Preparation method of high-fluidity composite permanent magnet material

Through the design of ultrasonic stirring and coating liquid, long-chain metal oxides are formed on the surface of SmFeN magnetic powder, which solves the problem of decomposition of SmFeN compounds at high temperatures and poor fluidity of composite materials, and realizes SmFeN composite permanent magnet materials with high fluidity and density Preparation improves the practicality of the material.

CN119069245APending Publication Date: 2024-12-03HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310632572.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The SmFeN compound will irreversibly decompose after the temperature exceeds 550°C, making it difficult for it to prepare dense magnets through traditional sintering processes. In the prior art, the flowability and coating density of composite permanent magnet materials are poor, which affects their usefulness.

Method used

The permanent magnet powder is mixed with the coating liquid by ultrasonic stirring, and then dried and kneaded to granulate. A coating liquid combined with specific organic phosphonic acid and inorganic acid is used to form long-chain metal oxides on the surface of the powder to improve the powder Tightness and fluidity, high-flow SmFeN composite permanent magnet material is obtained through twin screw extruder and injection molding.

Benefits of technology

It significantly improves the fluidity and intrinsic coercivity of composite permanent magnet materials, with the fluidity reaching 98g/10min or higher, and the intrinsic coercivity Hcj≥7.39KOe, which solves the problems of fluidity and density and improves the material's Practicality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-fluidity composite permanent magnet material, and the preparation method comprises the steps: carrying out the ultrasonic stirring of permanent magnet powder and a coating liquid, then carrying out the drying, mixing the dried material and resin, carrying out the mixing granulation, and then carrying out the molding, thereby obtaining the high-fluidity SmFeN composite permanent magnet material. The coating liquid comprises organic phosphonic acid, inorganic acid and a solvent. According to the preparation method provided by the invention, a reagent for coating is designed, a specific coating liquid formed by matching organic phosphonic acid and inorganic acid is adopted, and long-chain metal oxide is formed on the surfaces of powder particles by virtue of the organic phosphonic acid, so that compact coating of the powder is realized, and meanwhile, the flowability of the powder is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, and in particular to a method for preparing a high-fluidity composite permanent magnetic material. Background Art

[0002] At present, the saturation magnetization intensity of SmFeN compound is 1.54T, which is equivalent to 1.6T of NdFeB compound. The Curie temperature is 470℃ and the anisotropy field is 14T, both higher than NdFeB compound. The above excellent intrinsic magnetic properties make SmFeN compound considered to have the potential to become a new generation of rare earth permanent magnet materials.

[0003] For example, CN108777204A discloses a method for preparing samarium iron nitrogen permanent magnetic powder. Samarium iron alloy or samarium and iron pure metal and carbide balls are placed in a ball milling tank of a plasma-assisted ball milling device according to a certain material-ball ratio, and nitrogen or ammonia is introduced after vacuuming, and then plasma-assisted ball milling is performed to obtain samarium iron nitrogen permanent magnetic powder. The present invention performs plasma-assisted ball milling under the condition of introducing nitrogen or ammonia, and no impurities are generated during the preparation process, and the magnetic powder is not oxidized, which can effectively improve the efficiency of N entering the samarium iron alloy, and significantly improve the magnetic properties of the samarium iron nitrogen magnetic powder by forming a unique structure.

[0004] However, compared with NdFeB permanent magnet materials, the disadvantage of SmFeN compounds is that they will undergo irreversible decomposition when the temperature exceeds 550°C, so it is difficult to prepare dense magnets through traditional sintering processes. Therefore, SmFeN compounds are generally prepared by mixing with binders to prepare bonded magnets. The most commonly used method is to mix SmFeN magnetic powder with plastic binders such as PA and PPS at 200-300°C through a twin-screw mixing and granulation, and then injection molding at a slightly higher temperature (180-330°C) to make bonded magnets; but the permanent magnet composite materials currently prepared still have poor fluidity and poor coating density, resulting in poor practicality of the permanent magnet composite materials during use. Summary of the invention

[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing a high-fluidity composite permanent magnetic material to solve the problems of poor coating density and fluidity of the composite permanent magnetic material in the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for preparing a high-fluidity composite permanent magnetic material, the preparation method comprising:

[0008] The permanent magnetic powder and the coating liquid are ultrasonically stirred, and then dried, the dried material is mixed with a resin, kneaded and granulated, and then formed to obtain a high-fluidity SmFeN composite permanent magnetic material;

[0009] The coating solution comprises organic phosphonic acid, inorganic acid and solvent.

[0010] The preparation method provided by the present invention designs the coating reagents, adopts a coating liquid composed of a specific organic phosphonic acid and an inorganic acid, and forms a long-chain metal oxide on the surface of the powder particles with the help of organic phosphoric acid to achieve dense coating of the powder and increase the fluidity of the powder.

[0011] As a preferred technical solution of the present invention, the permanent magnetic powder includes SmFeN magnetic powder;

[0012] Preferably, the average particle size D50 of the permanent magnetic powder is 1-15 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable, preferably 2-5 μm.

[0013] As a preferred technical solution of the present invention, the mass ratio of organic phosphonic acid to inorganic acid in the coating solution is 100:(2-8), for example, it can be 100:2, 100:2.2, 100:2.4, 100:2.6, 100:2.8, 100:3, 100:3.2, 100:3.4, 100:3.6, 100:3.8, 100:4, 100:4.2, 100:4.4, 100:4.6, 100:4.8, 100:5, 100:5.2, 100:5.4, 100:5.6, 100:5.8, 100:6, 100:6.2, 100:6.4, 100:6.6, 100:6.8, 100:7, 100:7.2, 100:7.4, 100:7.6, 100:7.8 or 100:8, but not limited to the listed values, other unlisted values ​​within the range are also applicable, preferably 100:(5-6).

[0014] Preferably, the mass ratio of the permanent magnetic powder to the organic phosphonic acid is 100:(1-8), for example, it can be 100:1, 100:1.2, 100:1.4, 100:1.6, 100:1.8, 100:2, 100:2.2, 100:2.4, 100:2.6, 100:2.8, 100:3, 100:3.2, 100:3.4, 100:3.6, 100:3.8, 100:4, 100:4.2, 100:4.4, 100:4. 0:4.6, 100:4.8, 100:5, 100:5.2, 100:5.4, 100:5.6, 100:5.8, 100:6, 100:6.2, 100:6.4, 100:6.6, 100:6.8, 100:7, 100:7.2, 100:7.4, 100:7.6, 100:7.8 or 100:8, but not limited to the listed values, other unlisted values ​​within the range are also applicable, preferably 100:(5-6).

[0015] As a preferred technical solution of the present invention, the organic phosphonic acid includes one or a combination of at least two of tetradecylphosphonic acid, 1-dodecylphosphonic acid, octadecylphosphonic acid, octylphosphonic acid, hexylphosphonic acid or decylphosphonic acid.

[0016] Preferably, the inorganic acid comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid.

[0017] Preferably, the solvent comprises n-butanol.

[0018] Preferably, the amount of the solvent added is 10-12% of the mass of the permanent magnetic powder, for example, it can be 10%, 10.1%, 10.2%, 10.3%, 10.4%, 10.5%, 10.6%, 10.7%, 10.8%, 10.9%, 11%, 11.1%, 11.2%, 11.3%, 11.4%, 11.5%, 11.6%, 11.7%, 11.8%, 11.9% or 12%, etc., but is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0019] As a preferred technical solution of the present invention, the power of the ultrasound in the ultrasonic stirring is 800-1300W, for example, it can be 800W, 820W, 840W, 860W, 880W, 900W, 920W, 940W, 960W, 980W, 1000W, 1020W, 1040W, 1060W, 1080W, 1100W, 1120W, 1140W, 1160W, 1180W, 1200W, 1220W, 1240W, 1260W, 1280W or 1300W, but is not limited to the listed values, and other unlisted values ​​within the range are equally applicable.

[0020] Preferably, the frequency of ultrasound in the ultrasonic stirring is 80-100kHz, for example, it can be 80kHz, 81kHz, 82kHz, 83kHz, 84kHz, 85kHz, 86kHz, 87kHz, 88kHz, 89kHz, 90kHz, 91kHz, 92kHz, 93kHz, 94kHz, 95kHz, 96kHz, 97kHz, 98kHz, 99kHz or 100kHz, but is not limited to the listed values, and other unlisted values ​​within the range are equally applicable.

[0021] Preferably, the stirring rate in the ultrasonic stirring is 1200-1500r / min, for example, it can be 1200r / min, 1220r / min, 1240r / min, 1260r / min, 1280r / min, 1300r / min, 1320r / min, 1340r / min, 1360r / min, 1380r / min, 1400r / min, 1420r / min, 1440r / min, 1460r / min, 1480r / min or 1500r / min, but is not limited to the listed values, and other values ​​not listed in this range are also applicable.

[0022] Preferably, the ultrasonic stirring time is 30-60 min, for example, it can be 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0023] As a preferred technical solution of the present invention, the drying temperature is 60-80°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C or 80°C, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0024] Preferably, the drying time is 30-45 min, for example, it can be 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min, 40 min, 41 min, 42 min, 43 min, 44 min or 45 min, but is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0025] As a preferred technical solution of the present invention, the particle size of the material obtained in the mixing is ≤0.18 mm. Specifically, it can be all particles within a certain particle size range, such as all particles within a particle size range of 0.01-0.05 mm, or all particles ≤ a certain particle size, such as all particles within ≤0.1 mm.

[0026] As a preferred technical solution of the present invention, the mass ratio of the material obtained in the mixing to the resin is 100:(7-9), for example, it can be 100:7, 100:7.1, 100:7.2, 100:7.3, 100:7.4, 100:7.5, 100:7.6, 100:7.8, 100:7.9, 100:8, 100:8.1, 100:8.2, 100:8.3, 100:8.4, 100:8.5, 100:8.6, 100:8.7, 100:8.8, 100:8.9 or 100:9, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0027] As a preferred technical solution of the present invention, the resin includes polyphenylene sulfide resin.

[0028] Preferably, the molding is injection molding.

[0029] As a preferred technical solution of the present invention, the preparation method comprises: ultrasonically stirring the permanent magnetic powder and the coating liquid, then drying, mixing the dried material with a resin and kneading and granulating, and then molding to obtain a high-fluidity SmFeN composite permanent magnetic material;

[0030] The permanent magnetic powder includes SmFeN magnetic powder; the average particle size D50 of the permanent magnetic powder is 2-5 μm;

[0031] The coating liquid comprises an organic phosphonic acid, an inorganic acid and a solvent; the organic phosphonic acid comprises one or a combination of at least two of tetradecylphosphonic acid, 1-dodecylphosphonic acid, octadecylphosphonic acid, octylphosphonic acid, hexylphosphonic acid or decylphosphonic acid; the inorganic acid comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid; the solvent comprises n-butanol; the amount of the solvent added is 10-12% of the mass of the permanent magnetic powder; the mass ratio of the organic phosphonic acid to the inorganic acid in the coating liquid is 100:(5-6); the mass ratio of the permanent magnetic powder to the organic phosphonic acid is 100:(5-6);

[0032] The power of the ultrasound in the ultrasonic stirring is 800-1300W; the frequency of the ultrasound in the ultrasonic stirring is 80-100kHz; the stirring rate in the ultrasonic stirring is 1200-1500r / min; the time of the ultrasonic stirring is 30-60min;

[0033] The drying temperature is 60-80°C; the drying time is 30-45 minutes;

[0034] The particle size of the material obtained in the mixing is ≤0.18 mm; the mass ratio of the material obtained in the mixing to the resin is 100:(7-9); the resin includes polyphenylene sulfide resin; and the molding is injection molding.

[0035] In the present invention, all reagents used are pure compound reagents. For example, inorganic acids are analytically pure reagents as raw materials, such as sulfuric acid using analytically pure concentrated sulfuric acid, hydrochloric acid using analytically pure hydrochloric acid, and the like. The same can be said for the reagents mentioned in the present invention. In other words, the reagents mentioned in the present invention can be relatively pure reagents in the prior art as far as possible without specific restrictions.

[0036] In the present invention, the mixing and granulation can be carried out by a twin-screw extruder, and the injection molding can be carried out by an injection molding machine; wherein the control parameters of the mixing and granulation process can be a control temperature of 200-250°C and a screw main engine speed of 300-400r / min.

[0037] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0038] The preparation method provided by the present invention forms a long-chain metal oxide on the surface of the permanent magnetic material by means of a specific coating material, organic phosphonic acid, to achieve dense coating of the powder and increase the fluidity of the powder, thereby preparing a composite permanent magnetic material with better fluidity. The fluidity (g / 10min) of the composite permanent magnetic material is ≥98, and in a more preferred range the fluidity can reach above 139, and the intrinsic coercive force Hcj is ≥7.39KOe. DETAILED DESCRIPTION

[0039] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0040] Example 1

[0041] This embodiment provides a method for preparing a high-fluidity composite permanent magnetic material, which is specifically as follows:

[0042] (1) SmFeN magnetic powder with an average particle size D50 of 3 μm is selected as the raw material powder, and the specific composition is Sm2Fe17Nx.

[0043] (2) preparing a coating solution, adding an inorganic acid and an organic phosphonic acid into a solvent at the same time, wherein the organic phosphonic acid is octylphosphonic acid and the inorganic acid is sulfuric acid; the mass ratio of sulfuric acid to octylphosphonic acid is 6:100; the mass ratio of octylphosphonic acid to 3 μm SmFeN magnetic powder is 5:100; and n-butanol is used as a solvent, and the added amount is 10% of the mass of the SmFeN magnetic powder.

[0044] (3) SmFeN magnetic powder with a particle size of 3 μm was added to the prepared coating solution, placed in an ultrasonic generator, and stirred while ultrasonicating (ultrasonic power of 1000 W, ultrasonic frequency of 90 kHz, stirring rate of 1350 r / min) for 40 minutes.

[0045] (4) The above powders were placed in an oven and dried at 60°C for 30 minutes. The dried powders were passed through an 80-mesh sieve to obtain high-fluidity SmFeN powders.

[0046] (5) The above powder was mixed with polyphenylene sulfide resin in a mass ratio of 100:8.

[0047] (6) The mixed powder is kneaded and granulated using a twin-screw extruder to obtain granules for injection molding, and the fluidity thereof is tested.

[0048] (7) The granular material is injection molded in an injection molding machine to obtain a target product, and the performance is tested.

[0049] The properties of the obtained products are shown in Table 1.

[0050] Example 2

[0051] The only difference from Example 1 is that the organic phosphonic acid is replaced by an equal amount of decyl phosphoric acid. The properties of the obtained product are shown in Table 1.

[0052] Example 3

[0053] The only difference from Example 1 is that the organic phosphonic acid is replaced by tetradecylphosphonic acid. The properties of the obtained product are shown in Table 1.

[0054] Example 4

[0055] The only difference from Example 1 is that the mass ratio of sulfuric acid to organic phosphonic acid is 3:100. The properties of the obtained product are shown in Table 1.

[0056] Example 5

[0057] The only difference from Example 1 is that the mass ratio of sulfuric acid to organic phosphonic acid is 8:100. The properties of the obtained product are shown in Table 1.

[0058] Example 6

[0059] The only difference from Example 1 is that the mass ratio of organic phosphonic acid to SmFeN magnetic powder is 1:100. The properties of the obtained product are shown in Table 1.

[0060] Example 7

[0061] The only difference from Example 1 is that the mass ratio of organic phosphonic acid to SmFeN magnetic powder is 8:100. The properties of the obtained product are shown in Table 1.

[0062] Example 8

[0063] The only difference from Example 1 is that the ultrasonic stirring reaction time is 30 minutes. The properties of the obtained product are shown in Table 1.

[0064] Example 9

[0065] The only difference from Example 1 is that the ultrasonic stirring reaction time is 60 minutes. The properties of the obtained product are shown in Table 1.

[0066] Comparative Example 1

[0067] The only difference from Example 1 is that the powder is directly replaced with an equal amount of SmFeN magnetic powder starting from step (5). The properties of the obtained product are shown in Table 1.

[0068] Comparative Example 2

[0069] The only difference from Example 1 is that the inorganic acid in the preparation process is replaced by an equal amount of acetic acid. The properties of the obtained product are shown in Table 1.

[0070] Comparative Example 3

[0071] The only difference from Example 1 is that the organic phosphonic acid in the preparation process is replaced by phosphoric acid (H3PO4). The properties of the obtained product are shown in Table 1.

[0072] Comparative Example 4

[0073] The only difference from Example 1 is that the organic phosphonic acid used in the preparation process is replaced by n-octanoic acid. The properties of the obtained product are shown in Table 1.

[0074] The intrinsic coercive force and fluidity of the product obtained in the above implementation process are tested by using the NIM-2000H permanent magnet precision measurement system developed and produced by the China Institute of Metrology to measure the coercive force, and the Jenike shear tester to measure the fluidity of the granular material.

[0075] Table 1

[0076] Sample <![CDATA[H cj (YOU)]]> Fluidity (g / 10min) Example 1 7.59 178 Example 2 7.39 162 Example 3 7.51 139 Example 4 7.55 98 Example 5 5.72 106 Example 6 7.26 129 Example 7 7.35 173 Example 8 7.49 153 Example 9 7.52 168 Comparative Example 1 7.58 59 Comparative Example 2 7.32 116 Comparative Example 3 7.38 121 Comparative Example 4 7.28 109

[0077] It can be seen from the results of the above examples that the preparation method provided by the present invention, by designing the reagents used for coating, adopting a coating liquid composed of a specific organic phosphonic acid and an inorganic acid, and using organic phosphoric acid to form long-chain metal oxides on the surface of the powder particles, achieves dense coating of the powder and increases the fluidity of the powder.

[0078] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0079] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0080] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0081] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a high-fluidity composite permanent magnetic material, characterized in that: The preparation method comprises: The permanent magnetic powder and the coating liquid are ultrasonically stirred, and then dried, the dried material is mixed with a resin, kneaded and granulated, and then formed to obtain a high-fluidity SmFeN composite permanent magnetic material; The coating solution comprises organic phosphonic acid, inorganic acid and solvent.

2. The preparation method according to claim 1, characterized in that: The permanent magnetic powder includes SmFeN magnetic powder; Preferably, the average particle size D50 of the permanent magnetic powder is 1-15 μm, preferably 2-5 μm.

3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the organic phosphonic acid to the inorganic acid in the coating solution is 100:(2-8), preferably 100:(5-6); Preferably, the mass ratio of the permanent magnetic powder to the organic phosphonic acid is 100:(1-8), preferably 100:(5-6).

4. The preparation method according to any one of claims 1 to 3, characterized in that: The organic phosphonic acid comprises one or a combination of at least two of tetradecylphosphonic acid, 1-dodecylphosphonic acid, octadecylphosphonic acid, octylphosphonic acid, hexylphosphonic acid or decylphosphonic acid; Preferably, the inorganic acid comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid; Preferably, the solvent comprises n-butanol; Preferably, the added amount of the solvent is 10-12% of the mass of the permanent magnetic powder.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The power of the ultrasound in the ultrasonic stirring is 800-1300W; Preferably, the frequency of ultrasound in the ultrasonic stirring is 80-100 kHz; Preferably, the stirring rate in the ultrasonic stirring is 1200-1500 r / min; Preferably, the ultrasonic stirring time is 30-60 min.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The drying temperature is 60-80°C; Preferably, the drying time is 30-45 minutes.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The particle size of the material obtained in the mixing is ≤0.18 mm.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The mass ratio of the material obtained in the mixing to the resin is 100:(7-9).

9. The preparation method according to any one of claims 1 to 8, characterized in that: The resin includes polyphenylene sulfide resin; Preferably, the molding is injection molding.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method comprises: The permanent magnetic powder and the coating liquid are ultrasonically stirred, and then dried, the dried material is mixed with a resin, kneaded and granulated, and then formed to obtain a high-fluidity SmFeN composite permanent magnetic material; The permanent magnetic powder includes SmFeN magnetic powder; the average particle size D50 of the permanent magnetic powder is 2-5 μm; The coating liquid comprises an organic phosphonic acid, an inorganic acid and a solvent; the organic phosphonic acid comprises one or a combination of at least two of tetradecylphosphonic acid, 1-dodecylphosphonic acid, octadecylphosphonic acid, octylphosphonic acid, hexylphosphonic acid or decylphosphonic acid; the inorganic acid comprises one or a combination of at least two of sulfuric acid, nitric acid or hydrochloric acid; the solvent comprises n-butanol; the amount of the solvent added is 10-12% of the mass of the permanent magnetic powder; the mass ratio of the organic phosphonic acid to the inorganic acid in the coating liquid is 100:(5-6); the mass ratio of the permanent magnetic powder to the organic phosphonic acid is 100:(5-6); The power of the ultrasound in the ultrasonic stirring is 800-1300W; the frequency of the ultrasound in the ultrasonic stirring is 80-100kHz; the stirring rate in the ultrasonic stirring is 1200-1500r / min; the time of the ultrasonic stirring is 30-60min; The drying temperature is 60-80°C; the drying time is 30-45 minutes; The particle size of the material obtained in the mixing is ≤0.18 mm; the mass ratio of the material obtained in the mixing to the resin is 100:(7-9); the resin includes polyphenylene sulfide resin; and the molding is injection molding.