Display cover plate, display module and terminal equipment

By adopting a combined structure of buffer layer and support layer in the display cover, the problem of glass cover plate easily breaking when impacted by external forces is solved, the cracking and impact resistance is improved, and the service life of the terminal equipment is extended.

CN119068763APending Publication Date: 2024-12-03HONOR DEVICE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310636050.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing glass cover assembly is prone to fragility when impacted by external forces, and has poor rupture resistance, which affects the service life of the display module.

Method used

The display cover structure consisting of a buffer layer, a substrate layer and a support layer are adopted, wherein the buffer layer and the support layer are arranged on the substrate layer by coating, and the modulus of the buffer layer is smaller than the modulus of the support layer, the buffer layer and the The support layers are all light-transmitting and impact-resistant, which improves the crack resistance of the substrate layer.

Benefits of technology

It effectively reduces the probability of microcracks spreading and rupture of the substrate layer when impacted by external forces, improves the impact resistance and cracking resistance of the display cover plate, and improves the impact resistance of the display end of the terminal equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119068763A_ABST
    Figure CN119068763A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the technical field of cover plates, and provides a display cover plate, a display module and terminal equipment, the display cover plate comprises a buffer layer, a base material layer and a supporting layer which are sequentially arranged from top to bottom, two opposite end faces of the base material layer are coated with the buffer layer and the supporting layer, and the modulus of the buffer layer is smaller than that of the supporting layer. After the base material layer is processed, certain microcracks inevitably exist on the upper surface and the lower surface of the base material layer, and after the supporting layer is additionally arranged on the lower surface of the base material layer, sunken deformation generated by external force impact can be resisted, and meanwhile, the microcracks on the lower surface can be filled; and the breakage of the base material layer caused by microcrack propagation when the base material layer is impacted by external force is effectively reduced. And moreover, after the buffer layer is added on the upper surface of the base material layer, micro cracks on the upper surface can be filled, the propagation probability of the micro cracks is reduced, certain external force impact can be resisted, and the impact resistance of the base material layer is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of display cover plates, and in particular to a display cover plate, a display module having the display cover plate, and a terminal device having the display module. Background Art

[0002] A display folding terminal is a terminal model whose display screen can be folded inward or outward. Usually, its display module includes a cover assembly, a screen assembly, and a support assembly. Among them, the cover assemblies currently on the market mainly include polyimide cover assemblies and glass cover assemblies. The polyimide cover assembly has excellent bending resistance and good impact resistance, and can be directly used for the protection of the display module, but its disadvantage is that the surface texture of the material is poor. The glass cover assembly has the advantages of high hardness, good resistance, and high transmittance, but its disadvantage is that it is easily broken by the ultimate. Summary of the invention

[0003] The embodiments of the present application provide a display cover plate, a display module and a terminal device, which are used to improve the technical problem of poor anti-fragmentation performance of a glass cover plate assembly.

[0004] To achieve the above purpose, the embodiment of the present application adopts the following technical solution:

[0005] In a first aspect, an embodiment of the present application provides a display cover plate, comprising a buffer layer, a substrate layer and a support layer arranged in sequence from top to bottom, wherein the buffer layer and the support layer are coated on opposite end surfaces of the substrate layer, and the modulus of the buffer layer is smaller than the modulus of the support layer.

[0006] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0007] The display cover provided by the embodiment of the present application has a buffer layer arranged on the upper surface of the substrate layer, and a support layer arranged on the lower surface thereof, and the buffer layer and the support layer are both arranged on the substrate layer by coating, and at the same time, the modulus of the buffer layer is less than the modulus of the support layer. After the substrate layer is processed, it is inevitable that there are certain microcracks on its upper and lower surfaces. During the assembly process, if it is directly or indirectly attached to a film material such as a display layer, the upper surface of the substrate layer is prone to depression under the impact of external force, and the microcracks on the lower surface away from the impact of external force are extended by the tensile force, so that the lower surface of the substrate layer first breaks and causes the entire substrate layer to break. After the support layer is added to the lower surface of the substrate layer, it can resist the depression deformation caused by the impact of external force, and at the same time, the microcracks on the lower surface can be filled, which effectively reduces the microcracks in the substrate layer when it is impacted by external force, resulting in the breakage of the substrate layer. Furthermore, after adding the buffer layer to the upper surface of the substrate layer, the microcracks on the upper surface can also be filled, reducing the probability of the microcracks extending, while also being able to withstand certain external force impacts, further improving the impact resistance of the substrate layer.

[0008] In one embodiment, the substrate layer includes a glass layer, the thickness of the substrate layer is 20 μm to 100 μm, and the modulus of the substrate layer is 63 GPa to 130 GPa.

[0009] In one embodiment, the buffer layer is a light-transmitting flexible layer, and the buffer layer includes one of organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane, or a combination of at least any two of them.

[0010] By adopting the above technical solution, the buffer layer has both light transmittance and impact resistance, which can improve the anti-cracking performance of the substrate layer.

[0011] In one embodiment, the thickness of the buffer layer is 10 μm to 60 μm, and the modulus of the buffer layer is 0.5 MPa to 1000 MPa.

[0012] In one embodiment, the support layer is a light-transmitting flexible layer, and the support layer includes one or a combination of at least any two of polysilazane resin, polyimide, organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane.

[0013] By adopting the above technical solution, the support layer has both light transmittance and impact resistance, which can improve the anti-cracking performance of the substrate layer.

[0014] In one embodiment, the thickness of the support layer is 2 μm to 25 μm, and the modulus of the buffer layer is 0.5 GPa to 7 GPa.

[0015] In one embodiment, the buffer layer has a normal temperature 25°C elongation of ≥5%, and a low temperature -20°C elongation of ≥2%; and / or the support layer has a normal temperature 25°C elongation of ≥5%, and a low temperature -20°C elongation of ≥2%.

[0016] By adopting the above technical solution, the buffer layer and the support layer can meet the structural strength required for the display cover to be folded inward or outward when the fracture elongation rate at room temperature 25°C and / or the fracture elongation rate at low temperature -20°C are the same.

[0017] In one embodiment, the display cover plate further includes a hardening layer, and the hardening layer is disposed on an end surface of the buffer layer facing away from the substrate layer.

[0018] By adopting the above technical solution, the function of the hardened layer is to reduce the probability of the substrate layer being scratched, and reduce the probability of the substrate layer being broken when impacted by external force.

[0019] In one embodiment, the hardening layer includes one or a combination of at least any two of epoxy resin, acrylic resin, polyurethane and silicone.

[0020] In one embodiment, the thickness of the hardened layer is 10 μm to 60 μm, the hardness of the hardened layer is ≥ 2H, and the surface water drop angle of the hardened layer is ≥ 90°.

[0021] In one embodiment, the display cover plate further includes an adhesive layer, and the adhesive layer is disposed on an end surface of the support layer that is away from the substrate layer.

[0022] By adopting the above technical solution, the adhesive layer is used to adhere the substrate layer to the display panel of the external device.

[0023] In a second aspect, an embodiment of the present application provides a display module, comprising the display cover plate described above.

[0024] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0025] The display module provided in the embodiment of the present application has a higher anti-cracking performance based on the above-mentioned display cover plate.

[0026] In a third aspect, an embodiment of the present application provides a terminal device, comprising the display module or the display cover plate described above.

[0027] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0028] The terminal device provided in the embodiment of the present application, based on the above-mentioned display module or display cover, has a higher impact resistance performance of the display end of the terminal device. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of the structure of a terminal device provided in an embodiment of the present application;

[0030] Figure 2 A schematic diagram of the structure of a display module provided in an embodiment of the present application;

[0031] Figure 3 A cross-sectional view of a buffer layer, a substrate layer, and a support layer of a display cover provided in an embodiment of the present application;

[0032] Figure 4 A cross-sectional view of a hardening layer, a buffer layer, a substrate layer, and a support layer of a display cover provided in an embodiment of the present application;

[0033] Figure 5 A cross-sectional view of a buffer layer, a substrate layer, a support layer, and an adhesive layer of a display cover provided in an embodiment of the present application;

[0034] Figure 6 A cross-sectional view of a hardening layer, a buffer layer, a substrate layer, a support layer, and an adhesive layer of a display cover provided in an embodiment of the present application;

[0035] Figure 7 A cross-sectional view of a display cover provided in an embodiment of the present application in a folded-in state;

[0036] Figure 8 A cross-sectional view of a display cover provided in an embodiment of the present application in an outwardly folded state.

[0037] Among them, the reference numerals in the figure are:

[0038] 100. Display cover;

[0039] 10. Buffer layer;

[0040] 20. Base material layer;

[0041] 30. Support layer;

[0042] 40. Hardened layer;

[0043] 50. Adhesive layer;

[0044] 200. Display module;

[0045] 1000. Terminal device. DETAILED DESCRIPTION

[0046] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.

[0047] In the description of the present application, it should be understood that the terms "length", "width", "thickness", "top", "bottom", "inside", "outside", "up", "down", "left", "right", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0048] The terms "first", "second", "third", "fourth", etc. are only used to distinguish descriptions and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, the first push part and the second push part are only used to distinguish different push parts, and their order is not limited. The first push part can also be named as the second push part, and the second push part can also be named as the first push part without departing from the scope of the various described embodiments. And the terms "first", "second", "third", "fourth", etc. do not limit the indicated features to be different.

[0049] In this application, unless otherwise clearly specified and limited, the terms "connected", "connection" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0050] In this application, "and / or" is only a description of the association relationship of associated objects, indicating that there can be three relationships; for example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0051] It should be noted that, in this application, words such as "in one embodiment", "exemplarily", "for example", etc. are used to indicate examples, illustrations or descriptions. Any embodiment or design described in this application as "in one embodiment", "exemplarily", "for example" should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "in one embodiment", "exemplarily", "for example", etc. is intended to present related concepts in a specific way.

[0052] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0053] The display module of a terminal device with a foldable display screen usually includes a cover assembly, a display assembly and a support assembly. Among them, in order to obtain a better picture texture, the cover assembly is a glass cover assembly, which includes a glass cover body and an adhesive layer body arranged on the glass cover body, and is connected to the display assembly or other film materials by the adhesive layer body. However, after the processing of the glass cover body, some micro cracks will inevitably appear on the upper and lower surfaces of the glass cover body. When the glass cover assembly is impacted by external force, the upper surface of the glass cover body will be dented under the action of the impact force because the adhesive layer body is too soft. Then, the micro cracks on the lower surface away from the external force impact are gradually broken by the outward-expanding tensile force, which eventually leads to the rupture of the glass cover body.

[0054] In view of this, an embodiment of the present application provides a display cover plate, including a buffer layer, a substrate layer and a support layer arranged in sequence from top to bottom. Among them, the buffer layer and the support layer are attached to the opposite end faces of the substrate layer through a coating process, and the modulus of the buffer layer is smaller than the modulus of the support layer. In this way, the buffer layer and the support layer can fill the microcracks that may appear on the substrate layer, and when impacted by external force, the probability of further rupture of the microcracks is reduced. At the same time, the impact toughness of the support layer is higher than the impact toughness of the buffer layer, which can further reduce the microcracks on the lower surface away from the impact of external force. The expansion is caused by the tensile force, thereby improving the overall impact resistance of the substrate layer, and the anti-fracture performance of the display cover plate is more superior.

[0055] Please refer to Figure 3 , Figure 7 and Figure 8 , Figure 3 A cross-sectional view of a display cover plate 100 provided in an embodiment of the present application; Figure 7 A cross-sectional view of a display cover provided in an embodiment of the present application in a folded-in state; Figure 8 A cross-sectional view of a display cover provided in an embodiment of the present application in an outwardly folded state.

[0056] The display cover plate 100 provided in the present application includes a buffer layer 10, a substrate layer 20 and a support layer 30 arranged in sequence from top to bottom. The buffer layer 10 and the support layer 30 are coated on opposite end surfaces of the substrate layer 20, and the modulus of the buffer layer 10 is smaller than the modulus of the support layer 30.

[0057] Here, the buffer layer 10, the substrate layer 20 and the support layer 30 are stacked along the thickness direction of the display cover 100. The initial state of the buffer layer 10 and the support layer 30 should be a fluid state, which can flow on the two opposite end surfaces of the substrate layer 20, thereby filling the microcracks on the two opposite end surfaces of the substrate layer 20, and the final state of the buffer layer 10 and the support layer 30 should be a solid state, which can be stably formed on the substrate layer 20.

[0058] Modulus refers to the ratio of stress to strain of a material under stress. For example, the elastic modulus can be regarded as an indicator of the ease with which a material can produce elastic deformation. The larger its value, the greater the stress for a certain elastic deformation of the material, that is, the greater the stiffness of the material, the smaller the elastic deformation under a certain stress. At the same time, under different stress states, it can be divided into tensile modulus, shear modulus, bulk modulus, and longitudinal compression. For example, the external force impact is from the buffer layer 10 to the support layer 30 in the direction of the substrate layer 20, the buffer layer 10 is subjected to compressive stress, and its modulus can be a shear modulus, while the support layer 30 is subjected to tensile stress, and its modulus can be a tensile modulus.

[0059] The modulus of the buffer layer 10 being smaller than the modulus of the support layer 30 may mean that the deformation of the support layer 30 is smaller than that of the buffer layer 10, that is, the support layer 30 is difficult to deform, thereby supporting the lower end surface of the substrate layer 20 to reduce the expansion of microcracks on the end surface.

[0060] Here, since the display cover plate 100 is applied to the display module, the buffer layer 10 and the support layer 30 both have a certain light transmittance. In addition, the buffer layer 10 and the support layer 30 can be made of the same material, for example, resin or polyurethane. To meet the difference in modulus, the thickness of the buffer layer 10 and the support layer 30 can be different. Alternatively, the buffer layer 10 and the support layer 30 can also be made of different materials, and the size of the modulus of the two can be adjusted according to the difference in material properties.

[0061] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0062] The display cover plate 100 provided in the embodiment of the present application has a buffer layer 10 disposed on the upper surface of the substrate layer 20, and a support layer 30 disposed on the lower surface thereof, and the buffer layer 10 and the support layer 30 are both disposed on the substrate layer 20 by coating, and at the same time, the modulus of the buffer layer 10 is less than the modulus of the support layer 30. Since the substrate layer 20 has certain microcracks on its upper and lower surfaces after processing. During the assembly process, if it is directly or indirectly attached to a film material such as a display layer, the upper surface of the substrate layer 20 is prone to depression under the impact of external force, and the microcracks on the lower surface away from the impact of external force are extended by tensile force, so that the lower surface of the substrate layer 20 first breaks and causes the entire substrate layer 20 to break. After the support layer 30 is added to the lower surface of the substrate layer 20, it can resist the depression deformation caused by the impact of external force, and at the same time, the microcracks on the lower surface can be filled, which effectively reduces the microcracks on the substrate layer 20 when the substrate layer 20 is impacted by external force, resulting in the breakage of the substrate layer 20. Furthermore, after adding the buffer layer 10 to the upper surface of the substrate layer 20 , the microcracks on the upper surface can also be filled to reduce the probability of the microcracks extending, and at the same time, it can also withstand a certain external force impact, further improving the impact resistance of the substrate layer 20 .

[0063] In one embodiment, the substrate layer 20 includes a glass layer, the thickness of the substrate layer 20 is 20 μm to 100 μm, and the modulus of the substrate layer 20 is 63 GPa to 130 GPa.

[0064] Here, the glass layer may be ultra-thin glass or micro-ceramic ultra-thin glass.

[0065] The thickness of the substrate layer 20 may be 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, etc. Of course, in addition to the above integer values, decimal values ​​such as 20.3 μm, 40.13 μm and 90.98 μm may also be used.

[0066] The modulus of the substrate layer 20 is 63 GPa, 70 GPa, 75 GPa, 80 GPa, 85 GPa, 90 GPa, 95 GPa, 100 GPa, 105 GPa, 110 GPa, 115 GPa, 120 GPa, 125 GPa, 130 GPa, or the like.

[0067] In one embodiment, the buffer layer 10 is a light-transmitting flexible layer, and the buffer layer 10 includes one of organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane, or a combination of at least any two of them.

[0068] It can be understood that since the display cover plate 100 is disposed on the display module, the buffer layer 10 needs to meet light transmittance requirements.

[0069] The buffer layer 10 includes one of organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane; or is a combination of at least any two of organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane.

[0070] With such configuration, the buffer layer 10 has both light transmittance and impact resistance, and can improve the anti-cracking performance of the substrate layer 20 .

[0071] In one embodiment, the thickness of the buffer layer 10 is 10 μm to 60 μm, and the modulus of the buffer layer 10 is 0.5 MPa to 1000 MPa.

[0072] The buffer layer 10 may have a thickness of 10 μm, 12 μm, 15 μm, 20 μm, 22 μm, 25 μm, 30 μm, 32 μm, 35 μm, 40 μm, 42 μm, 45 μm, 50 μm, 52 μm, 55 μm, 60 μm, or the like.

[0073] The modulus of the buffer layer 10 is 0.5 MPa, 1 MPa, 10 MPa, 100 MPa, 120 MPa, 130 MPa, 140 MPa, 150 MPa, 200 MPa, 250 MPa, 300 MPa, 350 MPa, 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, 750 MPa, 800 MPa, 850 MPa, 1000 MPa, etc.

[0074] In one embodiment, the support layer 30 is a light-transmitting flexible layer, and the support layer 30 includes one or a combination of at least any two of polysilazane resin, polyimide, organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane.

[0075] It can be understood that, since the display cover plate 100 is disposed on the display module, the support layer 30 also needs to meet the light transmittance requirements.

[0076] The support layer 30 includes one of organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane; or is a combination of at least any two of organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane.

[0077] With such configuration, the support layer 30 has both light transmittance and impact resistance, and can improve the anti-cracking performance of the substrate layer 20 .

[0078] In one embodiment, the thickness of the support layer 30 is 2 μm to 25 μm, and the modulus of the buffer layer 10 is 0.5 GPa to 7 GPa.

[0079] The thickness of the substrate layer 20 may be 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 25 μm, etc.

[0080] The modulus of the substrate layer 20 is 0.5 GPa, 1 GPa, 1.2 GPa, 1.5 GPa, 2 GPa, 2.2 GPa, 2.5 GPa, 3 GPa, 3.2 GPa, 3.5 GPa, 4 GPa, 4.2 GPa, 4.5 GPa, 5 GPa, 5.2 GPa, 5.5 GPa, 6 GPa, 6.2 GPa, 6.5 GPa, 7 GPa, etc.

[0081] In one embodiment, the elongation at break of the buffer layer 10 at room temperature 25°C is ≥5%, and the elongation at break of the low temperature -20°C is ≥2%; and / or, the elongation at break of the support layer 30 at room temperature 25°C is ≥5%, and the elongation at break of the low temperature -20°C is ≥2%.

[0082] It can be understood that the current folding display terminals generally include inner folding products and outer folding products. Among them, when bending occurs, the inner folding product is that the buffer layer 10 in the display cover 100 is subjected to compressive stress, and the support layer 30 is subjected to tensile stress; the outer folding product is that the buffer layer 10 in the display cover 100 is subjected to tensile stress, and the support layer 30 is subjected to compressive stress. Therefore, in order to meet the use of two bending scenarios at the same time, and the display cover 100 does not break, the buffer layer 10 has a normal temperature 25°C fracture elongation rate of ≥5%, and a low temperature -20°C fracture elongation rate of ≥2%; and, the support layer 30 has a normal temperature 25°C fracture elongation rate of ≥5%, and a low temperature -20°C fracture elongation rate of ≥2%.

[0083] In other usage scenarios, only the buffer layer 10 has a normal temperature 25°C elongation rate ≥5%, and a low temperature -20°C elongation rate ≥2%; or, only the support layer 30 has a normal temperature 25°C elongation rate ≥5%, and a low temperature -20°C elongation rate ≥2%.

[0084] With such configuration, the buffer layer 10 and the support layer 30 can meet the structural strength required for the display cover plate 100 to be folded inwards or outwards when the elongation at break at room temperature 25° C. and / or the elongation at break at low temperature -20° C. are the same.

[0085] Please refer to Figure 4 In one embodiment, the display cover 100 further includes a hardening layer 40 , and the hardening layer 40 is disposed on an end surface of the buffer layer 10 that is away from the substrate layer 20 .

[0086] It can be understood that the function of the hardening layer 40 is to protect the upper surface of the substrate layer 20, improve the anti-scratch performance of the substrate layer 20, and to a certain extent keep the substrate layer 20 from breaking when impacted.

[0087] The initial state of the hardened layer 40 may be solid, directly attached to the buffer layer 10. Alternatively, the initial state of the hardened layer 40 is a fluid state, which can flow on the buffer layer 10 and finally solidify on the buffer layer 10, that is, in a solid state.

[0088] With such a configuration, the hardening layer 40 functions to reduce the probability of the substrate layer 20 being scratched, and to reduce the probability of the substrate layer 20 being broken when impacted by an external force.

[0089] In one embodiment, the hardening layer 40 includes one or a combination of at least any two of epoxy resin, acrylic resin, polyurethane and silicone.

[0090] It can be understood that, since the display cover plate 100 is disposed on the display module, the hardening layer 40 also needs to meet the light transmittance requirement.

[0091] The hardening layer 40 includes one of epoxy resin, acrylic resin, polyurethane and siloxane; or a combination of at least any two of epoxy resin, acrylic resin, polyurethane and siloxane.

[0092] In one embodiment, the thickness of the hardened layer 40 is 10 μm to 60 μm, the hardness of the hardened layer 40 is ≥ 2H, and the surface water drop angle of the hardened layer 40 is ≥ 90°.

[0093] The thickness of the substrate layer 20 may be 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, 22μm, 24μm, 26μm, 28μm, 30μm, 32μm, 34μm, 36μm, 38μm, 40μm, 42μm, 44μm, 46μm, 48μm, 50μm, 52μm, 54μm, 56μm, 58μm, 60μm, etc.

[0094] The hardness of the hardened layer 40 is ≥2H, which means that the hardened layer 40 can resist external impact to a certain extent.

[0095] The surface water drop angle is the contact angle, which refers to the angle between the tangent line of the gas-liquid interface at the intersection of the gas, liquid and solid phases and the solid-liquid boundary line on the liquid side, and is a measure of wettability. When the surface water drop angle is ≥90°, the rougher the surface of the hardened layer 40 is, the worse the wettability is.

[0096] Please refer to Figure 5 In one embodiment, the display cover 100 further includes an adhesive layer 50 , and the adhesive layer 50 is disposed on an end surface of the support layer 30 that is away from the substrate layer 20 .

[0097] It can be understood that the function of the adhesive layer 50 is to connect the support layer 30 to the external display panel or film material. The adhesive layer 50 can be one of OCA (Optically Clear Adhesive) optical glue or OCR (Optical Clear Resin) optical glue.

[0098] In this way, the adhesive layer 50 is used to adhere the substrate layer 20 to the display panel of the external device.

[0099] The following pen drop test is performed, where a 50μm adhesive layer 50 (OCA optical glue) and a 50μm polyethylene terephthalate layer are attached to the lower surface of the test sample and placed on a marble plate for testing. Among them, the hardening layer 40 in each test group is made of acrylic material, the buffer layer 10 is made of polyurethane with a modulus of 450MPa, the substrate layer 20 is glass with a thickness of 30μm, and the support layer 30 is made of polyimide with a modulus of 8000MPa. Please refer to the table below for specific data:

[0100] Solution 1 Solution 2 Solution 3 Solution 4 Solution 5 Solution 6 Hardened layer 40 / μm 5 5 5 5 5 5 Buffer layer 10 / μm / 15 / 25 15 15 Base material layer 20 / μm 30 30 30 30 30 30 Support layer 30 / μm / / 15 / 10 20 Pencil stroke / mm 10 15 40 25 60 62 Pencil hardness / H 6H 2H 5H HB 2H 2H

[0101] From the comparison results of Scheme 1, Scheme 2 and Scheme 3, it can be seen that coating the buffer layer 10 or the support layer 30 on the upper or lower surface of the substrate layer 20 can improve the writing of the substrate layer 20 to a certain extent. Adding a support protective layer on the lower surface of the substrate layer 20 has a better effect on the writing than adding a buffer protective layer on the upper surface of the substrate layer 20, and the surface hardness loss is less. From the comparison of Scheme 2 and Scheme 4, it can be seen that increasing the thickness of the buffer layer 10 on the upper surface of the substrate layer 20 can improve the writing height, but the hardness loss is large. From the comparison of Scheme 2, Scheme 4 and Scheme 5, it can be seen that adding a 10μm support layer 30 on the lower surface on the basis of Scheme 2 (Scheme 5) has basically no effect on the pencil hardness, but it has a better effect on the writing than adding 10μm of the buffer layer 10 on the upper surface of the substrate layer 20 (Scheme 4). From the comparison of Scheme 5 and Scheme 6, it can be seen that increasing the thickness of the support layer 30 on the lower surface of the substrate layer 20 from 10μm to 20μm has a certain effect on the writing, but the effect is not obvious. Considering that the increased thickness of the buffer layer 10 and the support layer 30 will affect the bending reliability, the thickness of the support layer 30 on the lower surface of the base layer 20 is preferably 20 μm or less.

[0102] Please refer to Figure 6In a specific embodiment, the display cover 100 includes a hardening layer 40, a buffer layer 10, a substrate layer 20, a support layer 30 and an adhesive layer 40 arranged in sequence from top to bottom, the buffer layer 10 and the support layer 30 are coated on the opposite end surfaces of the substrate layer 20, the modulus of the buffer layer 10 is less than the modulus of the support layer 30; the thickness of the hardening layer 40 is 10μm to 60μm, the hardness of the hardening layer 40 is ≥2H, and the surface water drop angle of the hardening layer 40 is ≥90°; the substrate layer 20 includes a glass layer, the thickness of the substrate layer 20 is 20μm to 100μm, and the modulus of the substrate layer 20 is 63GPa to 130GPa; the thickness of the buffer layer 10 is 10μm to 60μm, and the modulus of the buffer layer 10 is 0.5MPa to 1000MPa; the thickness of the support layer 30 is 2μm to 25 μm, the modulus of the buffer layer 10 is 0.5GPa~7GPa; the elongation at break of the buffer layer 10 at room temperature of 25℃ is ≥5%, and the elongation at break at low temperature of -20℃ is ≥2%; and / or, the elongation at break of the support layer 30 at room temperature of 25℃ is ≥5%, and the elongation at break at low temperature of -20℃ is ≥2%; the hardening layer 40 includes one or a combination of at least any two of epoxy resin, acrylic resin, polyurethane and siloxane; the buffer layer 10 is a light-transmitting flexible layer, and the buffer layer 10 includes one or a combination of at least any two of organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane; the support layer 30 is a light-transmitting flexible layer, and the support layer 30 includes one or a combination of at least any two of polysilazane resin, polyimide, organic resin, epoxy resin, acrylic resin, polyamide resin and polyurethane.

[0103] Please refer to Figure 2 , an embodiment of the present application provides a display module 200 , including the above-mentioned display cover 100 .

[0104] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0105] The display module 200 provided in the embodiment of the present application has a higher anti-cracking performance based on the above-mentioned display cover plate 100.

[0106] The display module 200 may also include a display panel, that is, a display screen with an output. The display cover 100 is disposed on the display end surface of the display screen to protect the display screen.

[0107] Please refer to Figure 1 , an embodiment of the present application provides a terminal device 1000, including the above-mentioned display module 200 or the display cover 100.

[0108] The above technical solutions in the embodiments of the present application have at least the following technical effects or advantages:

[0109] The terminal device 1000 provided in the embodiment of the present application has the above-mentioned display module 200 or display cover plate 100 , and the display end of the terminal device 1000 has higher impact resistance.

[0110] Here, the terminal device 1000 may be a mobile phone, a tablet computer, a wearable device (such as a smart watch), a vehicle-mounted device, etc., but is not limited thereto. In particular, it may refer to a terminal device 1000 whose display screen can be folded inward, folded outward, or folded inward and outward.

[0111] The above are only specific implementation methods of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be covered by the protection scope of the present application.

Claims

1. A display cover, characterized in that: The invention comprises a buffer layer, a substrate layer and a support layer which are arranged in sequence from top to bottom. The buffer layer and the support layer are coated on two opposite end surfaces of the substrate layer. The modulus of the buffer layer is smaller than that of the support layer.

2. The display cover according to claim 1, characterized in that: The substrate layer includes a glass layer, the thickness of the substrate layer is 20 μm to 100 μm, and the modulus of the substrate layer is 63 GPa to 130 GPa.

3. The display cover according to claim 1, characterized in that: The buffer layer is a light-transmitting flexible layer, and the buffer layer includes one of organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane, or a combination of at least any two of them.

4. The display cover according to claim 3, characterized in that: The thickness of the buffer layer is 10 μm to 60 μm, and the modulus of the buffer layer is 0.5 MPa to 1000 MPa.

5. The display cover according to any one of claims 1 to 4, characterized in that: The support layer is a light-transmitting flexible layer, and the support layer includes one of polysilazane resin, polyimide, organic resin, epoxy resin, acrylic resin, polyamide resin, and polyurethane, or a combination of at least any two of them.

6. The display cover according to claim 5, characterized in that: The thickness of the support layer is 2 μm to 25 μm, and the modulus of the buffer layer is 0.5 GPa to 7 GPa.

7. The display cover according to any one of claims 1 to 6, characterized in that: The buffer layer has a normal temperature 25°C elongation at break of ≥5%, and a low temperature -20°C elongation at break of ≥2%; and / or the support layer has a normal temperature 25°C elongation at break of ≥5%, and a low temperature -20°C elongation at break of ≥2%.

8. The display cover according to any one of claims 1 to 7, characterized in that: The display cover plate further includes a hardening layer, and the hardening layer is arranged on an end surface of the buffer layer away from the substrate layer.

9. The display cover according to claim 8, characterized in that: The hardening layer includes one or a combination of at least any two of epoxy resin, acrylic resin, polyurethane and siloxane.

10. The display cover plate according to claim 8, characterized in that: The thickness of the hardened layer is 10 μm to 60 μm, the hardness of the hardened layer is ≥2H, and the surface water drop angle of the hardened layer is ≥90°.

11. The display cover according to any one of claims 1 to 10, characterized in that: The display cover plate further comprises an adhesive layer, and the adhesive layer is arranged on an end surface of the support layer away from the substrate layer.

12. A display module, characterized in that: The invention comprises the display cover plate as claimed in any one of claims 1 to 11.

13. A terminal device, characterized in that: Comprising the display cover plate as described in any one of claims 1 to 11; or, the display module as described in claim 12.

Citation Information

Patent Citations

  • Display module and electronic equipment

    CN113972333A