Positive electrode composite pole piece, preparation method thereof and solid-state battery
By transferring the step slurry to the positive electrode current collector and performing roll-compression processing, the problems of electrode sheet damage and short circuit caused by step stress concentration in solid-state batteries are solved, and the battery preparation efficiency is improved.
Patent Information
- Application Number
- CN202411385884.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
During the compaction process of solid-state batteries, the steps on the edges of the positive/negative electrode sheets lead to stress concentration, which easily leads to damage to the electrode sheet and short circuit problems. The existing filling washer methods are complex in operation and low in production efficiency.
The step slurry is applied to the release film for drying and die cutting, and then transferred to the positive electrode current collector. Through the rolling composite treatment, a continuous preparation process is established to reduce the presence of the step.
It effectively reduces the pole sheet damage and short circuit problems caused by step stress concentration during the compaction of the battery cell, and improves the preparation efficiency of solid-state batteries.
Smart Images

Figure CN119069650A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy batteries, and in particular to a positive electrode composite electrode sheet and a preparation method thereof, and a solid-state battery. Background Art
[0002] The preparation of all-solid-state batteries generally includes the preparation of positive / negative electrode sheets, electrolyte membrane preparation, lamination, packaging and compaction. In order to ensure battery performance, the negative electrode sheet is generally larger than the positive electrode sheet, which will cause steps at the edges of the positive / negative electrode sheets of the battery cell after lamination. In the subsequent compaction process, stress is concentrated at the steps, generating large shear forces, which will cause damage to the electrode sheets and short circuit problems. The current common solution is to fill gaskets at the steps, but this method is complicated to operate and has low production efficiency. Summary of the invention
[0003] In view of this, the present invention is committed to providing a positive electrode composite electrode sheet and a preparation method thereof and a solid-state battery, so as to solve the problem in the prior art that stress concentration at the step during the compaction process of the battery cell easily causes damage to the electrode sheet and short circuit.
[0004] In order to solve the above technical problems, this application is implemented as follows:
[0005] A first aspect of the present invention provides a method for preparing a positive electrode composite electrode sheet, the method comprising:
[0006] S1, performing a fiberization treatment and a first die-cutting treatment on the positive electrode slurry to obtain a positive electrode film;
[0007] S2, placing the step slurry on the surface of the release film and performing a drying process and a second die-cutting process to obtain a step material film having a step dressing layer on the surface and a blank position; wherein the blank position has the same shape and area as the positive electrode film;
[0008] S3, transferring the step dressing layer on the surface of the step material film to the surface of the first positive electrode current collector to obtain a second positive electrode current collector having a step dressing layer on the surface; wherein the step dressing layer has the blank position;
[0009] S4, placing the positive electrode film at the blank position of the second positive electrode current collector and performing a roll-combination process and a third die-cutting process.
[0010] Optionally, the step slurry includes step powder and a first binder; wherein the mass ratio of the step powder to the first binder is (80-99.9): (0.1-20).
[0011] Optionally, the step powder includes at least one of a first solid electrolyte, boehmite and nano-alumina; optionally, the first solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide electrolyte.
[0012] Optionally, the first binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylic acid, sodium carboxymethyl cellulose, polyimide, polyacrylonitrile, polypropylene, polyethylene and polystyrene.
[0013] Optionally, the difference between the thickness of the step dressing layer and the thickness of the positive electrode film is less than 1 μm; optionally, the thickness of the step dressing layer is 80-200 μm.
[0014] Optionally, the first positive electrode current collector is a carbon-coated current collector; the carbon-coated current collector comprises a metal foil and a carbon-coated layer disposed on the surface of the metal foil.
[0015] Optionally, in step S2, the drying treatment conditions include: a temperature of 60 to 120° C. and a time of 10 to 60 min.
[0016] Optionally, in step S4, the conditions of the roller-compression composite treatment include: a temperature of 20 to 120° C., a pressure of 0.2 to 2 t / cm, and a time of 10 to 60 min.
[0017] A second aspect of the present invention provides a positive electrode composite electrode sheet, which is prepared according to the above method.
[0018] A third aspect of the present invention provides a solid-state battery, comprising a positive electrode plate, wherein the positive electrode plate is a positive electrode composite plate prepared according to the above method and / or is the above positive electrode composite plate.
[0019] Through the above technical solution, the beneficial technical effects of the present invention are:
[0020] The preparation method of the positive composite electrode sheet of the present invention adopts the method of applying the step slurry to the release film, drying and second die-cutting, and then transferring it to the first positive current collector. The positive electrode sheet of the present invention is made into a film by a dry process, and after die-cutting, it is composited to the blank position of the step dressing layer on the first positive current collector. The preparation method of the present invention establishes a continuous preparation process for step filling to reduce the presence of steps at the edges of the positive / negative electrode sheets, thereby reducing the electrode sheet damage and short circuit problems caused by stress concentration at the steps during the compaction of the battery cell, thereby improving the preparation efficiency of solid-state batteries.
[0021] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 Shown is an implementation of the solid-state battery preparation process of the present invention.
[0024] Figure 2 Shown is a schematic diagram of a release film coated with a step slurry in one embodiment of the present invention.
[0025] Figure 3 Shown is a schematic diagram of a step material film having a step dressing layer and blank positions on the surface in one embodiment of the present invention.
[0026] Figure 4 a) is an original positive electrode current collector, and b) is a schematic diagram of a second positive electrode current collector having a step dressing layer disposed on its surface in one embodiment of the present invention.
[0027] Figure 5 Shown is a schematic diagram of a positive electrode composite electrode sheet in one embodiment of the present invention.
[0028] Figure 6 Shown is a schematic diagram of a positive electrode plate in one embodiment of the present invention.
[0029] Figure 7 Shown is a schematic diagram of a negative electrode plate in one embodiment of the present invention.
[0030] Figure 8 Shown is a schematic diagram of a solid-state battery cell in one embodiment of the present invention.
[0031] Description of Reference Numerals
[0032] 1 Release film 2 Step dressing layer
[0033] 3 Blank position 4 First positive electrode current collector
[0034] 5 Carbon coating layer 6 Positive electrode dressing layer
[0035] 7 Negative electrode current collector 8 Negative electrode dressing layer
[0036] 9 electrolyte layer 10 negative electrode sheet
[0037] 11 Positive electrode DETAILED DESCRIPTION
[0038] The present invention discloses a positive electrode composite electrode sheet and a preparation method thereof and a solid-state battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0039] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0040] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0041] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0042] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0043] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0044] In order to solve the problem in the prior art that the positive / negative electrode sheets have steps due to the area difference, and the stress is concentrated at the steps during the compaction process of the battery cell, which easily causes damage to the electrode sheets and short circuits, the present invention adopts the following technical solutions:
[0045] A first aspect of the present invention provides a method for preparing a positive electrode composite electrode sheet, the method comprising:
[0046] S1, performing a fiberization treatment and a first die-cutting treatment on the positive electrode slurry to obtain a positive electrode film;
[0047] S2, placing the step slurry on the surface of the release film and performing a drying process and a second die-cutting process to obtain a step material film having a step dressing layer on the surface and a blank position; wherein the blank position has the same shape and area as the positive electrode film;
[0048] S3, transferring the step dressing layer on the surface of the step material film to the surface of the first positive electrode current collector to obtain a second positive electrode current collector having a step dressing layer on the surface; wherein the step dressing layer has the blank position;
[0049] S4, placing the positive electrode film at the blank position of the second positive electrode current collector and performing a roll-combination process and a third die-cutting process.
[0050] The preparation method of the positive composite electrode sheet of the present invention adopts the method of applying the step slurry to the release film, drying and second die-cutting, and then transferring it to the first positive current collector. The positive electrode sheet is made by a dry process, and after die-cutting, it is composited to the blank position of the step dressing layer on the first positive current collector. The preparation method of the present invention establishes a continuous preparation process for step filling to reduce the presence of steps at the edges of the positive / negative electrode sheets, thereby reducing the electrode sheet damage and short circuit problems caused by stress concentration at the steps during the compaction of the battery cell, thereby improving the preparation efficiency of solid-state batteries.
[0051] According to the present invention, the step slurry may include a step powder and a first binder; the mass ratio of the step powder to the first binder is (80-99.9): (0.1-20). The step slurry in the present invention may also include an optional solvent. In one embodiment of the present invention, the solid content of the step slurry is 20-80%.
[0052] According to the present invention, the step powder may include at least one of a first solid electrolyte, boehmite and nano-alumina. Optionally, the first solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide electrolyte.
[0053] Exemplarily, the sulfide electrolyte is selected from Li 10 G 2 S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 C l0.3 , Li 9.6P 3 S 12 、Li 6 PS 5 X、Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 、Li 6 PS 5 Any one or a combination of two or more of Br, where X is selected from any one of Cl, Br, or I. The oxide solid electrolyte is selected from Li 7-x La 3 Zr 2-x Ta x O 12 、Li 7-2y La 3 Zr 2-y W y O 12 、Li 7- z La 3 Zr 2-z Nb z O 12 、Li 7 La 3 Zr 2 O 12 、Li 1+m Al m Ti 2-m (PO 4 ) 3 、LiPON and Li 1+n Al n Ge 2-n (PO 4 ) 3 Any one or a combination of two or more of them, where 0.2 < x < 2, 0.2 < y < 2, 0.2 < z < 2, 0.2 < m < 2, 0.2 < n < 2. The halide solid electrolyte is selected from Li 3 YCl 6 、Li 3 ErCl 6 、Li 3 YBr 6 、Li 3 InBr 6 和Li 3 InCl 6 Any one or a combination of two or more of them.
[0054] According to the present invention, the first binder is selected from at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium carboxymethyl cellulose (CMC), polyimide (PI), polyacrylonitrile (PAN), polypropylene (PP), polyethylene (PE) and polystyrene (PS).
[0055] According to the present invention, the difference between the thickness of the step dressing layer and the thickness of the positive electrode film is less than 1 μm; optionally, the thickness of the step dressing layer is 80-200 μm.
[0056] According to the present invention, the first positive electrode current collector is preferably a carbon-coated current collector; the carbon-coated current collector includes a metal foil and a carbon-coated layer disposed on the surface of the metal foil, and the carbon-coated current collector used in the present invention can be purchased from a commercial source or prepared by itself. Exemplarily, the metal foil can be an aluminum foil; optionally, the thickness of the carbon-coated layer is less than 0.5 μm. Exemplarily, the carbon-coated layer can include 50 to 99.5 wt% of a conductive agent and 0.5 to 50 wt% of a binder, wherein the conductive agent and the binder can be well known in the art and are not particularly limited here.
[0057] In one embodiment of the present invention, the release film may be a polyethylene terephthalate (PET) release film.
[0058] In one embodiment of the present invention, the positive electrode slurry may include a positive electrode active material, a conductive agent, a second solid electrolyte and a second binder.
[0059] For example, the positive electrode active material is lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, LiFePO 4 、LiFe 0.2 Mn 0.8 PO 4 、LiMn 2 O 4 、LiCoPO 4 、LiNiO 2、 LiNi 0.5 Mn 1.5 O 4、 LiCoO 2 、LiTiS 2 、LiNiO 2 , elemental sulfur and sulfur-carbon mixture, or any one or a combination of two or more thereof. Further, the nano-coating layer material may be selected from Li 3 PO 4 、Al 2 O 3 、LiNbO 3 、LiAlO 2 , Li3 BO 3 , Li 2 OZO 2 、MgO、HfO 2 , Li 2 SiO 3 , B 2 O 3 , Li 2 O、Nb 2 O 5 , P 2 O 5 、SiO 2 Sc 2 O 3 、TiO 2 and ZrO 2 Any one or a combination of two or more. And / or, the conductive agent is selected from any one or a combination of two or more of conductive carbon black (Super P), carbon nanofiber (VGCF), carbon nanotube, acetylene black, Ketjen black and conductive graphene. And / or, the second binder is selected from at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium carboxymethyl cellulose (CMC) polyimide (PI), polyacrylonitrile (PAN), polypropylene (PP), polyethylene (PE) and polystyrene (PS). And / or, the second solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide electrolyte.
[0060] The fiberization treatment involved in step S1 of the present invention may be well known to those skilled in the art. For example, the specific conditions of the fiberization treatment may be mixing at a temperature of 70 to 90° C. for 45 to 90 seconds using an internal mixer.
[0061] According to the present invention, in step S2, the drying conditions may include: a temperature of 60 to 120° C. and a time of 10 to 60 minutes.
[0062] In one embodiment of the present invention, the transfer involved in step S3 may include laminating a step material film having a step dressing layer and a blank position on the surface (the surface having a step dressing layer) with the surface of the first positive electrode current collector and then rolling. The rolling conditions may include: a temperature of 20 to 120°C, a pressure of 0.2 to 2 t / cm, and a time of 10 to 60 min.
[0063] According to the present invention, in step S4, the conditions of the roll-composite treatment may include: a temperature of 20 to 120° C., a pressure of 0.2 to 2 t / cm, and a time of 10 to 60 min. In an embodiment of the present invention, the size of the positive electrode composite sheet obtained by the third die-cutting treatment is preferably the same as the target negative electrode sheet size, so as to eliminate the presence of steps to the greatest extent.
[0064] A second aspect of the present invention provides a positive electrode composite electrode sheet, which is prepared according to the above method.
[0065] A third aspect of the present invention provides a solid-state battery, comprising a positive electrode plate, wherein the positive electrode plate is a positive electrode composite plate prepared according to the above method and / or is the above positive electrode composite plate.
[0066] One embodiment of the present invention, as Figure 1 As shown, the process flow for preparing solid-state batteries may include:
[0067] (1) Preparation of positive electrode sheet: The positive electrode powder is mixed evenly to obtain a positive electrode slurry, and the positive electrode slurry is subjected to a fiberization process and a first die-cutting process to obtain a positive electrode film. The step powder, the first binder and the solvent are homogenized to obtain a step slurry; the step slurry is applied to the surface of the release film to obtain a release film coated with the step slurry, such as Figure 2 The release film coated with the step slurry is dried and subjected to a second die-cutting process to obtain a step material film having a step coating layer on the surface and a blank position, as shown. Figure 3 As shown, the blank position is the same as the shape and area of the positive electrode film. The step material layer on the surface of the step material film is transferred to the surface of the positive electrode current collector provided with a carbon coating layer to obtain a second positive electrode current collector with a step dressing layer on the surface, such as Figure 4 As shown, the step dressing layer on the surface of the second positive electrode current collector has a blank position. The positive electrode film prepared in the above steps is placed on the blank position of the second positive electrode current collector and subjected to a roll-pressing composite treatment to obtain a positive electrode composite film, such as Figure 5 The positive electrode composite film is subjected to a third die-cutting process to obtain a positive electrode composite electrode sheet. The schematic diagram of the positive electrode composite electrode sheet is shown in Figure 6 shown.
[0068] (2) Preparation of negative electrode sheet: The negative electrode powder is mixed evenly to obtain negative electrode slurry, and the negative electrode slurry is subjected to fiberization treatment and fourth die-cutting treatment to obtain a negative electrode film. The electrolyte membrane prepared by dry or wet method is transferred to the negative electrode film and fifth die-cutting treatment is performed to obtain a negative electrode sheet. The schematic diagram of the negative electrode sheet is shown in FIG. Figure 7 shown.
[0069] (3) Preparation of solid-state battery cells: The prepared positive electrode composite plate and negative electrode plate are stacked, compacted and other subsequent steps to prepare a solid-state battery cell. The schematic diagram of the solid-state battery cell is shown in the figure. Figure 8 shown.
[0070] After the battery cell is prepared, the subsequent welding, packaging and other process steps can be adapted and carried out according to the commonly used methods in the industry to finally obtain a solid-state battery. If pressure needs to be applied to exert the performance of the solid-state battery, commonly used pressurizing equipment can be used to apply pressure during the preparation process or during use.
[0071] The equipment that may be used in the specific implementation process of the present invention includes but is not limited to mixers, coaters, ovens, roller presses, die cutters, spot welders, stacking machines, sealing machines, isostatic presses, etc. The above equipment are all commonly used equipment in the industry. Within the scope understandable to technicians in this field, each equipment can be replaced without limitation.
[0072] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0073] Example 1
[0074] Preparation of positive electrode film: ternary 8 series materials, Li 6 PS 5 Cl, Super P and polytetrafluoroethylene (PTFE) are mixed in a ratio of 80:17:1:2 to obtain a positive electrode slurry, and the positive electrode slurry is subjected to fiberization and film-forming treatment to obtain a first positive electrode material film, and the first positive electrode material film has a thickness of 190 μm (150 μm after compaction). The first positive electrode material film is subjected to a first die-cutting treatment in a size of 43*56 mm to obtain a positive electrode film.
[0075] Preparation of step layer: Boehmite and PVDF are homogenized in a ratio of 95:5, the solvent is N-methylpyrrolidone (NMP), the solid content is 40%, and the step slurry is prepared after homogenization. The step slurry is coated on the PET release film with a width of 62mm and a thickness of 150μm. After drying, a second die-cutting process is performed according to the size of 43*56mm to obtain a step material film with a step dressing layer on the surface and a blank position. Then the step dressing layer on the surface of the step material film is transferred to the surface of the first positive electrode collector (carbon-coated aluminum foil) (both sides), wherein the transfer includes a roller pressing process, the roller pressing temperature is 40°C, and the pressure is 0.5t / cm, to obtain a second positive electrode collector with a step dressing layer on the surface.
[0076] Preparation of positive electrode sheet: accurately stack the die-cut positive electrode film on the blank area of the step dressing layer on the second positive electrode collector for roller pressing and compounding treatment. The rolling temperature is 40°C and the pressure is 0.5t / cm, and then the third die-cutting treatment is performed according to the size of 45*58mm to obtain the positive electrode sheet of this embodiment.
[0077] Preparation of negative electrode; SIC, Li 6 PS 5 Cl, SuperP and PTFE are mixed in a ratio of 82:15:1:2 to obtain negative electrode slurry, and the negative electrode slurry is subjected to fiberization and film-forming treatment to obtain a negative electrode film with a thickness of 60μm, which is then composited onto a carbon-coated copper foil. After film formation, it is die-cut into a size of 45*58mm to obtain a negative electrode sheet. When composited, only one side is composited to obtain a single-sided negative electrode sheet.
[0078] Preparation of battery cells: stack 5 double-sided positive electrode sheets, 4 double-sided negative electrode sheets and 2 single-sided negative electrode sheets, weld the tabs, and then package them in aluminum plastic film. After isostatic pressing, the battery cell of the embodiment can be obtained. The isostatic pressing pressure is 500Mpa and the temperature is 80°C. Prepare 5 parallel sample battery cells with a designed capacity of 1000mAh.
[0079] Comparative Example 1
[0080] Preparation of positive electrode: ternary 8 series materials, Li 6 PS 5 Cl, Super P and PTFE were mixed in a ratio of 80:17:1:2 to obtain a positive electrode slurry, and the positive electrode slurry was subjected to fiberization and film-forming treatment to obtain a first positive electrode material film with a thickness of 190 μm. The first positive electrode material film was composited onto a carbon-coated aluminum foil. After film formation, it was die-cut into a size of 43*56 mm to obtain a positive electrode sheet of this comparative example.
[0081] Negative electrode preparation: SIC, Li 6 PS 5 Cl, Super P and PTFE are mixed in a ratio of 82:15:1:2 to obtain negative electrode slurry, and the negative electrode slurry is subjected to fiberization and film-forming treatment to obtain a negative electrode film with a thickness of 60μm, which is then composited onto a carbon-coated copper foil. After film formation, it is die-cut into a size of 45*58mm to obtain a negative electrode sheet. When composited, only one side is composited to obtain a single-sided negative electrode sheet.
[0082] Preparation of battery cells: 5 double-sided positive electrode sheets, 4 double-sided negative electrode sheets and 2 single-sided negative electrode sheets are stacked, the pole ears are welded, and then packaged in aluminum plastic film. After isostatic pressing, the battery cell of this comparative example can be obtained. The isostatic pressing pressure is 500Mpa and the temperature is 80°C. Five parallel sample battery cells are prepared with a designed capacity of 1000mAh.
[0083] Test Example 1
[0084] Data testing was performed on the five parallel sample cells prepared in Example 1 and Comparative Example 1, and the test results are shown in Table 1.
[0085] The initial voltage is measured by a charge and discharge instrument.
[0086] Test method for first discharge capacity and first coulomb efficiency: the battery cell is subjected to constant current charge and discharge test, 0.1C rate, voltage range 2.0~4.25V. The specific operation is: constant current charge to 4.25V at current density 0.1C, record the charge capacity at this time as the first charge capacity; discharge at 4.25V constant voltage to cut-off current 0.05C, record the discharge capacity at this time as the first discharge capacity. First coulomb efficiency = first discharge capacity / first charge capacity*100%.
[0087] Table 1
[0088] Battery Cell / Performance Initial voltage / V First discharge capacity / mAh First coulombic efficiency / % Example 1-1 0.35 1002.07 89.05 Example 1-2 0.26 991.28 88.09 Examples 1-3 0.30 1000.44 88.35 Examples 1-4 0.29 1014.90 88.89 Examples 1-5 0.33 999.17 88.84 Comparative Example 1-1 0.02 213.16 21.70 Comparative Example 1-2 0.11 580.53 57.73 Comparative Examples 1-3 0.08 304.07 30.73 Comparative Examples 1-4 0.03 278.15 28.07 Comparative Examples 1-5 0.10 682.69 67.75
[0089] It can be seen from the data in Table 1 that the initial voltage of each parallel sample battery cell prepared in Example 1 is normal, the discharge capacity also meets the design value of 1000mAh, and the first coulombic efficiency is significantly higher than that of the comparative example. Each parallel sample battery cell prepared in Comparative Example 1 has a short circuit to varying degrees, resulting in a low initial voltage, a low first discharge capacity and a low first coulombic efficiency.
[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a positive electrode composite electrode sheet, It is characterized in that The method comprises: S1, performing a fiberization treatment and a first die-cutting treatment on the positive electrode slurry to obtain a positive electrode film; S2, placing the step slurry on the surface of the release film and performing a drying process and a second die-cutting process to obtain a step material film having a step dressing layer on the surface and a blank position; wherein the blank position has the same shape and area as the positive electrode film; S3, transferring the step dressing layer on the surface of the step material film to the surface of the first positive electrode current collector to obtain a second positive electrode current collector having a step dressing layer on the surface; wherein the step dressing layer has the blank position; S4, placing the positive electrode film at the blank position of the second positive electrode current collector and performing a roll-combination process and a third die-cutting process.
2. The preparation method according to claim 1, It is characterized in that The step slurry includes a step powder and a first binder; wherein the mass ratio of the step powder to the first binder is (80-99.9): (0.1-20).
3. The preparation method according to claim 2, It is characterized in that The step powder includes at least one of a first solid electrolyte, boehmite and nano-alumina; Optionally, the first solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte and a halide electrolyte.
4. The preparation method according to claim 2, It is characterized in that The first binder is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylic acid, sodium carboxymethyl cellulose, polyimide, polyacrylonitrile, polypropylene, polyethylene and polystyrene.
5. The preparation method according to claim 1, It is characterized in that The difference between the thickness of the step dressing layer and the thickness of the positive electrode film is less than 1 μm; Optionally, the step dressing layer has a thickness of 80-200 μm.
6. The preparation method according to claim 1, It is characterized in that The first positive electrode current collector is a carbon-coated current collector; the carbon-coated current collector comprises a metal foil and a carbon-coated layer arranged on the surface of the metal foil.
7. The preparation method according to claim 1, It is characterized in that In step S2, the drying process conditions include: a temperature of 60 to 120°C and a time of 10 to 60 minutes.
8. The preparation method according to claim 1, It is characterized in that In step S4, the conditions of the roller-combination treatment include: temperature of 20 to 120° C., pressure of 0.2 to 2 t / cm, and time of 10 to 60 min.
9. A positive electrode composite electrode sheet, It is characterized in that The positive electrode composite electrode sheet is prepared according to the method described in any one of claims 1 to 8.
10. A solid-state battery, It is characterized in that The solid-state battery comprises a positive electrode sheet, and the positive electrode sheet is a positive electrode composite sheet prepared by the method according to any one of claims 1 to 8 and / or is the positive electrode composite sheet according to claim 9.