Lithium ion battery positive plate and preparation method thereof, battery and electric equipment

By adding phosphate coating and sintering treatment to the positive electrode material of lithium ion battery, the cycle capacity attenuation and structural stability of nickel-cobalt-manganese oxide materials under high voltage conditions is solved, and higher cycle life and heat are achieved stability.

CN119069635APending Publication Date: 2024-12-03DONGGUAN YIHUA NEW ENERGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310623603.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The problems of fast cycling capacity decay, agglomerated particles powdering and poor structural stability of the nickel-cobalt lithium manganate positive electrode material under high voltage conditions limit their application under high voltage conditions.

Method used

A lithium-ion battery positive electrode sheet is adopted, including a positive electrode current collector and a coating, which contains a positive electrode active material, conductive agent and adhesive, and is coated with phosphate on the coating, and improves the material by sintering and grinding. structural stability and cyclic performance.

Benefits of technology

The crystal plane spacing is increased, a firmer chemical bond is formed, which improves the cycle life and structural stability, inhibits the corrosion of the electrolyte on the material, and improves the circulation performance and thermal stability of the nickel-cobalt-manganate lithium positive electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069635A_ABST
    Figure CN119069635A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery positive plate and a preparation method thereof, a battery and electric equipment, and solves the problems of rapid cycle capacity attenuation, agglomeration particle pulverization, poor structural stability and the like of a conventional nickel cobalt lithium manganate positive electrode material under high voltage, and the preparation method comprises the following steps: S1, mixing a metal precursor and a lithium source to obtain a preposed mixture, wherein the transition metal oxide in the metal precursor is nickel oxide; s2, sintering the pre-mixture in a reactor, carrying out heat preservation, and naturally cooling to obtain a first positive electrode active material; s3, the first positive electrode active material and phosphoric acid are mixed through jet milling, and a mixed raw material is obtained; s4, sintering the mixed raw material in a reactor, preserving heat, and naturally cooling to obtain a second positive electrode active material coated with nickel phosphate on the surface; and S5, mixing a second positive electrode active material, an adhesive and a conductive agent to obtain positive electrode slurry, and coating a positive electrode current collector with the positive electrode slurry to obtain the positive plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite batteries, and in particular to a lithium ion battery positive electrode sheet and a preparation method thereof, a battery and an electrical device. Background Art

[0002] Lithium-ion batteries usually use reversibly deintercalable materials such as lithium iron phosphate and ternary positive electrode materials as positive electrodes to achieve reversible charge and discharge of lithium-ion batteries. The existing positive electrode material system has a limited specific capacity and is difficult to significantly improve. Lithium batteries usually use lithium titanate as the negative electrode, and the positive electrode uses materials with high voltage and high specific capacity, such as graphite fluoride, transition metal oxides, sulfides, etc. Although lithium batteries assembled with these materials have very high energy density, these materials usually do not have reversible charge and discharge capabilities, so they are usually used as disposable batteries.

[0003] Lithium-ion batteries have been widely used in mobile phones, laptops, electric vehicles, hybrid electric vehicles and other fields due to their high operating voltage, high energy density and long cycle life. The proportion of nickel in ternary materials determines the energy density of the material; cobalt can stabilize the material structure, enhance the material's cycle performance and rate performance; manganese can improve the material's thermal stability, enhance structural stability and reduce costs. As a rare metal, cobalt is also widely used in cemented carbide, catalytic materials, radiochemistry, national defense, military and aerospace fields due to its excellent physical and chemical properties.

[0004] In the prior art, doping or coating methods are usually used to improve the problems of low initial efficiency, poor rate performance and cycle performance of lithium-rich materials. At present, for example, a Chinese invention patent with publication number CN115799487A discloses a boron-phosphorus co-doped modified lithium-rich manganese-based positive electrode material. The general formula of the lithium-rich manganese-based positive electrode material is Li 1+a (Mn b Me 1-b )B x P y O 2+z , wherein: Me is nickel element and / or cobalt element; 0≤a≤1, 0<b<1, 0<x≤0.05, 0<y≤0.05, 0≤z≤1. The present invention also provides a method for preparing the material, which effectively improves the discharge specific capacity, first coulomb efficiency, and rate of the lithium-rich manganese-based positive electrode material through the synergistic co-doping effect of boron and phosphorus elements, while also greatly improving the cycle stability. The preparation method of the present invention is in-situ doping, with uniform distribution of doping elements and good doping effect, and the method is simple in process and low in cost, which effectively simplifies the industrial preparation process, improves efficiency and reduces the cost of industrial preparation, and is convenient for scale-up, promotion and application. The present invention also provides the application of the lithium-rich manganese-based positive electrode material.

[0005] Although the above scheme proposes a method for preparing a lithium-rich manganese-based positive electrode material modified by boron-phosphorus co-doping, during the contact between the electrolyte and the surface of the nickel-cobalt-manganese-oxide positive electrode material, the nickel-cobalt-manganese-oxide positive electrode material faces problems such as fast cycle capacity decay, agglomerated particle pulverization, and poor structural stability under high voltage conditions, which significantly limits its application under high voltage conditions. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the defects of the prior art. The present invention proposes a lithium ion battery positive electrode sheet and a preparation method thereof, a battery and an electrical device that can improve the structural stability, cycle performance and thermal stability of nickel cobalt manganese oxide lithium positive electrode materials.

[0007] In order to solve the above technical problems, the technical solution provided by the present invention is: A positive electrode sheet for a lithium-ion battery comprises a positive electrode current collector and a coating disposed on at least one side of the positive electrode current collector, wherein the coating comprises a positive electrode active material, a conductive agent and an adhesive, wherein an additive is further disposed in the positive electrode active material, wherein the additive is one or a combination of graphite fluoride, transition metal oxide and sulfide, wherein the additive has a chemical formula of LixMyO2 oxide, wherein M is selected from at least one of Group VII transition metals and Group VIII transition metals, 0.9≤y≤1.1, x≤y, and the coating is further covered with a phosphate, wherein the phosphate is preferably selected from any one or more of magnesium phosphate, zinc phosphate and calcium phosphate.

[0008] Furthermore, it is preferred that the positive electrode active material, the additive, the conductive agent and the binder have a content ratio of 90:3.5:4:2.5.

[0009] Furthermore, it is preferred that the positive electrode active material is selected from any one or more of lithium cobalt oxide, lithium manganese oxide, ternary materials, and lithium iron phosphate. It is preferred that the additive is selected from any one or more of manganese oxide, cobalt oxide, and nickel oxide when it is a transition metal oxide. It is preferred that the additive is selected from any one or more of manganese sulfide, cobalt sulfide, and nickel sulfide when it is a sulfide. It is preferred that the conductive agent is selected from any one or more of super P, acetylene black, and carbon black, and the binder is PVDF.

[0010] A method for preparing a lithium-ion battery positive electrode sheet comprises the following steps: S1, mixing a metal precursor and a lithium source to obtain a premixture, wherein the transition metal oxide in the metal precursor is nickel oxide; S2, placing the premixture in a reactor for sintering and heat preservation, and obtaining a first positive electrode active material after natural cooling; S3, grinding and mixing the first positive electrode active material and phosphoric acid by air flow to obtain a mixed raw material; S4, placing the mixed raw materials in a reactor for sintering and heat preservation, and obtaining a second positive electrode active material with a surface covered with nickel phosphate after natural cooling.

[0011] Furthermore, the sintering process in step S2 satisfies: The heating rate of the sintering is 0.5°C / min~8°C / min; The sintering temperature is 300°C to 800°C; The holding temperature is lower than the sintering temperature and the holding time is not less than 4 hours; The sintering time is 2h~15h.

[0012] Furthermore, in step S4, the sintering temperature is 600° C.-800° C., and the calcination time is 10 h-12 h.

[0013] Furthermore, in the step S1, the phosphoric acid is solid phosphoric acid powder, and the first positive electrode material and the solid phosphoric acid powder are mixed in a mass ratio of 1:n, wherein 0.02≤n≤0.2.

[0014] Furthermore, in step S1, the phosphoric acid is a phosphoric acid solution, and the first positive electrode material and the phosphoric acid solution are mixed in a molar ratio of 1:m, wherein 0.01≤m≤0.2.

[0015] A lithium ion battery comprises a positive electrode sheet and a negative electrode sheet, wherein both the positive electrode sheet and the negative electrode sheet are provided with a current collector and a coating is provided on the surface of the current collector, wherein the coating corresponding to the negative electrode sheet is lithium titanate, and the positive electrode sheet is the lithium ion battery positive electrode sheet described above or is made by the preparation method of the lithium ion battery positive electrode sheet described above.

[0016] An electrical device includes: the lithium-ion battery as described above.

[0017] Compared with the prior art, the beneficial effects of the present invention include: The positive electrode sheet made of the positive electrode material of the present invention can increase the inter-crystalline spacing to promote the migration of lithium ions, and the chemical bonds formed by the metal ions in the nickel cobalt manganese oxide positive electrode material are more solid, thereby improving its compaction density and cycle life, and can improve the structural stability and safety of the nickel cobalt manganese oxide positive electrode material. The coating layer including phosphate avoids the contact between the electrolyte and the surface of the nickel cobalt manganese oxide positive electrode material, inhibits the surface side reaction, and can inhibit the corrosion of the electrolyte to it, thereby further improving the structural stability, cycle performance and thermal stability of the nickel cobalt manganese oxide positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 The present invention is a flow chart of a method for preparing a positive electrode sheet for a lithium-ion battery according to an embodiment of the present invention. DETAILED DESCRIPTION

[0019] The preferred examples of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred examples described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0020] like Figure 1 As shown in the figure, the mainstream positive electrode materials for lithium-ion batteries are lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and nickel cobalt manganese oxide. Due to the coordination effect of nickel, cobalt and manganese, the nickel cobalt manganese oxide positive electrode material has advantages in comprehensive performance such as energy density, cycle performance, safety performance and cost, and is one of the most popular positive electrode materials. However, the nickel cobalt manganese oxide positive electrode material faces problems such as fast cycle capacity decay, agglomerated particle pulverization and poor structural stability under high voltage conditions, which limits its application under high voltage conditions.

[0021] Regarding the working principle of lithium-ion batteries, current lithium-ion batteries mostly use transition metal oxide particles as positive electrode materials. However, due to the insufficient strength of transition metal oxide particles, during the cyclic charge and discharge process, the shape and structure of transition metal oxide particles are easily destroyed due to the frequent extraction and embedding of lithium ions, which causes the transition metal to easily dissolve from the positive electrode material into the electrolyte, which will affect the cycle stability and rate performance of the lithium-ion battery.

[0022] To this end, we propose a lithium-ion battery positive electrode that can overcome the defect of insufficient strength of transition metal oxide particles and help improve the cycle stability and rate performance of lithium-ion batteries. The following is a specific solution: A lithium-ion battery positive electrode sheet comprises a positive electrode current collector and a coating disposed on at least one side of the positive electrode current collector, wherein the coating comprises a positive electrode active material, an additive, a conductive agent and an adhesive, wherein the additive is one or a combination of graphite fluoride, transition metal oxides and sulfides, and the coating is also covered with nickel phosphate.

[0023] Furthermore, the additive has a chemical formula of LixMyO2 oxide, wherein M is selected from at least one of Group VII transition metals and Group VIII transition metals, and 0.9≤y≤1.1, x≤y.

[0024] In some embodiments, the transition metal precursor is selected from transition metal oxides or transition metal hydroxides. Optionally, the transition metal oxide is selected from at least one of Group VII transition metal oxides and Group VIII transition metal oxides.

[0025] Furthermore, it is preferred that the positive electrode active material, the additive, the conductive agent and the binder have a content ratio of 90:3.5:4:2.5.

[0026] Furthermore, it is preferred that the positive electrode active material is selected from any one or more of lithium cobalt oxide, lithium manganese oxide, ternary materials, and lithium iron phosphate. It is preferred that the additive is selected from any one or more of manganese oxide, cobalt oxide, and nickel oxide when it is a transition metal oxide. It is preferred that the additive is selected from any one or more of manganese sulfide, cobalt sulfide, and nickel sulfide when it is a sulfide.

[0027] Furthermore, it is preferred that the conductive agent is selected from any one or more of super P, acetylene black, and carbon black, and the adhesive is PVDF.

[0028] Similarly, the preparation method of the positive electrode sheet corresponding to the above ratio mainly includes the following steps: S1, mixing a metal precursor and a lithium source to obtain a premixture, wherein the transition metal oxide in the metal precursor is nickel oxide; S2, placing the premixture in a reactor for sintering and heat preservation, and obtaining a first positive electrode active material after natural cooling; S3, grinding and mixing the first positive electrode active material and phosphoric acid by air flow to obtain a mixed raw material; S4, placing the mixed raw materials in a reactor for sintering and heat preservation, and obtaining a second positive electrode active material with a surface covered with nickel phosphate after natural cooling.

[0029] Furthermore, the sintering process in step S2 satisfies: the sintering heating rate is 0.5°C / min to 8°C / min; The sintering temperature is 300°C to 800°C; the insulation temperature is lower than the sintering temperature and the insulation time is not less than 4h; The sintering time is 2h~15h.

[0030] Furthermore, in step S4, the sintering temperature is 600° C.-800° C., and the calcination time is 10 h-12 h.

[0031] Furthermore, in the step S1, the phosphoric acid is solid phosphoric acid powder, and the first positive electrode material and the solid phosphoric acid powder are mixed in a mass ratio of 1:n, wherein 0.02≤n≤0.2.

[0032] Furthermore, in step S1, the phosphoric acid is a phosphoric acid solution, and the first positive electrode material and the phosphoric acid solution are mixed in a molar ratio of 1:m, wherein 0.01≤m≤0.2.

[0033] The above ratio and operation steps are described in detail below in conjunction with the embodiments: Example 1

[0034] In this embodiment, the transition metal oxide is nickel oxide, that is, the corresponding additive chemical formula is LiNiO2, and the preparation steps of the corresponding battery positive electrode material are as follows: Step 1: Weigh iron oxide (Fe2O3) and nickel oxide (NiO) at a molar ratio of 0.5:1 and place them in a ball mill, and ball mill them at a speed of 300 r / min for more than 3 hours to mix and obtain the corresponding transition metal oxides; Step 2: Mix the transition metal oxide and the lithium source in a molar ratio of 4:3 to obtain a premixture. Step 3: sintering the premixture in a reactor at a heating rate of 3°C / min, while the reactor is in an oxygen atmosphere, heating to 750°C, maintaining the temperature for no less than 4 hours, and finally cooling naturally to room temperature to obtain a first positive electrode active material; Step 4: 100 g of the first positive electrode active material and 5 g of solid phosphoric acid powder are mixed evenly and dried, and after drying, the mixture is ball-milled at a speed of 300 r / min for more than 3 hours to obtain a mixed raw material; Step 5: The mixed raw materials are heated and sintered in a reactor at a heating rate of 3°C / min. After the temperature is raised to 600°C, the mixture is naturally cooled to obtain a lithium nickel oxide positive electrode material with a phosphate-coated surface. Example 2

[0035] The difference from Example 1 is that, for step 4, in Example 1, phosphoric acid is solid phosphoric acid powder, and the first positive electrode material and the solid phosphoric acid powder are mixed in a mass ratio of 1:n, wherein 0.02≤n≤0.2, while in this embodiment, phosphoric acid is a phosphoric acid solution, and the first positive electrode material and the phosphoric acid solution are mixed in a molar ratio of 1:m, wherein 0.01≤m≤0.2, and the corresponding steps are, Step 4: Mix the diammonium hydrogen phosphate aqueous solution and the first positive electrode active material in a mass ratio of 0.01:1, dry at 150° C. after mixing evenly, ball-mill the dried material again at a speed of 300 r / min for 3 hours to obtain the corresponding mixed raw material, wherein the mass fraction of diammonium hydrogen phosphate in the diammonium hydrogen phosphate aqueous solution is 30wt%.

[0036] Step 5: Raise the temperature to 800° C. in a muffle furnace at a heating rate of 5° C. / min, calcine for more than 10 hours in an oxygen atmosphere, and obtain the desired lithium nickel oxide positive electrode material after natural cooling.

[0037] In Example 1 and Example 2, the present application forms nickel phosphate with a more stable crystal structure on the basis of the first positive electrode material, which can reduce the retention space of oxygen free radicals in the positive electrode material, and can avoid the irreversible transformation of the corresponding compounds in the positive electrode active material to the rock salt phase, thereby improving the cycle performance of the nickel-based positive electrode material; at the same time, after the original nickel oxide and lithium oxide in the positive electrode material are converted into nickel phosphate, it can not only effectively improve the structural stability of the positive electrode material, but also improve the purity of the positive electrode material, and further improve the charge and discharge performance of the material.

[0038] The embodiment of the present application adjusts the aspect ratio L / H of the primary particles of the positive electrode material to a range of 1.3 to 11.1. The primary particles with this aspect ratio have smaller stress and higher particle strength. During the cyclic charge and discharge process, as lithium ions repeatedly escape and embed in the primary particles, the primary particles can still maintain a complete structure, and basically will not cause the transition metal inside the primary particles to escape from the primary particles and dissolve into the electrolyte, thereby improving the cycle stability and rate performance of the battery. Example 3

[0039] In this embodiment, the transition metal oxide is a mixture of cobalt oxide and manganese oxide, and the steps for making the corresponding positive electrode material are as follows: Step 1: weigh MnSO4, NiSO4, and CoSO4 according to a molar ratio of 0.44:0.4:0.16 and dissolve them in deionized water to prepare a metal salt solution; dissolve NaOH and ammonia water in deionized water to prepare a corresponding alkaline solution, wherein the molar ratio of NaOH to NH3 is 1: 0.04; control the concentration ratio of the metal salt solution to the alkaline solution to be 1:2; Step 2: Add water as the base liquid to the reactor, i.e., the solution reactor, and stir and mix at a certain temperature and rate. At the same time, use a peristaltic pump to add the metal salt solution and the alkaline solution to the reactor, mix for more than 24 hours, control the pH of the mixed solution to be greater than 11, and then cool for 10 hours, wash the obtained precipitate with deionized water, and then filter and dry to prepare the nickel-cobalt-manganese hydroxide precursor; Step 3: Mix the nickel cobalt manganese hydroxide precursor with a lithium source, wherein the lithium source can be lithium carbonate, and the molar ratio of the two is 1:0.6. After mixing, place it in a muffle furnace and pre-sinter it to 800°C. The sintering time is not less than 10 hours. After natural cooling, the corresponding lithium-rich manganese cobalt first positive electrode material can be obtained.

[0040] Step 4: Grind and mix the first cathode active material obtained above with phosphoric acid by air flow, take solid phosphoric acid powder, and mix the first cathode material and the solid phosphoric acid powder in a mass ratio of 1:n, wherein 0.02≤n≤0.2, to obtain a mixed raw material; Step 5: The mixed raw materials are heated to 600° C. in a reactor at a heating rate of 5° C. / min, and the calcination time is 10 h. After natural cooling, a second positive electrode active material with manganese phosphate and cobalt phosphate coated on the surface is obtained. Example 4

[0041] The difference from Example 3 is that phosphoric acid is selected as a phosphoric acid solution, and the first positive electrode material and the phosphoric acid solution are mixed in a molar ratio of 1:m, wherein 0.01≤m≤0.2, and the corresponding steps are: Step 4: Mix the diammonium hydrogen phosphate aqueous solution and the first positive electrode active material in a mass ratio of 0.01:1, dry at 150° C. after mixing evenly, ball-mill the dried material again at a speed of 300 r / min for 3 hours to obtain the corresponding mixed raw material, wherein the mass fraction of diammonium hydrogen phosphate in the diammonium hydrogen phosphate aqueous solution is 30wt%.

[0042] Step 5: heating the mixture to 800° C. in a muffle furnace at a heating rate of 5° C. / min, calcining the mixture for more than 10 hours in an oxygen atmosphere, and naturally cooling the mixture to obtain the desired second positive electrode active material.

[0043] For Example 3 and Example 4, the second positive electrode material produced therefrom has phosphorus coated on the surface which effectively improves the migration and diffusion of lithium ions, so that the discharge specific capacity, first coulomb efficiency and rate performance of the material are greatly improved, and the cycle performance is also significantly improved.

[0044] By adding metal salt solution and alkali solution in situ during the precursor co-precipitation preparation process, the doping elements are evenly distributed and the doping effect is good. The overall process is simple and low-cost, which effectively simplifies the industrial preparation process, improves efficiency and reduces the cost of industrial preparation, making it easier to scale up and apply.

[0045] Comparative Example 1 In this embodiment, the preparation method of the positive electrode material is to dope nickel phosphate in Li2NiO2. The difference between the preparation method and Example 1 is that in step 4, 5g of solid phosphoric acid powder is replaced by 0.5g of solid phosphoric acid powder, and the mixture is fully ground and mixed.

[0046] The materials prepared in the above Examples 1-4 and Comparative Example 1 were used as positive electrode materials, and lithium carbonate was used as negative electrode material to assemble R2032 button half-cells. Constant current charge and discharge tests were carried out at 25° C. The initial charge and discharge capacity, initial efficiency and rate performance were tested in the voltage range of 2.0-4.8 V and at rates of 0.1C, 0.2C, 0.5C, 1C, and 3C (1C=200mAg -1 ); the battery was activated for three weeks at 2.0-4.8 V and a current density of 0.1C, and the cycle performance was tested at a voltage range of 2.0-4.6 V and a rate of 1C.

[0047] Serial number Charge capacity (mAg / g) Discharge capacity (mAg / g) Coulomb efficiency (%) Example 1 335 121 36.1 Example 2 334 118 35.3 Example 3 331 116 35 Example 4 334 120 35.9 Comparative Example 1 310 108 34.8 Table 1 Table 1 shows the first charge and discharge, rate performance and cycle performance test data of the materials prepared in Examples 1-4 and Comparative Example 1. It is obvious that in Comparative Example 1, due to the insufficient amount of solid phosphoric acid powder, the electrochemical performance of the battery is obviously insufficient, while in the first four embodiments, the charging capacity and the discharging capacity are correspondingly improved, and the electrochemical performance is better.

[0048] Similarly, for the subsequent production of positive electrode sheets, with reference to the preceding steps of the above four embodiments, the preparation method of the positive electrode sheets includes: mixing the above positive electrode materials with the conductive agent, the binder and the solvent to obtain positive electrode slurry, and then making the positive electrode sheets through the processes of screening, coating, rolling, striping and cutting. The compacted density of the positive electrode sheets is 2.8-3.4 g / cm 3 , which is 2.8~3.4g / cc Specifically, the type of conductive agent is not limited, and any known conductive agent can be used. Examples of conductive agents may include, but are not limited to, one or more of the following: natural graphite, artificial graphite, Super P conductive carbon black, acetylene black, needle coke, carbon nanotubes, graphene and other carbon materials. The above conductive agents can be used alone or in any combination.

[0049] Examples of the binder may include, but are not limited to, one or more of the following: polyethylene, polypropylene, polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, etc. The above binders may be used alone or in any combination.

[0050] The preparation method of the battery comprises: assembling the above-mentioned positive electrode sheet, negative electrode sheet, separator and electrolyte into a battery. The negative electrode material used in the negative electrode sheet can be one or more of artificial graphite, natural graphite, mesophase carbon microspheres, amorphous carbon, lithium titanate or silicon-carbon alloy.

[0051] Some embodiments of the present application also provide an electrical device, which includes the battery of any of the above embodiments. The electrical device includes but is not limited to: backup power supplies, motors, electric vehicles, electric motorcycles, power-assisted bicycles, bicycles, electric tools, large household batteries, etc.

[0052] The positive electrode sheet made of the positive electrode material of the present invention can increase the inter-crystalline spacing to promote the migration of lithium ions, and the chemical bonds formed by the metal ions in the nickel cobalt manganese oxide positive electrode material are more solid, thereby improving its compaction density and cycle life, and can improve the structural stability and safety of the nickel cobalt manganese oxide positive electrode material. The coating layer including phosphate avoids the contact between the electrolyte and the surface of the nickel cobalt manganese oxide positive electrode material, inhibits the surface side reaction, and can inhibit the corrosion of the electrolyte to it, thereby further improving the structural stability, cycle performance and thermal stability of the nickel cobalt manganese oxide positive electrode material.

[0053] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A positive electrode sheet for a lithium-ion battery, Features: It includes a positive electrode current collector and a coating arranged on at least one side of the positive electrode current collector, wherein the coating includes a positive electrode active material, a conductive agent and a binder, and the positive electrode active material is also provided with an additive, wherein the additive is one or a combination of graphite fluoride, transition metal oxide, and sulfide, and the additive has a chemical formula of LixMyO2 oxide, wherein M is selected from at least one of Group VII transition metals and Group VIII transition metals, 0.9≤y≤1.1, x≤y, and the coating is further covered with a phosphate, and preferably the phosphate is selected from any one or more of magnesium phosphate, zinc phosphate, and calcium phosphate.

2. A lithium-ion battery positive electrode sheet according to claim 1, Features: Preferably, the positive electrode active material, the additive, the conductive agent and the binder have a content ratio of 90:3.5:4:2.

5.

3. A lithium-ion battery positive electrode sheet according to claim 1, Features: Preferably, the positive electrode active material is selected from any one or more of lithium cobalt oxide, lithium manganese oxide, ternary materials, and lithium iron phosphate. Preferably, the additive is selected from any one or more of manganese oxide, cobalt oxide, and nickel oxide when it is a transition metal oxide. Preferably, the additive is selected from any one or more of manganese sulfide, cobalt sulfide, and nickel sulfide when it is a sulfide. Preferably, the conductive agent is selected from super P and acetylene.

4. A method for preparing a positive electrode sheet for a lithium-ion battery, It is characterized in that The steps include: S1, mixing a metal precursor and a lithium source to obtain a premixture, wherein the transition metal oxide in the metal precursor is nickel oxide; S2, placing the premixture in a reactor for sintering and heat preservation, and obtaining a first positive electrode active material after natural cooling; S3, grinding and mixing the first positive electrode active material and phosphoric acid by air flow to obtain a mixed raw material; S4, placing the mixed raw materials in a reactor for sintering and heat preservation, and obtaining a second positive electrode active material with a surface covered with nickel phosphate after natural cooling; S5. Mix the second positive electrode active material, the binder and the conductive agent to obtain a positive electrode slurry, and apply the positive electrode slurry on the positive electrode collector to obtain a positive electrode sheet, wherein the conductive agent is selected from any one or more of super P, acetylene black and carbon black, and the binder is PVDF.

5. A method for preparing a lithium ion battery positive electrode sheet according to claim 4, Features: The sintering process in step S2 satisfies: The heating rate of the sintering is 0.5°C / min to 8°C / min; The sintering temperature is 300°C to 800°C; The holding temperature is lower than the sintering temperature and the holding time is not less than 4 hours; The sintering time is 2h to 15h.

6. A method for preparing a lithium ion battery positive electrode sheet according to claim 4, Features: In step S4, the sintering temperature is 600° C.-800° C., and the calcination time is 10 h-12 h.

7. A method for preparing a lithium ion battery positive electrode sheet according to claim 6, Features: In the step S1 , the phosphoric acid is solid phosphoric acid powder, and the first positive electrode material and the solid phosphoric acid powder are mixed in a mass ratio of 1:n, wherein 0.02≤n≤0.

2.

8. The method for preparing a lithium ion battery positive electrode sheet according to claim 6, Features: In the step S1 , the phosphoric acid is a phosphoric acid solution, and the first positive electrode material and the phosphoric acid solution are mixed in a molar ratio of 1:m, wherein 0.01≤m≤0.

2.

9. A lithium-ion battery, comprising a positive electrode sheet and a negative electrode sheet, wherein both the positive electrode sheet and the negative electrode sheet are provided with a current collector and a coating is provided on the surface of the current collector, wherein the coating corresponding to the negative electrode sheet is lithium titanate, Features: The positive electrode sheet is a lithium-ion battery positive electrode sheet as described in any one of claims 1-3 or is made by the preparation method of a lithium-ion battery positive electrode sheet as described in any one of claims 4-8.

10. An electrical device, It is characterized in that include: The lithium ion battery as claimed in claim 9.

Citation Information

Patent Citations

  • Boron-phosphorus co-doping modified lithium-rich manganese-based positive electrode material, preparation method and application

    CN115799487A