Method for analyzing laterite-nickel ore by X-ray fluorescent powder tabletting method

Through the X-ray fluorescent powder tableting method and the optimization of standard curve, the problem of long detection time and high cost of laterite nickel ore is solved, faster and more economical detection results are achieved, and the accuracy and stability of the detection are improved.

CN119064397APending Publication Date: 2024-12-03INDONESIA GREEN INSPECTION TECHNOLOGY RESEARCH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411400534.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing laterite nickel ore detection methods have problems such as long detection time, high cost and complex sample preparation, especially the molten X-ray fluorescence method requires valuable consumables and is difficult to master.

Method used

The X-ray fluorescent powder tableting method is used to statistically analyze the typical values ​​of different suppliers, establish and optimize standard curves, and combine the melting tableting method and the fluorescent tableting method for detection to reduce detection costs and improve analysis speed.

Benefits of technology

It effectively reduces the cost of laterite nickel ore detection, improves the analysis speed, and improves the accuracy and stability of the detection results by optimizing the standard curve.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064397A_ABST
    Figure CN119064397A_ABST
Patent Text Reader

Abstract

The invention provides a method for analyzing laterite-nickel ore by an X-ray fluorescent powder tabletting method, which comprises the following steps: S1, carrying out statistical analysis on nickel ore detection values of various suppliers, and finding out typical values and representative samples of different suppliers and mines; s2, analyzing the representative sample selected in the step S1 by adopting a fuse piece valuing method and a fluorescent tabletting method, and establishing a standard curve of the fluorescent tabletting method by taking a result of the fuse piece valuing method as a standard value; s3, optimizing the standard curve obtained in the step S2; s4, verifying whether the optimized standard curve accurately analyzes the content of each element in the laterite-nickel ore or not; and if yes, detecting the to-be-detected sample by using a fluorescence tabletting method aiming at the subsequent laterite-nickel ore sample. Compared with a fuse piece valuing method, when the laterite-nickel ore of a supplier is detected through fluorescent powder tabletting and the optimized standard curve, the detection cost can be greatly reduced, the economic benefit can be improved, and the analysis speed of the laterite-nickel ore can be increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laterite nickel ore detection, and in particular to a method for analyzing laterite nickel ore by an X-ray fluorescence powder tabletting method. Background Art

[0002] Nickel in laterite is mainly used as raw material for stainless steel and battery production. It is a silicate mineral whose main components are nickel, iron, magnesium oxide, calcium oxide, silicon dioxide, chromium oxide and other elements. The important basis for evaluating its quality index is the content of nickel, silicon, magnesium and other components. At present, the chemical method and fluorescence method are generally used to determine the components in laterite. The chemical method is cumbersome to operate. The determination of nickel content requires dissolution, separation, colorimetry and other steps, which takes about six hours. The fluorescence method mostly uses melting sample preparation, such as the non-ferrous metal industry standard YST 820.23-2012 & Chemical Analysis Method of Laterite Nickel Ore Part 23: Determination of Cobalt, Iron, Nickel, Phosphorus, Aluminum Oxide, Calcium Oxide, Chromium Oxide, Magnesium Oxide, Manganese Oxide, Silicon Dioxide and Titanium Dioxide by wavelength dispersion X-ray fluorescence spectrometry. The use of X-ray fluorescence melting method has the disadvantages of long sample preparation cycle and difficult to master analysis operation. In the prior art, the detection method for laterite ore is to use the fusion film method to melt the sample and then use the X-ray fluorescence analyzer to detect it. This method takes about 30 minutes to detect, and requires a matching fusion machine, lithium tetraborate, lithium metaborate, platinum crucible and other expensive and consumable consumables with high consumption, and has the disadvantages of high cost. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for analyzing laterite nickel ore by using an X-ray fluorescence powder tableting method, which can reduce the detection cost of laterite ore.

[0004] The present invention is achieved in that:

[0005] The present invention provides a method for analyzing laterite nickel ore by X-ray fluorescence powder tableting method, comprising the following steps:

[0006] S1. Statistical analysis of nickel ore test values ​​from various suppliers to find typical values ​​and representative samples from different suppliers and mines;

[0007] S2, analyzing the representative sample selected in step S1 by using the fused plate determination method and the fluorescent plate pressing method, taking the result of the fused plate determination method as the standard value, and establishing a standard curve for the fluorescent plate pressing method analysis;

[0008] S3, optimizing the standard curve obtained in step S2 to obtain an optimized standard curve;

[0009] S4. Verify whether the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore;

[0010] If not, return to step S3;

[0011] If yes, for the subsequent laterite nickel ore samples, the fluorescent tablet method is used to detect the samples to be tested, and the equipment calculates the element content in the laterite nickel ore samples based on the optimized standard curve.

[0012] Furthermore, in the step S2, sample preparation of the representative sample is also included, and the sample preparation process is:

[0013] The representative sample was ground for 70 seconds and then sieved through a 200-mesh sieve.

[0014] Furthermore, in the steps S2 and S4, the pressure of the press used in the fluorescent tableting method is 30 tons, and the pressure stabilization time is 30 seconds.

[0015] Furthermore, in step S3, the optimization of the standard curve is carried out by changing the calculation method of the curve, adjusting the slope and intercept of the standard curve, or adjusting the spectral interference between the detection element and the interfering element.

[0016] Furthermore, the method further comprises the following steps:

[0017] S5. Formulate a quality control method for monitoring the stability of the curve; the quality control method is internal control sample, method comparison, instrument comparison or standard sample comparison;

[0018] The internal control samples are specifically:

[0019] The inspectors take internal control samples with known content every day or every shift, and use fluorescent tablets to test them. The stability of the equipment and the optimized standard curve is determined by the fluctuation of the sample data.

[0020] The method comparison is specifically as follows:

[0021] Take multiple samples regularly and compare them with the fused sheet value method or chemical analysis method. The accuracy of the test data can be comprehensively determined by comparing the data of different methods to provide feedback on the accuracy and stability of the equipment and curves.

[0022] The instrument comparison is specifically as follows:

[0023] Regularly take multiple samples to test on the same curve of different devices, and compare the data differences of different devices to determine the stability of the equipment;

[0024] The standard sample comparison is specifically as follows:

[0025] Regularly use the equipment curve to test a set of standard samples, and determine the accuracy and stability of the equipment and curve by the difference between the standard values ​​and the test values ​​of the standard samples.

[0026] Furthermore, in step S4, the specific process of verifying whether the optimized standard curve accurately analyzes the content of each element in the laterite nickel ore is:

[0027] Select batch samples from 7 suppliers, 10 batch samples from each supplier;

[0028] The optimized standard curve was used to analyze batch samples from 7 suppliers to obtain the measured values ​​of the content of each element in laterite nickel ore;

[0029] Then, the same batch samples from seven suppliers were analyzed using the melt value method to obtain the standard values ​​of the content of each element in laterite nickel ore;

[0030] Set the deviation range of the measured value that is allowed to exceed the standard value;

[0031] If the measured value is within the standard value deviation range, it is determined that the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore;

[0032] If the measured value exceeds the deviation range of the standard value, the process returns to step S3.

[0033] The advantages of the present invention are that when the laterite nickel ore of the supplier is tested by pressing the fluorescent powder into tablets and optimizing the standard curve, the testing cost can be greatly reduced, the economic benefit can be improved, and the analysis speed of the laterite nickel ore can be increased compared with the fused sheet determination method. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The present invention will be further described below in conjunction with embodiments with reference to the accompanying drawings.

[0035] Figure 1 The present invention is a schematic flow chart of a method for analyzing laterite nickel ore by using an X-ray fluorescence powder tabletting method.

[0036] Figure 2 This is a comparison chart of Ni analysis curve parameters of ore samples from different suppliers in the present invention.

[0037] Figure 3 It is a comparison chart of Fe analysis curve parameters of ore samples from different suppliers in the present invention.

[0038] Figure 4 This is a comparison chart of SiO2 analysis curve parameters of ore samples from different suppliers in the present invention.

[0039] Figure 5 This is a comparison chart of MgO analysis curve parameters of ore samples from different suppliers in the present invention.

[0040] Figure 6 This is a comparison chart of nickel content deviation before optimization of the standard curve of the present invention.

[0041] Figure 7This is a comparison chart of nickel content deviation after the standard curve of the present invention is optimized.

[0042] Figure 8 This is a comparison chart of the iron content deviation before the standard curve of the present invention is optimized.

[0043] Fig. 9 This is a comparison chart of the iron content deviation after the standard curve of the present invention is optimized. DETAILED DESCRIPTION

[0044] The overall idea of ​​the present invention is:

[0045] (1) Find the optimal sample particle size through experiments to reduce the impact of particle size effect on the results;

[0046] (2) Statistical analysis of nickel ore test values ​​from various suppliers: by analyzing different batches of nickel ore, typical values ​​and representative samples from different suppliers and mines can be found;

[0047] (3) Prepare and optimize the standard curve for tablet analysis: select the same number of samples with different contents from different mines and purchased standard samples, use the fused sheet as the value, use the pressure of the fluorescent tablet press at 30 tons and the stabilization time of 30 seconds to ensure that the sample surface is smooth and the particle size is uniform, and analyze and prepare the standard curve; analyze samples from different mineral sources, analyze the deviation between the data of different mineral sources and the fused sheet, and adjust the standard curve;

[0048] (4) After the curve adjustment is completed, the tableting method and the optimized standard curve are used to detect the laterite samples.

[0049] (5) Develop quality control methods to monitor the stability of the curve and ensure the accuracy and reliability of the data. The quality control methods include one or more of the following: internal control samples, method comparison, instrument comparison, or standard sample comparison.

[0050] See also Figures 1 to 9 The present invention provides a method for analyzing laterite nickel ore by X-ray fluorescence powder tableting, comprising the following steps:

[0051] S1. Statistical analysis of nickel ore test values ​​from various suppliers to find typical values ​​and representative samples from different suppliers and mines;

[0052] S2, analyzing the representative sample selected in step S1 by using the fused plate determination method and the fluorescent plate pressing method, taking the result of the fused plate determination method as the standard value, and establishing a standard curve for the fluorescent plate pressing method analysis;

[0053] S3, optimizing the standard curve obtained in step S2 to obtain an optimized standard curve;

[0054] S4. Verify whether the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore;

[0055] If not, return to step S3;

[0056] If yes, for the subsequent laterite nickel ore samples, the fluorescent tablet method is used to detect the samples to be tested, and the equipment calculates the element content in the laterite nickel ore samples based on the optimized standard curve.

[0057] Specifically, in step S2, the representative sample is further prepared, and the sample preparation process is as follows:

[0058] The representative sample was ground for 70 seconds and then sieved through a 200-mesh sieve.

[0059] Specifically, in the steps S2 and S4, the pressure of the press used in the fluorescent tableting method is 30 tons, and the pressure stabilization time is 30 seconds.

[0060] Specifically, in step S3, the optimization of the standard curve is carried out by changing the calculation method of the curve, adjusting the slope and intercept of the standard curve, or adjusting the spectral interference between the detection element and the interfering element.

[0061] Specifically, the following steps are also included:

[0062] S5. Formulate a quality control method for monitoring the stability of the curve; the quality control method is internal control sample, method comparison, instrument comparison or standard sample comparison;

[0063] The internal control samples are specifically:

[0064] The inspectors take internal control samples with known content every day or every shift, and use fluorescent tablets to test them. The stability of the equipment and the optimized standard curve is determined by the fluctuation of the sample data.

[0065] The method comparison is specifically as follows:

[0066] Take multiple samples regularly and compare them with the fused sheet value method or chemical analysis method. The accuracy of the test data can be comprehensively determined by comparing the data of different methods to provide feedback on the accuracy and stability of the equipment and curves.

[0067] The instrument comparison is specifically as follows:

[0068] Regularly take multiple samples to test on the same curve of different devices, and compare the data differences of different devices to determine the stability of the equipment;

[0069] The standard sample comparison is specifically as follows:

[0070] Regularly use the equipment curve to test a set of standard samples, and determine the accuracy and stability of the equipment and curve by the difference between the standard values ​​and the test values ​​of the standard samples.

[0071] Specifically, in step S4, the specific process of verifying whether the optimized standard curve accurately analyzes the content of each element in the laterite nickel ore is:

[0072] Select batch samples from 7 suppliers, 10 batch samples from each supplier;

[0073] The optimized standard curve was used to analyze batch samples from 7 suppliers to obtain the measured values ​​of the content of each element in laterite nickel ore;

[0074] Then, the same batch samples from seven suppliers were analyzed using the melt value method to obtain the standard values ​​of the content of each element in laterite nickel ore;

[0075] Set the deviation range of the measured value that is allowed to exceed the standard value;

[0076] If the measured value is within the standard value deviation range, it is determined that the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore;

[0077] If the measured value exceeds the deviation range of the standard value, the process returns to step S3.

[0078] A specific application of this application is:

[0079] In the same batch of nickel ore, sampling and reduction were carried out according to the national standard requirements. Nine different samples were ground out with different grinding times from 60s to 140s. Then a 200-mesh sieve was used to sieve the samples at different grinding times to measure the screening rates. The accuracy and repeatability of the Ni, Fe, Si and Mg analysis data of the samples ground for 70s and 80s can meet the requirements. Since the standard deviation range of each content in the 70s sample tablet analysis is relatively small and the short grinding time can save sample preparation time and increase the service life of the machine, it is recommended to use a 70s grinding time.

[0080] Statistical analysis of nickel ore test values ​​from various suppliers: By analyzing different batches of nickel ore, typical values ​​and representative samples from different suppliers and mines are found. The following takes 7 suppliers as an example, and selects several representative samples from 7 suppliers for fusing value determination: select samples according to national standards, sample and reduce them, and prepare samples according to the optimal grinding time. After mixing several representative samples from the same supplier, perform fusing value determination and fluorescent powder pressing analysis.

[0081] Fluorescent powder pressed tablet analysis uses an X-ray fluorescence spectrometer to measure the element emission intensity of the sample; the working parameters of the fluorescence spectrometer used are:

[0082] Working voltage / current: 40KV / 70mA;

[0083] Vacuum optical path;

[0084] Spectrophotometer temperature: 35.0±0.5℃.

[0085] The standard curve of fluorescent powder pressed tablet analysis was established using the results of melt fixed value analysis as the standard value.

[0086] Standard curves are prepared for Ni, Fe, SiO2 and MgO in representative samples to obtain the slope b, intercept c and correlation coefficient R of the Ni, Fe, SiO2 and MgO standard curves, such as Figures 2 to 5 shown.

[0087] The differences between mineral samples from different suppliers were analyzed by comparing the slopes, intercepts and correlation coefficients of the tableting curves of mineral samples from different suppliers.

[0088] There is no significant difference in the composition of the ore samples from suppliers, among which: the nickel content is between 1.4% and 2.3%;

[0089] The iron content is between 10% and 30%; the SiO2 content is between 25% and 50%; and the MgO content is between 10% and 25%.

[0090] Through analysis, it was found that the intensity of the analysis of mineral samples from different suppliers with the same content range using the same method and the same equipment using the fluorescence tablet method was different, resulting in large differences in the slope and intercept of the standard curve (i.e., mineral effect). Therefore, in order to address this problem, it is necessary to optimize the standard curve to reduce the impact of the mineral effect on the test results. The standard curves of Ni, Fe, SiO2 and MgO were optimized respectively. Four optimized standard curves of Ni, Fe, SiO2 and MgO were obtained respectively.

[0091] The optimization of the standard curve can be done by one or more of the following three methods:

[0092] 1. Change the calculation method of the curve:

[0093] When testing samples, a curve of the relationship between strength and percentage content will be fitted based on the strength measured by the equipment and the standard value. The standard value detected by the fuse value method will be added to the curve through the software in the equipment. In the linear function and quadratic function selection window provided by the software in the equipment, the appropriate function will be selected to re-fit the standard curve. After selection and recalculation, it will be compared with the standard value (obtained by the fuse value method) to finally determine whether to use a linear function or a quadratic function for curve fitting, so that the test results of different samples are closer to the standard value.

[0094] 2. Adjust the slope and intercept of the curve:

[0095] Normally, the standard curve is a relationship curve that uses a linear function Y=aX+b to fit the standard value and the detection intensity (a is the slope and b is the intercept). When adjusting, the result obtained by recalculation after adjusting the slope and intercept is compared with the standard value obtained by the fuse value determination method, and finally the difference between the recalculated result and the standard value meets the use requirements, so as to ensure the accuracy of the test results.

[0096] 3. Adjust the spectrum interference between the detection element and the interfering element:

[0097] Determine the interfering elements in the main element spectrum of the sample, and use the corresponding method of subtracting interference in the software to subtract the interference of the elements (for example, iron will have overlapping interference on the intensity of nickel, which can be eliminated by subtracting the interference of iron on nickel).

[0098] To verify whether the optimized standard curve can accurately analyze the content of each element in laterite nickel ore, batch samples from 7 suppliers were selected, and 10 batch samples from each supplier were analyzed by melting and pressing. The deviations of the pressing data and the standard value (measured by the melting value method) before and after the adjustment of the pressing curve were compared, as follows:

[0099] Select batch samples from 7 suppliers, 10 batch samples from each supplier;

[0100] The same batch of samples were then analyzed using the optimized standard curves of Ni, Fe, SiO2 and MgO to obtain the measured values ​​of the contents of nickel, iron, SiO2 and MgO in the samples respectively;

[0101] The same batch of samples was analyzed using the fused sheet determination method to obtain the standard values ​​of the nickel, iron, SiO2 and MgO contents in the samples.

[0102] Set the deviation range of the measured value to exceed the standard value; for example, set the deviation range to ±5% of the standard value

[0103] like Figures 6 to 9 As shown in the figure, if the measured value is within the standard value deviation range, it is determined that the optimized standard curves of Ni, Fe, SiO2 and MgO can accurately analyze the content of each element in the laterite nickel ore; for subsequent laterite nickel ore samples, fluorescent pressed films are used to detect the samples to be tested, and the equipment calculates the element content in the laterite nickel ore samples according to the optimized standard curves.

[0104] If the measured value exceeds the deviation range of the standard value, the curve should be optimized again.

[0105] In the subsequent use process, in order to monitor the stability of the optimized standard curve and ensure the accuracy and reliability of the data, one or more of the following methods can be used.

[0106] 1. Internal control samples; internal control samples are specifically:

[0107] The inspector takes the corresponding internal control sample (the content of the components in the internal control sample is known) and prepares it into a powder sample. Every day or every shift, the internal control sample is tested using the fluorescent tablet method. The sample data obtained from the test is compared with the known component content, and the stability of the equipment and the curve is determined by the fluctuation of the sample data.

[0108] 2. Method comparison; the specific method comparison is as follows:

[0109] Multiple samples are taken regularly and compared with different analysis methods such as the fused sheet determination method or chemical analysis method. The accuracy of the test data is comprehensively determined through the data compared by different methods to provide feedback on the accuracy and stability of the equipment and curves.

[0110] The content of components in the sample analyzed by the fusion plate determination method or chemical analysis method is the standard value.

[0111] For example, 10 samples were analyzed using the optimized standard curves of Ni, Fe, SiO2 and MgO to obtain the contents of nickel, iron, SiO2 and MgO in the 10 samples respectively;

[0112] Take another 10 samples from the same batch and analyze them using the fusion plate determination method or chemical analysis method to obtain the standard values ​​of nickel, iron, SiO2 and MgO in the 10 samples.

[0113] If the contents of nickel, iron, SiO2 and MgO analyzed using the optimized standard curve are close to the standard values ​​analyzed by the fusion plate determination method or the chemical analysis method, it is determined that the accuracy and stability of the four optimized standard curves and equipment are high.

[0114] If the contents of nickel, iron, SiO2 and MgO analyzed by the optimized standard curve are compared with the standard values ​​analyzed by the fusion plate determination method or the chemical analysis method, only one set of data or two sets of data are different, because there is a possibility of misoperation when analyzing the sample by the optimized standard curve, fusion plate determination method or chemical analysis method. Therefore, when only one set of data or two sets of data are different, it is also determined that the accuracy and stability of the four optimized standard curves and equipment are high.

[0115] 3. Instrument comparison; the specific instrument comparison is as follows:

[0116] Regularly take multiple samples from different devices and test them on the same curve. The stability of different devices can be determined by comparing the data differences between them.

[0117] 4. Comparison of standard samples. The specific comparison of standard samples is as follows:

[0118] Regularly use the equipment curve to test a set of standard samples, and determine the accuracy and stability of the equipment and curve by the difference between the standard values ​​and the test values ​​of the standard samples.

[0119] Although the specific implementation modes of the present invention are described above, those skilled in the art should understand that the specific implementation modes described are only illustrative and are not intended to limit the scope of the present invention. Equivalent modifications and changes made by those skilled in the art in accordance with the spirit of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. A method for analyzing laterite nickel ore by X-ray fluorescence powder tableting, characterized in that: The steps include: S1. Statistical analysis of nickel ore test values ​​from various suppliers to find typical values ​​and representative samples from different suppliers and mines; S2, analyzing the representative sample selected in step S1 by using the fusion plate determination method and the fluorescence compression method, taking the result of the fusion plate determination method as the standard value, and establishing a standard curve of the fluorescence compression method; S3, optimizing the standard curve obtained in step S2 to obtain an optimized standard curve; S4. Verify whether the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore; If not, return to step S3; If yes, for the subsequent laterite nickel ore samples, the fluorescent tablet method is used to detect the samples to be tested, and the equipment calculates the element content in the laterite nickel ore samples based on the optimized standard curve.

2. The method for analyzing laterite nickel ore by X-ray fluorescence powder tableting as claimed in claim 1, characterized in that: In the step S2, the representative sample is also prepared, and the sample preparation process is as follows: The representative sample was ground for 70 seconds and then sieved through a 200-mesh sieve.

3. The method for analyzing laterite nickel ore by X-ray fluorescence powder tableting as claimed in claim 1, characterized in that: In the steps S2 and S4, the pressure of the press used in the fluorescent tableting method is 30 tons, and the stabilization time is 30 seconds.

4. The method for analyzing laterite nickel ore by X-ray fluorescence powder tableting as claimed in claim 1, characterized in that: In step S3, the standard curve is optimized by changing the calculation method of the curve, adjusting the slope and intercept of the standard curve, or adjusting the spectral interference between the detection element and the interfering element.

5. The method for analyzing laterite nickel ore by X-ray fluorescence powder tableting as claimed in claim 1, characterized in that: It also includes the following steps: S5. Formulate a quality control method for monitoring the stability of the curve; the quality control method is internal control sample, method comparison, instrument comparison or standard sample comparison; The internal control samples are specifically: The inspectors take internal control samples with known content every day or every shift, and use fluorescent tablets to test them. The stability of the equipment and the optimized standard curve is determined by the fluctuation of the sample data. The method comparison is specifically as follows: Take multiple samples regularly and compare them with the fused sheet value method or chemical analysis method. The accuracy of the test data can be comprehensively determined by comparing the data of different methods to provide feedback on the accuracy and stability of the equipment and curves. The instrument comparison is specifically as follows: Regularly take multiple samples and test them on the same curve of different devices, and compare the data of different devices to determine the stability of the equipment; The standard sample comparison is specifically as follows: Regularly use the equipment curve to test a set of standard samples, and determine the accuracy and stability of the equipment and curve by the difference between the standard values ​​and the test values ​​of the standard samples.

6. The method for analyzing laterite nickel ore by X-ray fluorescence powder tableting as claimed in claim 1, characterized in that: In step S4, the specific process of verifying whether the optimized standard curve accurately analyzes the content of each element in the laterite nickel ore is: Select batch samples from 7 suppliers, 10 batch samples from each supplier; The optimized standard curve was used to analyze batch samples from 7 suppliers to obtain the measured values ​​of the content of each element in laterite nickel ore; Then, the same batch samples from seven suppliers were analyzed using the melt value method to obtain the standard values ​​of the content of each element in laterite nickel ore; Set the deviation range of the measured value that is allowed to exceed the standard value; If the measured value is within the standard value deviation range, it is determined that the optimized standard curve can accurately analyze the content of each element in the laterite nickel ore; If the measured value exceeds the deviation range of the standard value, the process returns to step S3.

Citation Information

Cited By

  • Method for detecting content of TiO2 in molten salt by using handheld X fluorescence

    CN120404819A