Samarium cobalt permanent magnet and preparation method thereof
By strictly controlling the oxidation heat treatment and sintering process of samarium-cobalt alloy, the problem of insufficient strength and toughness of samarium-cobalt permanent magnets is solved, and the balance of high bending strength and hard magnetic properties is achieved, which is suitable for industrial production, and the stability of magnets is improved and consistency.
Patent Information
- Application Number
- CN202411145159.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The strength and toughness of samarium-cobalt permanent magnets are less strong, resulting in easy cracking and slag loss during processing, reducing yield and processing accuracy, and limiting their application in high-precision, earthquake resistance, impact resistance and other fields.
By strictly controlling the oxidation heat treatment process of samarium-cobalt alloy, including the insulation time, heating temperature and vacuum degree of oxidation heat treatment, the oxide content and distribution can be regulated, combined with crushing, powdering and sintering treatment, the samarium-cobalt permanent magnet is produced, and the improvement of the oxidation heat treatment is improved. Its bending strength.
It achieves the high bending strength improvement of samarium-cobalt permanent magnets, while maintaining hard magnetic properties, simplifies the preparation process, is suitable for industrial production, and improves the consistency and stability of the magnetic and mechanical properties of the magnets.
Smart Images

Figure CN119069246A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of permanent magnet preparation, in particular to a samarium cobalt permanent magnet and a preparation method thereof. Background Art
[0002] As the second generation of rare earth permanent magnet materials, samarium cobalt permanent magnet materials have significant advantages such as high Curie temperature, high magnetic energy product, excellent temperature stability and strong corrosion resistance. They are widely used in cutting-edge equipment in the fields of magnetic power, sensing and communication, and play an irreplaceable role in aerospace, radar communications and national defense industry.
[0003] However, due to the intrinsic crystal structure, strong magnetic anisotropy, orientation molding process, and internal stress and defects generated during the sintering process of rare earth permanent magnets, the strength and toughness of the magnets are poor. Among them, samarium cobalt permanent magnets are cleavage brittle fractures, and the bending strength is usually only 80MPa-120MPa, which makes samarium cobalt permanent magnets easy to crack and slag during processing, which greatly reduces the yield and processing accuracy of the magnets, increases the processing cost of the magnets, and limits the application of magnets in high-precision, earthquake-resistant, and impact-resistant fields.
[0004] The existing technology achieves mechanical strength improvement by pre-oxidizing ultrafine powder (0.01μm-2μm) to make its oxygen content as high as 4000ppm-10000ppm, and then mixing it with conventional powder in proportion. However, these methods of adding additives or mixing multiple materials with each other not only increase costs, but also make it difficult to ensure uniform mixing. For example, when adding samarium oxide, it is easy to agglomerate, and after adding ultrafine powder oxide, fine grains are concentrated, resulting in local stress concentration in the magnet, which reduces the consistency and stability of the magnetic and mechanical properties of the magnet.
[0005] Therefore, how to improve the toughness of SmCo permanent magnets while ensuring their high hard magnetic properties has become an urgent and important problem. Summary of the invention
[0006] Based on this, it is necessary to provide a samarium cobalt permanent magnet and a preparation method thereof to address the above problems; the preparation method can achieve a significant improvement in bending strength while ensuring the high hard magnetic properties of the samarium cobalt permanent magnet, and the preparation process is simple and efficient, and is suitable for industrial production.
[0007] A method for preparing a samarium cobalt permanent magnet comprises the following steps:
[0008] Provide samarium cobalt alloy;
[0009] The samarium-cobalt alloy is subjected to an oxidation heat treatment, wherein the oxidation heat treatment process satisfies the following relationship: t=kP / T, wherein t is the holding time, in units of h; T is the heating temperature, in units of °C; P is the vacuum degree, in units of Pa; k is a coefficient, k=100-5000;
[0010] Crushing and pulverizing the samarium-cobalt alloy after the oxidation heat treatment to obtain alloy powder;
[0011] The alloy powder is oriented and molded to obtain a samarium-cobalt green body, and then a samarium-cobalt permanent magnet is obtained through a sintering treatment.
[0012] In one embodiment, the heating temperature T is 300°C-1200°C;
[0013] And / or, the vacuum degree P is 0.1Pa-20Pa.
[0014] In one embodiment, when P ≥ 10Pa, 100 ≤ k ≤ 300, 300°C ≤ T < 600°C;
[0015] Or, when 5Pa≤P<10Pa, 200 <k≤500,500℃<T<800℃;
[0016] Or, when 1Pa≤P<5Pa, 400 <k≤800,700℃<T<1000℃;
[0017] Or, when 0.1Pa≤P<1Pa, 800 <k≤3000,900℃<T≤1200℃。
[0018] In one embodiment, the composition of the samarium-cobalt alloy includes: 23%-28% Sm, 13%-25% Fe, 4%-10% Cu, 1.5%-3.5% Zr and the balance Co.
[0019] In one embodiment, the thickness of the oxide layer on the surface of the samarium-cobalt alloy after the oxidation heat treatment is 1 μm-5 μm;
[0020] And / or, the oxygen content of the samarium-cobalt alloy after the oxidation heat treatment is 1500ppm-4000ppm.
[0021] In one embodiment, the particle size of the coarse particles obtained by crushing is less than 5 mm;
[0022] And / or, the average particle size of the alloy powder is 3 μm-8 μm, and the maximum particle size is less than or equal to 35 μm.
[0023] In one embodiment, in the orientation forming step, the magnetic field strength is greater than or equal to 2T;
[0024] And / or, the density of the samarium cobalt green body is 4.5 g / cm 3 -5.5g / cm 3 .
[0025] In one embodiment, the sintering treatment includes sintering and solid solution treatment, and the sintering and solid solution treatment process includes: under the condition of vacuum degree less than or equal to 0.05Pa, heating to 1130℃-1180℃ at a heating rate of 0.5℃ / min-10℃ / min and keeping warm for 0.5h-5h for pre-sintering, then heating to 1170℃-1240℃ in an inert gas environment and keeping warm for 1h-8h for sintering, then cooling to 1110℃-1180℃ at a cooling rate of 0.2℃ / min-5℃ / min and keeping warm for 2h-72h for solid solution treatment, and after the solid solution treatment, rapid quenching to below 400℃ at a cooling rate of 40℃ / min-200℃ / min;
[0026] And / or, the sintering treatment also includes tempering and aging, and the tempering and aging process includes: in an inert gas environment or under a vacuum degree of ≤0.1Pa, heating the temperature to 750℃-900℃ at a heating rate of 0.5℃ / min-10℃ / min and keeping it for 1h-50h, and then cooling the temperature to 300℃-500℃ at a cooling rate of 0.1℃ / min-1℃ / min and keeping it for 1h-30h.
[0027] A samarium cobalt permanent magnet is prepared by the preparation method as described above, and the oxygen content of the samarium cobalt permanent magnet is 3500ppm-6000ppm.
[0028] In one embodiment, the average grain size of the samarium cobalt permanent magnet is 30 μm-80 μm;
[0029] And / or, the maximum grain size of the samarium cobalt permanent magnet is less than 170 μm.
[0030] The preparation method of the present invention achieves the regulation of oxide content and distribution by strictly controlling the process conditions during the oxidation heat treatment of the samarium cobalt alloy, thereby ensuring that the hard magnetic properties of the magnet are not damaged while achieving high bending strength, and effectively improving the component segregation of the samarium cobalt alloy, further optimizing the consistency and stability of the magnet, and then, relying on high melting point oxides to refine the grains of the samarium cobalt magnet and hinder crack propagation, thereby achieving a significant increase in bending strength. In addition, the samarium cobalt alloy after the oxidation heat treatment is subjected to processes such as powdering, so that the oxides are evenly dispersed in the magnet, and a relatively uniform distribution of oxides or fine grains in the magnet can be achieved, which is conducive to further enhancing the good consistency and stability of the magnetic and mechanical properties of the magnet.
[0031] Therefore, the preparation method of the present invention not only successfully achieves the balance between the high hard magnetic properties and high bending strength of the samarium cobalt permanent magnet, but also does not need to add external additives or materials to the samarium cobalt alloy. The preparation method is simple, efficient and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 This is a scanning electron microscope (SEM) image of the cross section of the oxidized samarium-cobalt alloy prepared in Example 1;
[0034] Figure 2 This is a metallographic photograph of the samarium cobalt permanent magnet obtained in Example 1;
[0035] Figure 3 This is a metallographic photograph of the samarium cobalt permanent magnet obtained in Comparative Example 1;
[0036] Figure 4 This is a scanning electron microscope (SEM) image of the cross section of the samarium-cobalt alloy after oxidation prepared in Comparative Example 3;
[0037] Figure 5 This is a metallographic photograph of the samarium cobalt permanent magnet prepared in Comparative Example 4. DETAILED DESCRIPTION
[0038] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0040] The present invention provides a method for preparing a samarium cobalt permanent magnet, comprising the following steps:
[0041] S1, providing samarium cobalt alloy;
[0042] S2, performing oxidation heat treatment on the samarium-cobalt alloy, wherein the oxidation heat treatment process satisfies the following relationship: t=kP / T, wherein t is the holding time, in h; T is the heating temperature, in °C; P is the vacuum degree, in Pa; k is a coefficient, k=100-5000;
[0043] S3, crushing and powdering the samarium-cobalt alloy after the oxidation heat treatment to obtain alloy powder;
[0044] S4, after orienting and molding the alloy powder to obtain a samarium-cobalt green body, sintering the green body to obtain a samarium-cobalt permanent magnet.
[0045] The present invention does not limit the samarium-cobalt alloy used in step S1. Existing samarium-cobalt alloys can be used, or the raw metal can be poured into a crucible for induction smelting, and then poured into a water-cooled mold to prepare a master alloy ingot after being melted into molten steel.
[0046] In one embodiment, the composition of the samarium-cobalt alloy includes: 23%-28% Sm, 13%-25% Fe, 4%-10% Cu, 1.5%-3.5% Zr and the balance Co.
[0047] In step S2, by strictly controlling the process conditions during the oxidation heat treatment of the samarium cobalt alloy, the oxide content and distribution can be regulated, thereby ensuring that the hard magnetic properties of the magnet are not damaged while achieving high bending strength, and effectively improving the composition segregation of the samarium cobalt alloy, further optimizing the consistency and stability of the magnet, and then, relying on high melting point oxides to refine the grains of the samarium cobalt magnet and hinder crack propagation, achieving a significant increase in bending strength.
[0048] It should be noted that the relationship formula of the oxidation heat treatment process is only a quantitative relationship conversion and does not involve unit conversion.
[0049] Preferably, the heating temperature T is 300°C-1200°C, including but not limited to any one of 300°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, and 1200°C, or a range consisting of any two of the values.
[0050] Preferably, the vacuum degree P is 0.1Pa-20Pa, including but not limited to any one point value of 0.1Pa, 0.5Pa, 1Pa, 5Pa, 10Pa, 15Pa, and 20Pa, or a range value consisting of any two point values.
[0051] In one embodiment, when P ≥ 10 Pa, 100 ≤ k ≤ 300, 300 °C ≤ T < 600 °C. Preferably, when 10 Pa ≤ P < 20 Pa, 100 ≤ k ≤ 200, 500 °C ≤ T < 600 °C.
[0052] In one embodiment, when 5 Pa ≤ P < 10 Pa, 200 < k ≤ 500, 500 °C < T < 800 °C. Preferably, 600 °C ≤ T < 800 °C.
[0053] In one embodiment, when 1 Pa ≤ P < 5 Pa, 400 < k ≤ 800, 700 °C < T < 1000 °C. Preferably, when 1 Pa ≤ P < 5 Pa, 500 < k ≤ 800, 800 °C ≤ T ≤ 900 °C.
[0054] In one embodiment, when 0.1 Pa ≤ P < 1 Pa, 800 < k ≤ 3000, 900 °C < T ≤ 1200 °C.
[0055] In one embodiment, the thickness of the surface oxide layer of the samarium cobalt alloy after oxidation heat treatment is 1 μm - 5 μm, including but not limited to any one point value among 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm or the range value formed by any two point values.
[0056] In one embodiment, the oxygen content of the samarium cobalt alloy after oxidation heat treatment is 1500 ppm - 4000 ppm, including but not limited to any one point value among 1500 ppm, 2000 ppm, 2500 ppm, 3000 ppm, 3500 ppm, 4000 ppm or the range value formed by any two point values.
[0057] In step S3, processes such as powder making are performed on the samarium cobalt alloy after oxidation heat treatment to uniformly disperse the oxides in the magnet, so that a relatively uniform distribution of oxides or fine grains in the magnet can be achieved, which is beneficial to further enhancing the magnetic properties of the magnet and the consistency and stability of mechanical properties.
[0058] In one embodiment, the crushing process includes but is not limited to mechanical crushing, and mechanical crushing is preferred in the present invention.
[0059] In one embodiment, the particle size of the coarse particles obtained by crushing is less than 5 mm.
[0060] In one embodiment, the powder making process includes but is not limited to jet milling or ball milling.
[0061] In one embodiment, the specific surface average particle size (SMD) of the alloy powder is 3 μm - 8 μm, and the maximum particle size in the alloy powder is less than or equal to 35 μm.
[0062] The present invention does not limit the orientation molding and sintering process used in step S4, and existing processes can be used.
[0063] In one embodiment, the orientation forming process comprises: orienting the alloy powder under the action of a magnetic field, and further isostatic pressing to obtain a samarium-cobalt green body.
[0064] Preferably, the magnetic field intensity of the orientation molding is greater than or equal to 2T; the density of the compact after magnetic field orientation molding is preferably 3.5g / cm 3 -4.5g / cm 3 The density of the samarium-cobalt green body obtained after isostatic pressing is preferably 4.5 g / cm 3 -5.5g / cm 3 .
[0065] In one embodiment, the sintering process includes sintering solid solution and tempering aging, wherein the sintering solid solution includes: oxygen-free sintering of the samarium cobalt green body, solid solution treatment after sintering to denseness, and rapid quenching and cooling after the solid solution is completed.
[0066] Preferably, the sintering and solution treatment process specifically includes the following steps: under the condition of a vacuum degree less than or equal to 0.05 Pa, heating to 1130℃-1180℃ at a heating rate of 0.5℃ / min-10℃ / min and keeping warm for 0.5h-5h for pre-sintering, then heating to 1170℃-1240℃ in an inert gas environment and keeping warm for 1h-8h for sintering, then cooling to 1110℃-1180℃ at a cooling rate of 0.2℃ / min-5℃ / min and keeping warm for 2h-72h for solution treatment, and after the solution treatment, rapidly quenching to below 400℃ at a cooling rate of 40℃ / min-200℃ / min.
[0067] It should be noted that the present invention is not limited to one-step or multiple-step treatment for each stage in the above-mentioned sintering and solution treatment process. For example, in the pre-sintering process, it can be first heated to 300°C and kept warm for 1 hour, then heated to 800°C and kept warm for 1.5 hours, and then heated to the pre-sintering temperature, or directly heated to the pre-sintering temperature; in the solution treatment process, the temperature can be first cooled to 1170°C and kept warm for 2 hours, then cooled to 1150°C and kept warm for 4 hours, then cooled to 1130°C and kept warm for 10 hours, or directly cooled to the solution treatment temperature.
[0068] In one embodiment, the tempering aging process preferably includes the following steps: in an inert gas environment or under a vacuum degree of ≤0.1 Pa, heating to 750°C-900°C at a heating rate of 0.5°C / min-10°C / min and keeping warm for 1h-50h, and then cooling to 300°C-500°C at a cooling rate of 0.1°C / min-1°C / min and keeping warm for 1h-30h.
[0069] It should be noted that the present invention is not limited to one or more steps for each stage in the above-mentioned tempering and aging process. For example, in the heating process, it can be first heated to 300°C and kept for 1 hour, then heated to 600°C and kept for 2 hours, and then heated to the primary aging temperature, or heated to the tempering temperature in one step; the cooling process can be first cooled to 700°C and kept for 2 hours, then cooled to 600°C and kept for 4 hours, and then cooled to the final aging temperature, or cooled to the secondary aging temperature in one step.
[0070] Therefore, the preparation method of the present invention not only successfully achieves the balance between the high hard magnetic properties and high bending strength of the samarium cobalt permanent magnet, but also does not need to add external additives or materials to the samarium cobalt alloy. The preparation method is simple, efficient and suitable for industrial production.
[0071] The present invention also provides a samarium cobalt permanent magnet, which is prepared by the preparation method as described above, and the oxygen content of the samarium cobalt permanent magnet is 3500ppm-6000ppm, including but not limited to any one point value of 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, and 6000ppm, or a range value consisting of any two point values.
[0072] In one embodiment, the average grain size of the samarium cobalt permanent magnet is 30 μm-80 μm, including but not limited to any one point value of 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, and 80 μm, or a range value consisting of any two point values.
[0073] In one embodiment, the maximum grain size of the samarium cobalt permanent magnet is less than 170 μm, including but not limited to any one of 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, and 150 μm, or a range consisting of any two of the values.
[0074] The samarium cobalt permanent magnet and its preparation method will be further described below by the following specific examples. However, those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0075] Example 1
[0076] 100 kg of raw metals were prepared by induction melting with 25% Sm, 17% Fe, 5% Cu, 3% Zr, and the balance Co, and then the ingot was prepared. The ingot was subjected to oxidation heat treatment: the ingot was heated to 1000°C for 1 hour under a vacuum of 0.5 Pa, and then cooled to room temperature. The cross section of the oxidized SmCo alloy ingot was characterized by scanning electron microscopy (SEM), as shown in FIG. Figure 1 As shown, it can be found that the thickness of the ingot oxide layer is about 3.5μm, and the overall oxygen content of the ingot is further measured to be 2684ppm.
[0077] The ingot was then mechanically crushed into coarse particles less than 1 mm, and then jet milled to prepare powder with a specific surface average particle size (SMD) of 4.35 μm and a maximum particle size of no more than 23.41 μm. The powder was then mixed evenly using a three-dimensional mixer. The mixed fine powder was oriented and formed in a 2T magnetic field, and the compact density was 4.2 g / cm 3 , and then isostatically pressed at 230 MPa for 30 min to obtain a density of 5.0 g / cm 3 of the green body.
[0078] The green body was placed in a sintering furnace, evacuated to below 0.01Pa, heated to 450℃ at a heating rate of 2℃ / min and kept at this temperature for 2h, then heated to 950℃ at a heating rate of 3℃ / min and kept at this temperature for 2h, and then heated to 1150℃ at a heating rate of 3.33℃ / min and kept at this temperature for 1h for pre-sintering; then filled with argon, heated to 1200℃ at a heating rate of 0.83℃ / min and kept at this temperature for 3h for sintering. After sintering, the temperature was cooled to 1180℃ at a cooling rate of 1℃ / min and kept at this temperature for 4h for solid solution treatment. After the solid solution treatment, it was quickly cooled to room temperature at a cooling rate of 65℃ / min to obtain a sintered blank.
[0079] Afterwards, the sintered blank was placed in a vacuum environment less than 0.1 Pa, heated to 650°C at a heating rate of 10°C / min and kept for 1 hour, then heated to 810°C at a heating rate of 2°C / min and kept for 10 hours for primary aging, then slowly cooled to 400°C at a cooling rate of 0.7°C / min and kept for 4 hours for secondary aging, and finally cooled to room temperature and taken out of the furnace to obtain a samarium cobalt permanent magnet.
[0080] The metallographic characterization of the prepared samarium cobalt permanent magnet is shown in the following figure: Figure 2 As shown, the average grain size of the magnet is 62.8μm, the maximum size is 136μm, the oxygen content of the magnet is 4316ppm, and the oxide (white substance in the metallographic image) is dispersed relatively evenly in the magnet.
[0081] Example 2
[0082] A total of 40 kg of raw metals were prepared according to the mass percentage of 24.8% Sm, 19.3% Fe, 5% Cu, 2.7% Zr, and the balance Co, and then induction smelting was performed to prepare a samarium-cobalt alloy ingot. The ingot was subjected to oxidation heat treatment: the ingot was heated to 550°C at 12 Pa for 3.5 hours, and then cooled to room temperature. The thickness of the ingot oxide layer was measured to be about 2.8 μm, and the overall oxygen content of the ingot was 2210 ppm.
[0083] The ingots were then mechanically crushed into coarse particles less than 1 mm, and then jet milled and ball milled to prepare powders with a specific surface average particle size (SMD) of 4.58 μm and 3.95 μm, respectively, and a maximum particle size of no more than 23.41 μm. The powders were then mixed evenly using a three-dimensional mixer. The mixed fine powders were oriented and formed in a 2T magnetic field, and the compact density was 4.0 g / cm 3 , and then isostatically pressed at 250 MPa for 30 min to obtain a density of 5.1 g / cm 3 of the green body.
[0084] The green body was placed in a sintering furnace, evacuated to below 0.01Pa, heated to 300℃ at a heating rate of 2℃ / min and kept at that temperature for 2h, then heated to 850℃ at a heating rate of 3.5℃ / min and kept at that temperature for 2h, then heated to 1000℃ at a heating rate of 2.5℃ / min and kept at that temperature for 1h, then heated to 1180℃ at a heating rate of 3℃ / min and kept at that temperature for 1h for pre-sintering; then filled with argon, heated to 1195℃ at a heating rate of 0.83℃ / min and kept at that temperature for 2.5h for sintering. After sintering, the temperature was cooled to 1175℃ at a cooling rate of 1℃ / min and kept at that temperature for 2h, then cooled to 1165℃ at a cooling rate of 0.7℃ / min and kept at that temperature for 4h, then cooled to 1160℃ at a cooling rate of 0.7℃ / min and kept at that temperature for 12h for solution treatment. After the solid solution is completed, it is quickly cooled to room temperature at a cooling rate of 80°C / min to obtain a sintered blank.
[0085] Afterwards, the sintered blank was placed in a vacuum environment of less than 0.1 Pa, heated to 600°C at a heating rate of 10°C / min and kept warm for 1 hour, then heated to 820°C at a heating rate of 2°C / min and kept warm for 15 hours for primary aging, then slowly cooled to 400°C at a cooling rate of 0.5°C / min and kept warm for 6 hours for secondary aging, and finally cooled to room temperature and taken out of the furnace to obtain a samarium cobalt permanent magnet.
[0086] Example 3
[0087] A total of 100 kg of raw metals were prepared according to the mass percentage of 24.8% Sm, 23% Fe, 5% Cu, 2.5% Zr, and the balance Co, and then induction smelting was performed to prepare a samarium-cobalt alloy ingot. The ingot was subjected to oxidation heat treatment: the ingot was heated to 750°C for 3.2 hours under a vacuum degree of 8 Pa, and then cooled to room temperature. The thickness of the ingot oxide layer was measured to be about 4.6 μm, and the overall oxygen content of the ingot was 3413 ppm.
[0088] The castings were then mechanically crushed into coarse particles of less than 2 mm, and then jet milled to prepare powders with a surface average particle size (SMD) of 4.14 μm and a maximum particle size of no more than 21.67 μm. The powders were then mixed evenly using a three-dimensional mixer. The mixed fine powders were oriented and formed in a 2T magnetic field, and the compact density was 3.8 g / cm 3 , and then isostatically pressed at 250 MPa for 45 min to obtain a density of 5.1 g / cm 3 of the green body.
[0089] The green body was placed in a sintering furnace, evacuated to below 0.01Pa, heated to 300℃ at a heating rate of 2℃ / min and kept at that temperature for 2h, then heated to 850℃ at a heating rate of 3.5℃ / min and kept at that temperature for 2h, then heated to 1000℃ at a heating rate of 2.5℃ / min and kept at that temperature for 1h, then heated to 1180℃ at a heating rate of 3℃ / min and kept at that temperature for 1h for pre-sintering; then filled with argon, heated to 1193℃ at a heating rate of 0.83℃ / min and kept at that temperature for 2.5h for sintering. After sintering, the temperature was cooled to 1160℃ at a cooling rate of 1℃ / min and kept at that temperature for 2h, then cooled to 1150℃ at a cooling rate of 1℃ / min and kept at that temperature for 8h, then cooled to 1140℃ at a cooling rate of 0.7℃ / min and kept at that temperature for 15h for solution treatment. After the solid solution is completed, it is quickly cooled to room temperature at a cooling rate of 80°C / min to obtain a sintered blank.
[0090] Afterwards, the sintered blank was placed in a vacuum environment less than 0.1 Pa, heated to 600°C at a heating rate of 10°C / min and kept for 1 hour, then heated to 810°C at a heating rate of 2°C / min and kept for 20 hours for primary aging, then slowly cooled to 400°C at a cooling rate of 0.3°C / min and kept for 10 hours for secondary aging, and finally cooled to room temperature and taken out of the furnace to obtain the final samarium cobalt magnet.
[0091] Example 4
[0092] A total of 40 kg of raw metals were prepared according to the mass percentage of 25% Sm, 21.5% Fe, 5% Cu, 3% Zr, and the balance Co, and then induction smelting was performed to prepare a samarium-cobalt alloy ingot. The ingot was subjected to oxidation heat treatment: the ingot was heated to 800°C at 2Pa for 1.5 hours, and then cooled to room temperature. The thickness of the ingot oxide layer was measured to be about 2.5 μm, and the overall oxygen content of the ingot was 1897 ppm.
[0093] The ingots were then mechanically crushed into coarse particles less than 1 mm, and then jet milled and ball milled to prepare powders with a specific surface average particle size (SMD) of 4.5 μm and 4.0 μm, respectively, and a maximum particle size of no more than 23.66 μm. The powders were then mixed evenly using a three-dimensional mixer. The mixed fine powders were oriented and formed in a 2.3 T magnetic field, and the compact density was 4.15 g / cm 3 , and then isostatically pressed at 250 MPa for 30 min to obtain a density of 5.1 g / cm 3 of the green body.
[0094] The green body was placed in a sintering furnace, evacuated to below 0.01Pa, heated to 300℃ at a heating rate of 2℃ / min and kept at that temperature for 2h, then heated to 850℃ at a heating rate of 3.5℃ / min and kept at that temperature for 2h, then heated to 1000℃ at a heating rate of 2.5℃ / min and kept at that temperature for 1h, then heated to 1180℃ at a heating rate of 3℃ / min and kept at that temperature for 1h for pre-sintering; then filled with argon, heated to 1195℃ at a heating rate of 0.83℃ / min and kept at that temperature for 2.5h for sintering. After sintering, the temperature was cooled to 1175℃ at a cooling rate of 1℃ / min and kept at that temperature for 2h, then cooled to 1165℃ at a cooling rate of 0.7℃ / min and kept at that temperature for 4h, then cooled to 1160℃ at a cooling rate of 0.7℃ / min and kept at that temperature for 12h for solution treatment. After the solid solution is completed, it is quickly cooled to room temperature at a cooling rate of 80°C / min to obtain a sintered blank.
[0095] Afterwards, the sintered blank was placed in a vacuum environment of less than 0.1 Pa, heated to 600°C at a heating rate of 10°C / min and kept warm for 1 hour, then heated to 820°C at a heating rate of 2°C / min and kept warm for 15 hours for primary aging, then slowly cooled to 400°C at a cooling rate of 0.5°C / min and kept warm for 6 hours for secondary aging, and finally cooled to room temperature and taken out of the furnace to obtain a samarium cobalt permanent magnet.
[0096] Comparative Example 1
[0097] The difference between Comparative Example 1 and Example 1 is that the ingot is not subjected to oxidation heat treatment, and the oxygen content of the ingot as a whole is 427ppm, the oxygen content of the magnet is 2568ppm, and the metallographic structure of the magnet is as follows: Figure 3As shown, the average grain size is 85.3 μm, the maximum grain size is 194 μm, and the oxide distribution is significantly lower than that of the magnet in Example 1. The magnetic properties are remanence Br = 11.21 kGs, intrinsic coercivity Hcj = 28.78 kOe, and maximum magnetic energy product (BH) max = 31.05 MGOe. It can be seen that the magnetic properties are similar to those of the magnet in Example 1, but the bending strength is only 117 MPa.
[0098] Comparative Example 2
[0099] The difference between Comparative Example 2 and Example 2 is that the ingot is subjected to oxidative heat treatment: the ingot is heated to 100°C at 12 Pa for 1.5 hours and then cooled to room temperature. The overall oxygen content of the ingot is measured to be 1098 ppm, and the oxygen content of the magnet is 2688 ppm.
[0100] Comparative Example 3
[0101] The difference between Comparative Example 3 and Example 1 is that the ingot is subjected to oxidation heat treatment: the ingot is heated to 1000°C for 2 hours under a vacuum degree of 30 Pa, and then cooled to room temperature. The cross section of the ingot is characterized by scanning electron microscopy (SEM). The results are as follows: Figure 4 As shown, it can be found that the thickness of the ingot oxide layer is about 5.8μm. It is further measured that the overall oxygen content of the ingot is 5238ppm, and the oxygen content of the magnet is 9897ppm.
[0102] Comparative Example 4
[0103] The difference between Comparative Example 4 and Comparative Example 1 is that an appropriate amount of the powder of Comparative Example 1 is taken, 3 wt% of samarium oxide is added, and the mixture is uniformly mixed, pressed, sintered, solid-solutionized and tempered to obtain a magnet. The oxygen content of the magnet is 2787 ppm, which is close to that of Comparative Example 1. The magnet is characterized by metallographic structure. The results are as follows: Figure 5 As shown, samarium oxide (white substance in the figure) is agglomerated and fine grains are concentrated locally.
[0104] The preparation parameters of Examples 1-4 and Comparative Examples 1-4 are shown in Table 1.
[0105] Table 1
[0106]
[0107] The magnetic properties of the magnets prepared in Examples 1-4 and Comparative Examples 1-4 were measured, and the flexural strength was measured in accordance with the standard "Test Methods for Physical Properties of Rare Earth Permanent Magnet Materials Part 2: Determination of Flexural Strength and Fracture Toughness" (GB / T31967.2-2015). The results are shown in Table 2.
[0108] Table 2
[0109]
[0110]
[0111] According to Examples 1-4 in Table 2, under different raw material ratios, the samarium cobalt permanent magnets prepared by the preparation method of the present invention can have both high hard magnetic properties and high bending strength. The samarium cobalt permanent magnet prepared in Comparative Example 1 has a remanence of 11.21 kGs, an intrinsic coercive force of 28.78 kOe, and a maximum magnetic energy product of 31.05 MGOe. Under the same raw material ratio, although the magnetic properties are similar to those of Example 1, the bending strength is only 117 MPa. The samarium cobalt permanent magnet prepared in Comparative Example 2 has a remanence of 11.61 kGs, an intrinsic coercive force of 26.13 kOe, and a maximum magnetic energy product of 32.01 MGOe. Under the same raw material ratio, although the magnetic properties are similar to those of Example 2, the bending strength is only 122 MPa. Due to the excessively high oxygen content in Comparative Example 3, the hard magnetic properties of the magnet are significantly reduced. In Comparative Example 4, since samarium oxide is a non-magnetic material, its aggregation not only leads to reduced consistency and stability of the magnetic properties of the magnet, but also local stress concentration affects the mechanical properties, resulting in a 11 MPa reduction in flexural strength compared with Example 1 under the same raw material ratio.
[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0113] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a samarium cobalt permanent magnet, characterized in that: The preparation method comprises the following steps: Provide samarium cobalt alloy; The samarium-cobalt alloy is subjected to an oxidation heat treatment, wherein the oxidation heat treatment process satisfies the following relationship: t=kP / T, wherein t is the holding time, in units of h; T is the heating temperature, in units of °C; P is the vacuum degree, in units of Pa; k is a coefficient, k=100-5000; Crushing and pulverizing the samarium-cobalt alloy after the oxidation heat treatment to obtain alloy powder; The alloy powder is oriented and molded to obtain a samarium-cobalt green body, and then a samarium-cobalt permanent magnet is obtained through a sintering treatment.
2. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: The heating temperature T is 300°C-1200°C; And / or, the vacuum degree P is 0.1Pa-20Pa.
3. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: When P≥10Pa, 100≤k≤300, 300℃≤T<600℃; Or, when 5Pa≤P<10Pa, 200 <k≤500,500℃<T<800℃; Or, when 1Pa≤P<5Pa, 400 <k≤800,700℃<T<1000℃; Or, when 0.1Pa≤P<1Pa, 800 <k≤3000,900℃<T≤1200℃。 4. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: The components of the samarium-cobalt alloy include: 23%-28% of Sm, 13%-25% of Fe, 4%-10% of Cu, 1.5%-3.5% of Zr and the balance of Co.
5. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: The thickness of the oxide layer on the surface of the samarium-cobalt alloy after oxidation heat treatment is 1 μm-5 μm; And / or, the oxygen content of the samarium-cobalt alloy after the oxidation heat treatment is 1500ppm-4000ppm.
6. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: The particle size of the coarse particles obtained by crushing is less than 5 mm; And / or, the average particle size of the alloy powder is 3 μm-8 μm, and the maximum particle size is less than or equal to 35 μm.
7. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: In the step of orientation molding, the magnetic field strength is greater than or equal to 2T; And / or, the density of the samarium cobalt green body is 4.5 g / cm 3 -5.5g / cm 3 .
8. The method for preparing a samarium cobalt permanent magnet according to claim 1, characterized in that: The sintering treatment includes sintering and solid solution treatment, and the sintering and solid solution treatment process includes: under the condition of vacuum degree less than or equal to 0.05Pa, heating to 1130℃-1180℃ at a heating rate of 0.5℃ / min-10℃ / min and keeping warm for 0.5h-5h for pre-sintering, then heating to 1170℃-1240℃ in an inert gas environment and keeping warm for 1h-8h for sintering, then cooling to 1110℃-1180℃ at a cooling rate of 0.2℃ / min-5℃ / min and keeping warm for 2h-72h for solid solution treatment, and after the solid solution treatment, rapidly quenching to below 400℃ at a cooling rate of 40℃ / min-200℃ / min; And / or, the sintering treatment also includes tempering and aging, and the tempering and aging process includes: in an inert gas environment or under a vacuum degree of ≤0.1Pa, heating the temperature to 750℃-900℃ at a heating rate of 0.5℃ / min-10℃ / min and keeping it for 1h-50h, and then cooling the temperature to 300℃-500℃ at a cooling rate of 0.1℃ / min-1℃ / min and keeping it for 1h-30h.
9. A samarium cobalt permanent magnet, characterized in that: The samarium cobalt permanent magnet is prepared by the preparation method according to any one of claims 1 to 8, and the oxygen content of the samarium cobalt permanent magnet is 3500ppm-6000ppm.
10. The samarium cobalt permanent magnet according to claim 9, characterized in that: The average grain size of the samarium cobalt permanent magnet is 30 μm-80 μm; And / or, the maximum grain size of the samarium cobalt permanent magnet is less than 170 μm.