection on the overall fracture toughness of the ceramic matrix composite material, so as to make the test results more reasonable and accurate.

[0004] Based on the above purpose, the technical solution adopted by the present invention is as follows:

[0005] A method for testing the fracture toughness of a fiber-reinforced ceramic matrix composite material, characterized in that the method comprises the following steps:

[0006] Referring to GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics", a single-side notched beam three-point bending test specimen was prepared, recorded as the first specimen, and an in-situ three-point bending test was carried out until the first specimen broke. During the test, a fixed displacement was used to control the loading, and the load-indenter displacement curve was recorded in real time. The crack tip of the prefabricated crack and its vicinity were observed to obtain the load and indenter displacement P corresponding to the initiation of the transverse crack, the indenter displacement Q corresponding to the maximum load, and the functional relationship between the indenter displacement and the transverse crack length or the transverse crack length at different indenter displacements, wherein the material of the first specimen is a two-dimensional woven fiber reinforced ceramic matrix composite material;

[0007] A finite element model with prefabricated cracks was established in the finite element software. The constructed specimen was recorded as the second specimen and the following conditions were set:

[0008] The material of the second sample is a purely elastic isotropic homogeneous material. Input the elastic modulus and Poisson's ratio.

[0009] A rigid indenter is set above the second specimen and displacement boundary conditions are used to control the downward pressure behavior. Two rigid rollers are set below to support and fix the movement of the second specimen in all directions. There is no friction between the second specimen and the rollers and indenter, and the face-to-face contact conditions are all hard contact.

[0010] The length, width, height, chamfer, prefabricated crack depth and cut width, lower span, roller diameter, indenter loading rate and test temperature of the second specimen are consistent with those of the in-situ three-point bending test.

[0011] When the indenter displacement reaches the value of the indenter displacement P, the vertical crack is deflected into a transverse crack, and according to the in-situ three-point bending test, a functional relationship between the indenter displacement and the transverse crack length or the transverse crack length at different indenter displacements is set, and loading is stopped when the indenter pressing depth increases linearly to a depth D;

[0012] Draw 5-10 layers of loop grids at the crack tip, where the circle of grids closest to the crack tip is set as a singular unit grid, solve the J integral of each layer of grids by the contour integration method, and then obtain the energy release rate and stress intensity factor, and draw the stress intensity factor-displacement load curve. The stress intensity factor corresponding to the indenter displacement Q in the curve is the fracture toughness;

[0013] The depth D is greater than the indenter displacement Q.

[0014] In the present invention, energy release rate = sum of J integrals of each layer of loop grids / total number of layers of loop grids.

[0015] The method uses in-situ mechanical testing technology to achieve actual observation of the entire process of crack initiation and expansion of ceramic-based composite materials under external loads, providing microscopic test data for the test of fracture toughness; based on a method combining in-situ testing with finite element simulation, it fully considers the influence of microstructure and interlaminar transverse cracking behavior on the overall fracture toughness of ceramic-based composite materials, greatly improving the effectiveness and rationality of fracture toughness prediction.

[0016] Preferably, 0.1 mm ≤ the depth D - the maximum indenter displacement Q ≤ 0.3 mm.

[0017] Preferably, the stress intensity factor is calculated according to formula (1):

[0018]

[0019] Among them, K eff is the stress intensity factor, in MPa*m 1 / 2 ;

[0020] E Y is the elastic modulus, in MPa;

[0021] v is Poisson’s ratio;

[0022] G is the energy release factor, the unit is J / m 2 It should be noted that, because the interface crack extension is a mixed extension mode, the stress intensity factor here is the equivalent stress intensity factor. Formula (1) mainly considers the influence of mode II cracking.

[0023] Preferably, when establishing a finite element model containing prefabricated cracks, the lengths of the transverse cracks at different indenter displacements are set, and the set indenter displacements include at least one indenter displacement greater than the indenter displacement Q.

[0024] Preferably, the first specimen is 18 mm long, 3 mm wide, 4 mm high, with a chamfer of 0.12 mm and a roughness of 0.2 μm. A wire saw is used to preform cracks, the cracks are located in the middle of the length direction of the first specimen, the lower surface is the tensile surface, the preformed crack depth is 2 mm, the incision width is 0.1 mm, the lower span is 16 mm, and the roller diameter is 4 mm.

[0025] Preferably, in the in-situ three-point bending test, a 10N preload is applied before loading for sample positioning and fixation; displacement-controlled loading is adopted, and the loading rate is 0.002mm / s; and the test temperature is 25-1300°C.

[0026] Preferably, the two-dimensional woven fiber-reinforced ceramic matrix composite material includes at least one of a carbon fiber-reinforced ceramic matrix composite material or a silicon carbide fiber-reinforced ceramic matrix composite material.

[0027] Preferably, the material of the first sample is a three-dimensional puncture fiber reinforced ceramic matrix composite material;

[0028] According to the in-situ three-point bending test, the corresponding indenter displacement L when the transverse crack is blocked is also obtained;

[0029] In the process of establishing the finite element model containing the prefabricated cracks, it is also set that when the displacement of the indenter reaches the value of the displacement L of the indenter, the transverse crack is blocked.

[0030] Preferably, the three-dimensional puncture fiber reinforced ceramic matrix composite material comprises a silicon carbide fiber reinforced ceramic matrix composite material.

[0031] In the present invention, during the in-situ three-point bending test, for two-dimensional woven fiber-reinforced ceramic matrix composites, the focus is on the transverse crack initiation and propagation process of the main crack being transversely deflected and along the fiber-matrix interface; for three-dimensional piercing fiber-reinforced ceramic matrix composites, in addition to focusing on the transverse crack initiation and propagation process of the main crack being transversely deflected and along the fiber-matrix interface, the focus is also on the process of the longitudinal fibers causing the transverse crack to undergo secondary deflection and changing the crack propagation path.

[0032] Preferably, the finite element software is ABAQUS or ANASYS.

[0033] Preferably, the in-situ three-point bending test is carried out on an in-situ mechanical testing system equipped with a scanning electron microscope or a high-power optical microscope.

[0034] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention realizes the actual observation of the whole process of crack initiation and expansion of ceramic-based composite materials under external load through in-situ mechanical testing technology, and provides microscopic test data for the test of fracture toughness; based on the method combining in-situ test with finite element simulation, the influence of microstructure and interlaminar transverse cracking behavior on the overall fracture toughness of ceramic-based composite materials is fully considered, which greatly improves the effectiveness and rationality of fracture toughness prediction. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A flow chart of a method for testing the fracture toughness of a fiber-reinforced ceramic matrix composite material according to the present invention;

[0036] Figure 2 The finite element model of Example a, (a) three-point bending finite element model with longitudinal pre-cracks and no interface cracking, (b) finite element mesh division;

[0037] Figure 3The finite element models of cases b and c are: (a) the three-point bending finite element geometric model with a transverse deflection interface crack, where the crack propagates transversely along the interface; (b) the three-point bending finite element geometric model with a transverse deflection interface crack blocked, where the crack stops propagating transversely when it reaches the longitudinal fiber;

[0038] Figure 4 Finite element geometric model and mesh generation for 2D-SiCf / SiC composites with interface cracks of different lengths;

[0039] Figure 5 are the functional relationship curves of stress intensity factor and displacement load in three finite element models, corresponding to example a-1, example b-1 and example c-1 respectively;

[0040] Figure 6 The fracture toughness prediction results of ceramic matrix composites with different preform structures at room temperature (25℃) and high temperature (1300℃). DETAILED DESCRIPTION

[0041] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0042] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial sources. The components and raw materials used in each parallel experiment are all of the same kind.

[0043] Calculation example a-1

[0044] Step 1: Prepare a single-side notched beam three-point bending test specimen according to GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics", which is recorded as the first specimen. The first specimen has a length of 18 mm, a width of 3 mm, a height of 4 mm, a chamfer of 0.12 mm, and a roughness of 0.2 μm. Use a wire saw to preform a crack, the crack is located in the middle of the length direction of the specimen, the lower surface is the tensile surface, the preformed crack depth is 2 mm, the notch width is 0.1 mm, and the span is 16 mm. The roller diameter is 4 mm, and the first specimen material is 2D-SiC f / SiC.

[0045] Step 2: Carry out an in-situ three-point bending test at room temperature (25°C, the same below) on an in-situ mechanical testing system equipped with a scanning electron microscope or a high-power optical microscope. Before loading, apply a 10N preload force for positioning and fixing the first sample. During loading, use a fixed displacement to control loading, and the loading rate is 0.002mm / s. During the test, record the load-indenter displacement curve in real time, and while loading, use a scanning electron microscope or a high-power optical microscope to observe the crack tip of the prefabricated crack and its surrounding area in situ, record the entire process of crack initiation and expansion, and obtain the corresponding indenter displacement Q when the load reaches the maximum value. When the sample breaks, the test ends, where the indenter displacement Q = 0.24mm.

[0046] Step 3: Based on the in-situ test results, a finite element model with prefabricated cracks and no interface transverse cracking is established in the finite element software ABAQUS (such as Figure 2 The constructed sample is recorded as the second sample and the following conditions are set:

[0047] The material of the second sample is a pure elastic isotropic homogeneous material with an input elastic modulus of 100 GPa and a Poisson's ratio of 0.1.

[0048] A rigid indenter is set above the second specimen and displacement boundary conditions are used to control the downward pressure behavior. Two rigid rollers are set below to support and fix the movement of the second specimen in all directions. There is no friction between the second specimen and the rollers and indenter, and the face-to-face contact conditions are all hard contact.

[0049] The length, width, height, chamfer, prefabricated crack depth and cut width, lower span, roller diameter, indenter loading rate and test temperature of the second specimen are consistent with those of the in-situ three-point bending test.

[0050] When the pressing depth of the indenter increases linearly to the depth D, the loading is stopped, where the depth D is 0.4 mm;

[0051] The above software is used to automatically draw 8 layers of loop mesh at the crack tip, among which the circle of mesh closest to the crack tip is set as a singular unit mesh. The J integral of each layer of mesh is automatically solved by the contour integration method. The average value of the 8 J integrals obtained under the same displacement load is the energy release rate under the displacement load. Then, the stress intensity factor under the displacement load is automatically calculated according to equations (1) and (2):

[0052]

[0053] Among them, K eff is the stress intensity factor, in MPa*m 1 / 2 ,

[0054] E Y is the elastic modulus, in MPa,

[0055] v is Poisson's ratio,

[0056] G is the energy release factor, the unit is J / m 2 ,

[0057] Automatically plot stress intensity factor-displacement load curves.

[0058] Step 4: The stress intensity factor corresponding to the above-mentioned indenter displacement Q in the stress intensity factor-displacement load curve is the fracture toughness.

[0059] Example b-1

[0060] Step 1: Prepare a single-side notched beam three-point bending test specimen according to GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics", which is recorded as the first specimen. The dimensions of the first specimen are 18 mm long, 3 mm wide, 4 mm high, 0.12 mm chamfer, and 0.2 μm roughness. Use a wire saw to preform a crack, the crack is located in the middle of the length direction of the specimen, the lower surface is the tensile surface, the preformed crack depth is 2 mm, the notch width is 0.1 mm, and the span is 16 mm. The roller diameter is 4 mm, and the material of the first specimen is 2D-SiC f / SiC.

[0061] Step 2: Carry out an in-situ three-point bending test at room temperature on an in-situ mechanical testing system equipped with a scanning electron microscope or a high-power optical microscope. Before loading, apply a 10N preload to position and fix the first sample. During loading, use a fixed displacement to control loading, and the loading rate is 0.002mm / s. During the test, record the load-indenter displacement curve in real time, and while loading, use a scanning electron microscope or a high-power optical microscope to observe the crack tip of the prefabricated crack and its surrounding area in situ, record the entire process of crack initiation and expansion, and obtain the corresponding indenter displacement P when the transverse crack initiates, the corresponding indenter displacement Q when the load reaches the maximum value, and the length of the transverse crack at different indenter displacements. When the sample breaks, the test ends, where the indenter displacement P = 0.074mm, and the indenter displacement Q = 0.24mm.

[0062] Step 3: Based on the in-situ test results, a finite element model with interface transverse cracking was established in the finite element software ABAQUS (such as Figure 3 The constructed sample is recorded as the second sample and the following conditions are set:

[0063] The material of the second sample is a pure elastic isotropic homogeneous material with an input elastic modulus of 100 GPa and a Poisson's ratio of 0.1.

[0064] A rigid indenter is set above the second specimen and displacement boundary conditions are used to control the downward pressure behavior. Two rigid rollers are set below to support and fix the movement of the second specimen in all directions. There is no friction between the second specimen and the rollers and indenter, and the face-to-face contact conditions are all hard contact.

[0065] The length, width, height, chamfer, prefabricated crack depth and cut width, lower span, roller diameter, indenter loading rate and test temperature of the second specimen are consistent with those of the in-situ three-point bending test.

[0066] When the indenter displacement reaches the value of the indenter displacement P, the vertical crack is deflected into a transverse crack (i.e., transverse crack initiation occurs, the same below), and the length of the transverse crack at different indenter displacements is set according to the above in-situ three-point bending test results, specifically:

[0067] When the pressing distance of the indenter (i.e., the displacement of the indenter, the same below) is 0.08 mm, the transverse crack length is about 0.25 mm;

[0068] When the pressing distance of the indenter is 0.11 mm, the transverse crack length is about 0.55 mm;

[0069] When the pressing distance of the indenter is 0.18 mm, the transverse crack length is about 0.75 mm;

[0070] When the pressing distance of the indenter is 0.23 mm, the transverse crack length is about 1.0 mm;

[0071] When the pressing distance of the indenter is 0.3 mm, the length of the transverse crack is about 1.5 mm.

[0072] And it is set to stop loading when the pressing depth of the pressure head increases linearly to the depth D, where the depth D is 0.4mm.

[0073] The above software is used to automatically draw 8 layers of loop mesh at the crack tip, among which the circle of mesh closest to the crack tip is set as a singular unit mesh. The J integral of each layer of mesh is automatically solved by the contour integration method. The average value of the 8 J integrals obtained under the same displacement load is the energy release rate under the displacement load. Then, the stress intensity factor under the displacement load is automatically calculated according to equations (1) and (2):

[0074]

[0075] Among them, K eff is the stress intensity factor, in MPa*m 1 / 2 ,

[0076] E Y is the elastic modulus, in MPa,

[0077] v is Poisson's ratio,

[0078] G is the energy release factor, the unit is J / m 2 ,

[0079] Automatically plot stress intensity factor-displacement load curves.

[0080] Step 4: The stress intensity factor corresponding to the above-mentioned indenter displacement Q in the stress intensity factor-displacement load curve is the fracture toughness.

[0081] Example c-1

[0082] Step 1: Prepare a single-side notched beam three-point bending test specimen according to GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics", which is recorded as the first specimen. The dimensions of the first specimen are 18 mm long, 3 mm wide, 4 mm high, 0.12 mm chamfer, and 0.2 μm roughness. Use a wire saw to preform a crack, the crack is located in the middle of the length direction of the specimen, the lower surface is the tensile surface, the preformed crack depth is 2 mm, the notch width is 0.1 mm, and the span is 16 mm. The roller diameter is 4 mm, and the material of the first specimen is 3D-SiC f / SiC.

[0083] Step 2: Carry out an in-situ three-point bending test at room temperature on an in-situ mechanical testing system equipped with a scanning electron microscope or a high-power optical microscope. Before loading, apply a 10N preload to position and fix the first sample. During loading, use a fixed displacement to control loading, and the loading rate is 0.002mm / s. During the test, record the load-indenter displacement curve in real time, and while loading, use a scanning electron microscope or a high-power optical microscope to observe the crack tip of the prefabricated crack and its surrounding area in situ, record the entire process of crack initiation and expansion, and obtain the corresponding indenter displacement P when the transverse crack is initiated, the corresponding indenter displacement L when the transverse crack is blocked, the corresponding indenter displacement Q when the load reaches the maximum value, and the length of the transverse crack at different indenter displacements. When the sample breaks, the test ends, where the indenter displacement P = 0.074mm, the indenter displacement L = 0.110mm, and the indenter displacement Q = 0.195mm.

[0084] Step 3: Based on the in-situ test results, a finite element model of the interface with transverse cracking obstruction was established in the finite element software ABAQUS (such as Figure 4 The constructed sample is recorded as the second sample and the following conditions are set:

[0085] The material of the second sample is a pure elastic isotropic homogeneous material with an input elastic modulus of 100 GPa and a Poisson's ratio of 0.1.

[0086] A rigid indenter is set above the second specimen and displacement boundary conditions are used to control the downward pressure behavior. Two rigid rollers are set below to support and fix the movement of the second specimen in all directions. There is no friction between the second specimen and the rollers and indenter, and the face-to-face contact conditions are all hard contact.

[0087] The length, width, height, chamfer, prefabricated crack depth and cut width, lower span, roller diameter, indenter loading rate and test temperature of the second specimen are consistent with those of the in-situ three-point bending test.

[0088] When the indenter displacement reaches the value of the indenter displacement P, the vertical crack is deflected into a transverse crack, and the length of the transverse crack at different indenter displacements is set according to the above in-situ three-point bending test results, specifically:

[0089] When the pressing distance of the indenter is 0.08 mm, the transverse crack length is about 0.25 mm;

[0090] When the pressing distance of the indenter is 0.11 mm, the transverse crack length is about 0.55 mm;

[0091] When the pressing distance of the indenter is 0.18 mm, the transverse crack length is about 0.55 mm;

[0092] When the pressing distance of the indenter is 0.23 mm, the transverse crack length is about 0.55 mm;

[0093] When the pressing distance of the indenter is 0.3 mm, the length of the transverse crack is about 0.55 mm.

[0094] It is set that when the displacement of the indenter reaches the value of the above-mentioned indenter displacement L, the cracks aggregate (that is, the transverse cracks are hindered, the same below), and the loading is stopped when the pressing depth of the indenter increases linearly to the depth D, where the depth D is 0.4 mm.

[0095] The above software is used to automatically draw 8 layers of loop mesh at the crack tip, among which the circle of mesh closest to the crack tip is set as a singular unit mesh. The J integral of each layer of mesh is automatically solved by the contour integration method. The average value of the 8 J integrals obtained under the same displacement load is the energy release rate under the displacement load. Then, the stress intensity factor under the displacement load is automatically calculated according to equations (1) and (2):

[0096]

[0097] Among them, K eff is the stress intensity factor, in MPa*m 1 / 2 ,

[0098] E Y is the elastic modulus, in MPa,

[0099] v is Poisson's ratio,

[0100] G is the energy release factor, the unit is J / m 2 ,

[0101] Automatically plot stress intensity factor-displacement load curves.

[0102] Step 4: The stress intensity factor corresponding to the above-mentioned indenter displacement Q in the stress intensity factor-displacement load curve is the fracture toughness.

[0103] Calculation example a-2

[0104] The difference from Example a-1 is that the test temperature of the in-situ three-point bending test is 1300°C, and the indenter displacement Q=0.265mm; when the finite element model is established in the finite element software ABAQUS, the input elastic modulus is 70GPa.

[0105] Example b-2

[0106] The difference from Example b-1 is that the test temperature of the in-situ three-point bending test is 1300°C, the indenter displacement P = 0.062mm, and the indenter displacement Q = 0.265mm; when the finite element model is established in the finite element software ABAQUS, the input elastic modulus is 70GPa, and the length of the transverse crack when the indenter displacement is set is as follows:

[0107] When the pressing distance of the indenter is 0.070 mm, the transverse crack length is about 0.21 mm;

[0108] When the pressing distance of the indenter is 0.130 mm, the transverse crack length is about 0.43 mm;

[0109] When the pressing distance of the indenter is 0.176 mm, the transverse crack length is about 0.50 mm;

[0110] When the pressing distance of the indenter is 0.19 mm, the transverse crack length is about 0.85 mm;

[0111] When the pressing distance of the indenter is 0.30 mm, the length of the transverse crack is about 1.60 mm.

[0112] Example c-2

[0113] The difference from Example c-1 is that the test temperature of the in-situ three-point bending test is 1300°C, the indenter displacement P = 0.062mm, the indenter displacement L = 0.176mm, and the indenter displacement Q = 0.205mm; when the finite element model is established in the finite element software ABAQUS, the input elastic modulus is 70GPa, and the length of the transverse crack when different indenter displacements are set is as follows:

[0114] When the pressing distance of the indenter is 0.070 mm, the transverse crack length is about 0.21 mm;

[0115] When the pressing distance of the indenter is 0.130 mm, the transverse crack length is about 0.43 mm;

[0116] When the pressing distance of the indenter is 0.176 mm, the transverse crack length is about 0.50 mm;

[0117] When the pressing distance of the indenter is 0.19 mm, the transverse crack length is about 0.50 mm;

[0118] When the pressing distance of the indenter is 0.30 mm, the length of the transverse crack is about 0.50 mm.

[0119] Depend on Figure 5 It can be seen that when the interface cracking is not considered (such as Example a-1), the stress intensity factor continues to increase linearly with the increase of displacement load. When the interface cracking is considered (such as Example b-1), the energy release rate decreases significantly, so the stress intensity factor decreases compared to when there is no interface cracking. With the downward pressure of the indenter and the expansion of the interface crack, the growth of the stress intensity factor is in the shape of a quadratic function until the crack becomes unstable when the critical value is reached. When the interface crack encounters an obstacle and stops expanding during its expansion (such as Example c-1), the strain energy will continue to accumulate, and the stress intensity factor will be higher than the growth rate of the interface crack that continues to expand until the critical fracture toughness specimen is destroyed.

[0120] The stress intensity factor-displacement load curves obtained by the finite element model in the above examples are as follows: Figure 6As shown in the figure. RT represents room temperature, HT represents 1300℃ high temperature, solid lines of different colors represent numerical simulation values ​​of stress intensity factors of different composite materials, dashed lines represent numerical simulation values ​​of stress intensity factors without considering interface cracking under ideal conditions, and lines of the same color represent the same set of parallel tests. The stress intensity factor corresponding to the displacement of the indenter when the load of each material reaches the maximum is the predicted fracture toughness value. The dotted lines are the experimental measurement values ​​of the fracture toughness of each composite material (calculated by the three-point bending fracture toughness formula provided by the national standard GB / T 23806-2009). It can be seen from the figure that the corresponding indenter displacement for the initiation of interface cracks in samples of different materials and temperatures is different, and the inflection point of the decrease in stress intensity factor appears at different locations. For 2D-SiCf / SiC and 3D-SiCf / SiC composites, interface cracking releases part of the strain energy, causing the stress intensity factor to decrease compared to when there is no interface cracking. In addition, since high temperature causes the elastic modulus of the material to decrease, the stress intensity factor of the two composite materials is slightly lower than that at room temperature, and the indenter displacement corresponding to the maximum load is slightly larger than the indenter displacement at room temperature, making the high-temperature fracture toughness of the two composite materials slightly lower than the room-temperature fracture toughness, which is consistent with the experimental results. Compared with 2D-SiCf / SiC composites, at room and high temperatures, the interface cracks of 3D-SiCf / SiC composites are blocked by the longitudinal fiber bundles and cannot expand laterally, causing strain energy to accumulate and tend to expand downward. Therefore, the stress intensity factor of 3D-SiCf / SiC composites is higher, the cracks are more likely to become unstable, and the fracture toughness is lower, which is consistent with the experimental results. In addition, due to Figure 6 As shown in the figure, the horizontal coordinates of the intersection of the stress intensity factors of the two composite materials at room temperature and high temperature and the experimentally measured fracture toughness values ​​are concentrated in the range of 0.18mm to 0.27mm, that is, the predicted crack instability moments of the three composite materials all occur during the period of 0.18mm < indenter displacement < 0.27mm, which is consistent with the in-situ test results. Based on the above results, the fracture toughness prediction model of ceramic matrix composites based on the finite element model is consistent with the experimental results, and has good validity and reliability.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for testing the fracture toughness of fiber-reinforced ceramic matrix composites, characterized in that: The method comprises the following steps: Referring to GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics", a single-side notched beam three-point bending test specimen was prepared, recorded as the first specimen, and an in-situ three-point bending test was carried out until the first specimen broke. During the test, a fixed displacement was used to control the loading, and the load-indenter displacement curve was recorded in real time. The crack tip of the prefabricated crack and its vicinity were observed to obtain the load and indenter displacement P corresponding to the initiation of the transverse crack, the indenter displacement Q corresponding to the maximum load, and the functional relationship between the indenter displacement and the transverse crack length or the transverse crack length at different indenter displacements, wherein the material of the first specimen is a two-dimensional woven fiber reinforced ceramic matrix composite material; A finite element model with prefabricated cracks was established in the finite element software. The constructed specimen was recorded as the second specimen and the following conditions were set: The material of the second sample is a purely elastic isotropic homogeneous material. Input the elastic modulus and Poisson's ratio. A rigid indenter is set above the second specimen and displacement boundary conditions are used to control the downward pressure behavior. Two rigid rollers are set below to support and fix the movement of the second specimen in all directions. There is no friction between the second specimen and the rollers and indenter, and the face-to-face contact conditions are all hard contact. The length, width, height, chamfer, prefabricated crack depth and cut width, lower span, roller diameter, indenter loading rate and test temperature of the second specimen are consistent with those of the in-situ three-point bending test. When the indenter displacement reaches the value of the indenter displacement P, the transverse crack initiates, and according to the in-situ three-point bending test, the functional relationship between the indenter displacement and the transverse crack length or the transverse crack length at different indenter displacements is set, and the loading is stopped when the indenter pressing depth increases linearly to the depth D; Draw 5-10 layers of loop grids at the crack tip, where the circle of grids closest to the crack tip is set as a singular unit grid, solve the J integral of each layer of grids by the contour integration method, and then obtain the energy release rate and stress intensity factor, and draw the stress intensity factor-displacement load curve. The stress intensity factor corresponding to the indenter displacement Q in the curve is the fracture toughness; The depth D is greater than the indenter displacement Q.

2. The method according to claim 1, characterized in that 0.1mm≤the depth D-the maximum pressure head displacement Q≤0.3mm.

3. The method according to claim 1, characterized in that The stress intensity factor is calculated according to formula (1): Among them, K eff is the stress intensity factor, in MPa*m 1 / 2 ; E Y is the elastic modulus, in MPa; v is Poisson’s ratio; G is the energy release factor, the unit is J / m 2 .

4. The method according to claim 1, characterized in that In the process of establishing a finite element model with prefabricated cracks, when setting the length of the transverse crack at different indenter displacements, the set indenter displacements include at least one indenter displacement greater than the indenter displacement Q.

5. The method according to claim 1, characterized in that The first sample is 18 mm long, 3 mm wide, 4 mm high, with a chamfer of 0.12 mm and a roughness of 0.2 μm. A wire saw is used to preform a crack, the crack is located in the middle of the length direction of the first sample, the lower surface is the tensile surface, the preformed crack depth is 2 mm, the incision width is 0.1 mm, the lower span is 16 mm, and the roller diameter is 4 mm.

6. The method according to claim 1, characterized in that In the in-situ three-point bending test, a 10N preload is applied before loading for sample positioning and fixation; displacement-controlled loading is adopted, and the loading rate is 0.002mm / s; and the test temperature is 25-1300°C.

7. The method according to claim 1, characterized in that The two-dimensional woven fiber-reinforced ceramic matrix composite material includes at least one of a carbon fiber-reinforced ceramic matrix composite material or a silicon carbide fiber-reinforced ceramic matrix composite material.

8. The method according to claim 1, characterized in that The material of the first sample is a three-dimensional puncture fiber reinforced ceramic matrix composite material; According to the in-situ three-point bending test, the corresponding indenter displacement L when the transverse crack is blocked is also obtained; In the process of establishing the finite element model containing the prefabricated cracks, it is also set that when the displacement of the indenter reaches the value of the displacement L of the indenter, the transverse crack is blocked.

9. The method according to claim 8, characterized in that The three-dimensional puncture fiber reinforced ceramic matrix composite material includes a silicon carbide fiber reinforced ceramic matrix composite material.

10. The method according to claim 1, characterized in that The finite element software is ABAQUS or ANASYS.

Citation Information

Patent Citations

  • Test piece and method for testing fracture toughness of hybrid mode of double-material interface

    CN103616299A

  • Heterogeneous material crack stress intensity factor calculation method applying DIC technology

    CN111398057A

  • Experiment-numerical method for testing dynamic fracture toughness of non-uniform material in weld zone

    CN118424916A

  • Determining plane strain fracture toughness and the J-Integral for solid materials using stress field modified miniature specimens

    US4895027A

Cited By

  • Prediction method for fracture toughness of polar region marine composite steel plate under different thicknesses

    CN120409132A