Super-folding lithium ion battery electrode material, preparation method thereof and super-folding total battery
The ultra-folded lithium-ion battery electrode material, prepared through electrostatic spinning and carbonization, addresses the flexibility issues of foldable devices by ensuring stable electrochemical performance and durability through 500,000 folds, facilitating large-scale production.
Patent Information
- Application Number
- CN202411198057.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Current foldable electronic devices are hindered by rigid energy storage devices that cannot withstand multiple true folds due to the limitations of traditional conductive materials and electrochemically active substances, which reduce flexibility and hinder the development of truly foldable electronics.
A method for preparing an ultra-folded lithium-ion battery electrode material using electrostatic spinning and gradient temperature carbonization, combining carbon nanotubes and LiFePO4 particles with polyacrylonitrile, and assembling them into a full battery with specific electrochemical components to achieve high conductivity and flexibility.
The ultra-folded lithium-ion battery electrode material and full battery can withstand 500,000 folds without structural damage, maintaining stable electrochemical properties and enabling flexible, large-scale production.
Smart Images

Figure CN119069673A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of flexible energy storage, and specifically relates to an ultra-folded lithium-ion battery electrode material, a preparation method thereof, and an ultra-folded full battery. Background Art
[0002] As people's demand for the portability and functionality of electronic products increases, the foldability of flexible electronics becomes increasingly important. However, the development of foldable electronic products is currently in its early stages. Although some foldable devices and even products have been launched, they are not "true folds" that are 180 degrees and close to each other on both sides. As for the foldable smartphones currently on sale, they are folded by rotating the axis and cannot be deformed or reduced in space at will. Energy storage devices, which are the cornerstone of the new generation of foldable electronic products, are still basically rigid structures, which will greatly hinder the development of foldable electronics. Traditional intrinsic conductive materials, whether metals, conductive polymers or carbon materials, cannot withstand a large number of true foldings due to the rigid short-range chemical bond limitations. In addition, existing electrochemically active substances usually have higher rigidity. When compounded with traditional flexible substrates, the overall flexibility will be further reduced, making it more difficult to achieve true folding operations. Based on this, the assembled devices are far from meeting the requirements of true folding.
[0003] Therefore, preparing an electrode material and a full battery that meets super-folding performance and has high conductivity has become an urgent problem to be solved. Summary of the invention
[0004] The present invention is made to solve the above-mentioned problems, and its purpose is to provide an ultra-folded lithium-ion battery electrode material, a preparation method thereof and an ultra-folded full battery.
[0005] The present invention provides a method for preparing an ultra-folded lithium-ion battery electrode material, which has the following characteristics: the material is prepared by utilizing electrostatic spinning combined with gradient temperature carbonization technology, and specifically comprises the following steps: S10, dispersing carbon nanotubes and LiFePO4 particles in an N,N-dimethylformamide solution, and sequentially ultrasonicating and stirring to obtain a suspension; S20, adding polyacrylonitrile to the suspension, and promoting the dissolution of polypropylene by stirring to obtain a polymer mixed gel; S30, loading the polymer mixed gel into a syringe and performing electrostatic spinning to prepare a polymer film precursor; S40, performing pre-carbonization treatment on the polymer film precursor in a tubular furnace to obtain a pre-carbonized sample; S50, carbonizing the pre-carbonized sample to obtain an ultra-folded lithium-ion battery electrode material.
[0006] The method for preparing the ultra-folded lithium-ion battery electrode material provided by the present invention may also have the following characteristics: in step S10, the amount of N,N-dimethylformamide solution is 5-10 mL, the amount of carbon nanotubes is 0.01-0.7 g, the LiFePO4 particle size is 10 nm-300 nm, the amount of LiFePO4 is 0.01-0.6 g, the ultrasonic time is 1 h-8 h, and the stirring time is 1 h-8 h.
[0007] The method for preparing the ultra-folded lithium-ion battery electrode material provided by the present invention may also have the following characteristics: in step S20, the amount of polyacrylonitrile is 1.0-1.6 g, the stirring time is 6 h-48 h, and in step S30, the conditions for electrospinning are: the voltage at the syringe needle connection end is set to 12-16 kV, the voltage at the spinning product receiving end is set to -2 kV, the propulsion speed is set to 0.01-0.02 mL / min, the receiving distance is set to 18 cm, and the needle propulsion amount is 2 mL / h;
[0008] The preparation method of the ultra-folded lithium-ion battery electrode material provided by the present invention may also have the following characteristics, wherein, in step S40, the pre-carbonization process is: heating to 250-300°C at a heating rate of 0.5-5°C / min in an air atmosphere, and keeping warm at 250-300°C for 2h, and then naturally cooling to room temperature after the end.
[0009] The method for preparing the ultra-folded lithium-ion battery electrode material provided by the present invention may also have the following characteristics, wherein the ultra-folded lithium-ion battery electrode material is an ultra-folded positive electrode material, and in step S50, the process of carbonization treatment is: heating to 250-300°C at a heating rate of 2-5°C / min under a nitrogen atmosphere and keeping warm for 1 hour, and then heating to 650-750°C at a heating rate of 0.5-1.5°C / min and keeping warm for 2 hours.
[0010] The method for preparing the ultra-folded lithium-ion battery electrode material provided by the present invention may also have the following characteristics, wherein the ultra-folded lithium-ion battery electrode material is an ultra-folded negative electrode material, and in step S50, the process of carbonization treatment is: heating to 250-300°C at a heating rate of 2-5°C / min under a nitrogen atmosphere and keeping warm for 1 hour, and then heating to 760-850°C at a heating rate of 0.5-1.5°C / min and keeping warm for 2 hours.
[0011] The present invention provides an ultra-folded lithium-ion battery electrode material having the following characteristics, and is prepared by the preparation method of the ultra-folded lithium-ion battery electrode material provided by the present invention.
[0012] The present invention provides an ultra-folded full battery having the following characteristics: it contains the ultra-folded lithium-ion battery electrode material provided by the present invention.
[0013] The ultra-folded full battery provided by the present invention may also have the following characteristics, including an ultra-folded positive electrode material prepared by the method for preparing an ultra-folded lithium-ion battery electrode material provided by the present invention and an ultra-folded negative electrode material prepared by the method for preparing an ultra-folded lithium-ion battery electrode material provided by the present invention.
[0014] The super-folded full battery provided by the present invention may also have such a feature, specifically comprising the following steps: a first step, taking two sheets of super-folded positive electrode material and super-folded negative electrode material, immersing them in a lithium naphthalene solution with a concentration of 1%, and performing a pre-lithiation treatment to obtain a lithiated super-folded positive electrode material and a lithiated super-folded negative electrode material; a second step, taking the lithiated super-folded positive electrode material as a self-supporting positive electrode, taking the lithiated super-folded negative electrode material as a self-supporting negative electrode, and selecting a Celgard series diaphragm (a microporous single-layer or multi-layer membrane whose main component is polypropylene or a composite mixture of polypropylene and polyethylene) as a porous The diaphragm, lithium salt organic system as electrolyte, insulating polymer film as outer packaging material, ultra-thin aluminum foil and copper foil as positive and negative ears respectively, are stacked and assembled into a full battery, wherein the porous diaphragm includes any one or more of Celgard series diaphragms (microporous single-layer or multi-layer membranes whose main components are polypropylene or a mixture of polypropylene and polyethylene), thin layers of glass fiber, and paper diaphragms, and the connection method of the ears to the self-supporting positive electrode and the self-supporting negative electrode is to bond them with the configured PVDF glue mixed with carbon nanotubes (PVDF: N-methylpyrrolidone: CNTs = 1:19:5wt%).
[0015] Functions and Effects of the Invention
[0016] According to an embodiment of the present invention, an ultra-folded lithium-ion battery electrode material, a preparation method thereof, and an ultra-folded full battery are provided. In the preparation method of the ultra-folded lithium-ion battery electrode material, carbon nanotubes and LiFePO4 particles are first dispersed in an N,N-dimethylformamide solution, and ultrasonic and stirring are performed in sequence to obtain a uniform suspension. Polyacrylonitrile is then added to the suspension, and the dissolution of polypropylene is promoted by stirring to obtain a polymer mixed gel. The polymer mixed gel is then loaded into a syringe for electrospinning to prepare a polymer film precursor. The polymer film precursor is then pre-carbonized in a tubular furnace to obtain a pre-carbonized sample. Finally, the pre-carbonized sample is carbonized to obtain an ultra-folded lithium-ion battery electrode material.
[0017] Therefore, the ultra-foldable full battery made of the ultra-foldable lithium-ion battery electrode material prepared in this way can not only avoid structural damage during 500,000 foldings, but also maintain stable and excellent electrochemical properties.
[0018] In addition, the preparation process of the ultra-folded lithium-ion battery electrode material is simple and efficient, which is conducive to large-scale production and has broad application prospects in the field of flexible devices.
[0019] In addition, since the ultra-folded full battery provided by the present invention includes the ultra-folded battery electrode material prepared by the preparation method of the ultra-folded lithium-ion battery electrode material of the present invention, the ultra-folded full battery can also be folded multiple times without its structure being damaged, and the electrochemical performance can remain stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The XRD and SEM images of the self-supporting superfolded cathode material in Example 2 are shown;
[0021] Figure 2 The XRD pattern and SEM image of the super-folded negative electrode material obtained in Example 2 are shown;
[0022] Figure 3 The resistivity change diagram and crease SEM image of the super-folded cathode material obtained in Example 2 after folding 500,000 times are shown;
[0023] Figure 4 The SEM image of the non-superfolded lithium-ion electrode material obtained in Example 4 after being folded several times is shown;
[0024] Figure 5 A digital photograph showing another non-superfolded lithium-ion electrode material obtained in Example 5 after being folded several times;
[0025] Figure 6 The digital images of the unfolding / folding test of the ultra-folded full battery obtained in Example 6 during multiple folding processes and the in-situ dynamic folding electrochemical test performance are shown. DETAILED DESCRIPTION
[0026] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the following embodiments and the accompanying drawings specifically illustrate an ultra-folded lithium-ion battery electrode material, a preparation method thereof and an ultra-folded full battery of the present invention.
[0027] Example 1
[0028] This embodiment provides an ultra-folded lithium-ion battery electrode material and a preparation method thereof.
[0029] The electrode material of the super-folded lithium-ion battery can be a super-folded positive electrode material or a super-folded negative electrode material, and the preparation processes of the two are slightly different.
[0030] The method for preparing the super-folded cathode material comprises the following steps:
[0031] Step 1: Disperse 0.4 g of carbon nanotubes and 0.1 g of LiFePO4 particles in 10 mL of N,N-dimethylformamide solution, ultrasonicate for 1 h and magnetically stir for 2 h to obtain a suspension.
[0032] Step 2: Dissolve 1.3 g of polyacrylonitrile in the suspension obtained in step 1, and stir magnetically for 6 h to obtain a polymer mixed gel.
[0033] Step three, load the polymer mixed gel obtained in step two into a syringe, set the voltage at the syringe needle connecting end to 12kV, set the voltage at the spinning product receiving end to -2kV, set the propulsion speed to 0.01mL / min, set the receiving distance to 18cm, and set the needle propulsion amount to 2mL / h, and perform electrospinning to prepare a polymer membrane precursor.
[0034] Step 4: Pre-carbonize the polymer composite film precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the material, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 700°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain a super-folded cathode material.
[0035] The preparation method of the super-folded negative electrode material is exactly the same as steps 1 to 4 of the preparation method of the super-folded positive electrode material, except that the reaction conditions of step 5 are slightly different. Specifically, step 5 of the preparation method of the super-folded negative electrode material is:
[0036] Step 5: Pre-carbonize the polymer composite membrane precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the polymer composite membrane precursor, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 800°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain the super-folded negative electrode material.
[0037] Example 2
[0038] This embodiment provides an ultra-folded lithium-ion battery electrode material and a preparation method thereof.
[0039] The electrode material of the super-folded lithium-ion battery can be a super-folded positive electrode material or a super-folded negative electrode material, and the preparation processes of the two are slightly different.
[0040] The method for preparing the super-folded cathode material comprises the following steps:
[0041] Step 1: Disperse 0.5 g of carbon nanotubes and 0.2 g of LiFePO4 particles in 10 mL of N,N-dimethylformamide solution, ultrasonicate for 1 h and magnetically stir for 2 h to obtain a suspension.
[0042] Step 2: dissolve 1.3 g of polyacrylonitrile in the suspension obtained in step 1, and stir magnetically for 8 h to obtain a polymer mixed gel.
[0043] Step three, load the polymer mixed gel obtained in step two into a syringe, set the voltage at the syringe needle connecting end to 12kV, set the voltage at the spinning product receiving end to -2kV, set the propulsion speed to 0.01mL / min, set the receiving distance to 18cm, and set the needle propulsion amount to 2mL / h, and perform electrospinning to prepare a polymer membrane precursor.
[0044] Step 4: Pre-carbonize the polymer composite film precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the material, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 700°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain a super-folded cathode material.
[0045] Figure 1 The XRD and SEM images of the super-folded fiber positive electrode material obtained in Example 2 are shown.
[0046] Depend on Figure 1 The XRD pattern shows that the composite material is composed of PAN-derived amorphous carbon, carbon nanotubes and LiFePO4. Figure 1 As can be seen from the SEM image, the composite material is mainly composed of a network structure assembled by mutually dispersed fibers overlapping each other, and LiFePO4 and carbon nanotubes are mainly wrapped inside the fibers.
[0047] The preparation method of the super-folded negative electrode material is exactly the same as steps 1 to 4 of the preparation method of the super-folded positive electrode material, except that the reaction conditions of step 5 are slightly different. Specifically, step 5 of the preparation method of the super-folded negative electrode material is:
[0048] Step 5: Pre-carbonize the polymer composite membrane precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the polymer composite membrane precursor, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 800°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain the super-folded negative electrode material.
[0049] Figure 2 The XRD and SEM images of the super-folded fiber positive electrode material obtained in Example 2 are shown.
[0050] Depend on Figure 2 From the XRD diagram, it can be seen that the composite material is composed of PAN-derived amorphous carbon, CNTs, Li3PO4 and Fe2P, and the LiFePO4 phase has been basically completely decomposed. Figure 2 As can be seen from the SEM image, the negative electrode material is also mainly composed of a network structure assembled by mutually dispersed fibers overlapping each other, and the fibers are still intact and without breaks.
[0051] Figure 3 The resistivity change graph and crease SEM image of the super-folded fiber positive electrode material obtained in Example 2 after folding 500,000 times are shown.
[0052] Depend on Figure 3 From the resistivity change diagram, it can be seen that the fiber membrane can maintain a relatively stable resistivity during folding. Figure 3 The SEM image of the crease shows that the fiber membrane is intact as a whole, with two obvious grooves at the crease. The fibers at the grooves remain intact without any signs of breakage.
[0053] Example 3
[0054] This embodiment provides an ultra-folded lithium-ion battery electrode material and a preparation method thereof.
[0055] The electrode material of the super-folded lithium-ion battery can be a super-folded positive electrode material or a super-folded negative electrode material, and the preparation processes of the two are slightly different.
[0056] The method for preparing the super-folded cathode material comprises the following steps:
[0057] Step 1: Disperse 0.6 g of carbon nanotubes and 0.3 g of LiFePO4 particles in 10 mL of N,N-dimethylformamide solution, ultrasonicate for 2 h and magnetically stir for 4 h to obtain a suspension.
[0058] Step 2: Dissolve 1.3 g of polyacrylonitrile in the suspension obtained in step 1, and stir magnetically for 12 h to obtain a polymer mixed gel.
[0059] Step three, load the polymer mixed gel obtained in step two into a syringe, set the voltage at the syringe needle connecting end to 12kV, set the voltage at the spinning product receiving end to -2kV, set the propulsion speed to 0.01mL / min, set the receiving distance to 18cm, and set the needle propulsion amount to 2mL / h, and perform electrospinning to prepare a polymer membrane precursor.
[0060] Step 4: Pre-carbonize the polymer composite film precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the material, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 700°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain a super-folded cathode material.
[0061] The preparation method of the super-folded negative electrode material is exactly the same as steps 1 to 4 of the preparation method of the super-folded positive electrode material, except that the reaction conditions of step 5 are slightly different. Specifically, step 5 of the preparation method of the super-folded negative electrode material is:
[0062] Step 5: Pre-carbonize the polymer composite membrane precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the polymer composite membrane precursor, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 800°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain the super-folded negative electrode material.
[0063] Example 4
[0064] This embodiment provides a non-superfolded lithium-ion battery electrode material and a preparation method thereof.
[0065] The method for preparing a non-superfolded lithium-ion battery electrode material comprises the following steps:
[0066] Step 1: Disperse 0.1 g of carbon nanotubes and 0.3 g of LiFePO4 particles in 5 mL of N,N-dimethylformamide solution, ultrasonicate for 3 h and magnetically stir for 2 h to obtain a suspension.
[0067] Step 2: Dissolve 1.6 g of polyacrylonitrile in the suspension obtained in step 1, and stir magnetically for 24 hours to obtain a polymer mixed gel.
[0068] Step three, load the polymer mixed gel obtained in step two into a syringe, set the voltage at the syringe needle connecting end to 16kV, the voltage at the spinning product receiving end to -2kV, the propulsion speed to 0.02mL / min, the receiving distance to 18cm, the needle propulsion amount to 2mL / h, and perform electrospinning to prepare a polymer membrane precursor.
[0069] Step 4: Pre-carbonize the polymer composite film precursor prepared in step 3, specifically, heating the temperature to 260°C at a heating rate of 1°C / min in air, then keeping it at 260°C for 2h, and then cooling it to room temperature. Then, carbonize the polymer composite film precursor, specifically, heating the temperature to 260°C at a heating rate of 2°C / min in a nitrogen atmosphere, keeping it for 1h, then heating the temperature to 700°C at a heating rate of 1°C / min, and keeping it for 2h, to obtain a lithium-ion battery electrode material.
[0070] Figure 4 The SEM image of the non-superfolded lithium-ion electrode material obtained in Example 4 after being folded several times is shown.
[0071] It can be seen from the figure that the fiber is obviously broken at the folding point.
[0072] Example 5
[0073] This embodiment provides another non-superfolded lithium-ion battery electrode material and a preparation method thereof.
[0074] The method for preparing a non-superfolded lithium-ion battery electrode material comprises the following steps:
[0075] Step 1: Disperse 0.7 g of carbon nanotubes and 0.6 g of LiFePO4 particles in 10 mL of N,N-dimethylformamide solution, ultrasonicate for 2 h and magnetically stir for 3 h to obtain a suspension.
[0076] Step 2: dissolve 1.0 g of polyacrylonitrile in the suspension obtained in step 1, and stir magnetically for 48 hours to obtain a polymer mixed gel.
[0077] Step three, load the polymer mixed gel obtained in step two into a syringe, set the voltage at the syringe needle connecting end to 12kV, set the voltage at the spinning product receiving end to -2kV, set the propulsion speed to 0.01mL / min, set the receiving distance to 18cm, and set the needle propulsion amount to 2mL / h, and perform electrospinning to prepare a polymer membrane precursor.
[0078] Step 4: Pre-carbonize the polymer composite film precursor prepared in step 3, specifically, heating the temperature to 300°C at a heating rate of 5°C / min in air, then keeping it at 300°C for 2h, and then cooling it to room temperature. Then, carbonize the polymer composite film precursor, specifically, heating the temperature to 300°C at a heating rate of 5°C / min in a nitrogen atmosphere for 1h, then heating the temperature to 700°C at a heating rate of 1°C / min, and keeping it at 2h, to obtain a non-superfolded lithium-ion battery electrode material.
[0079] Figure 5 A digital photograph of another non-superfolded lithium-ion electrode material obtained in Example 5 after being folded several times is shown.
[0080] It is obvious that after folding, the originally complete fiber membrane breaks into two halves.
[0081] Example 6
[0082] This embodiment provides a method for preparing a super-folded full battery comprising a super-folded positive electrode material and a super-folded negative electrode material prepared in any one of Embodiments 1-3, comprising the following steps:
[0083] Step 1: Take two sheets of the super-folded positive electrode material and the super-folded negative electrode material prepared in any one of Examples 1-3, soak them in a 1% lithium naphthalene solution for pre-lithiation treatment.
[0084] Step 2: Take the lithiated superfolded positive electrode material in step 1 as a self-supporting positive electrode, the lithiated superfolded negative electrode material as a self-supporting negative electrode, the Celgard series diaphragm (a microporous single-layer or multi-layer film whose main component is polypropylene or a mixture of polypropylene and polyethylene) as a porous diaphragm, a lithium salt organic system as an electrolyte, an insulating polymer film as an outer packaging material, ultra-thin aluminum foil and copper foil as positive and negative electrode ears respectively, and stack and assemble them into a full battery.
[0085] Figure 6 The digital images of the unfolding / folding test of the ultra-folded full battery obtained in Example 6 during multiple folding processes and the in-situ dynamic folding electrochemical test performance are shown.
[0086] like Figure 6 As shown in the figure, the digital photos are the unfolded and folded states of the full battery during multiple folding processes, indicating that the full battery did not break during the multiple folding processes. The full battery was able to perform normal charge and discharge behavior during 500,000 dynamic foldings, and maintained a relatively stable specific capacity (1Ag -1 Its capacity is about 117 mAh g -1 ), which illustrates the excellent folding electrochemical stability of the full cell.
[0087] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing an ultra-folded lithium-ion battery electrode material, characterized in that: The preparation is carried out by using electrospinning combined with gradient temperature carbonization technology, which specifically includes the following steps: S10, dispersing carbon nanotubes and LiFePO4 particles in N,N-dimethylformamide solution, and sequentially ultrasonicating and stirring to obtain a suspension; S20, adding polyacrylonitrile to the suspension, and promoting the dissolution of polypropylene by stirring to obtain a polymer mixed gel; S30, loading the polymer mixed gel into a syringe for electrospinning to prepare a polymer membrane precursor, S40, pre-carbonizing the polymer film precursor in a tube furnace to obtain a pre-carbonized sample; S50, performing carbonization treatment on the pre-carbonized sample to obtain an ultra-folded lithium-ion battery electrode material.
2. The method for preparing an ultra-folded lithium-ion battery electrode material according to claim 1, characterized in that: in, In the step S10, the amount of the N,N-dimethylformamide solution is 5-10 mL, the amount of the carbon nanotube is 0.01-0.7 g, the LiFePO4 particle size is 10 nm-300 nm, the amount of LiFePO4 is 0.01-0.6 g, the ultrasonic time is 1 h-8 h, and the stirring time is 1 h-8 h.
3. The method for preparing the ultra-folded lithium-ion battery electrode material according to claim 1, characterized in that: in, In step S20, the amount of polyacrylonitrile is 1.0-1.6 g, and the stirring time is 6 h-48 h. In step S30, the conditions for performing the electrospinning are: the voltage at the syringe needle connection end is set to 12-16 kV, the voltage at the spinning product receiving end is set to -2 kV, the propulsion speed is set to 0.01-0.02 mL / min, the receiving distance is set to 18 cm, and the needle propulsion amount is 2 mL / h.
4. The method for preparing the ultra-folded lithium-ion battery electrode material according to claim 1, characterized in that: in, In step S40, the pre-carbonization process is as follows: heating the temperature to 250-300°C at a heating rate of 0.5-5°C / min in an air atmosphere, and keeping the temperature at 250-300°C for 2 hours, and then naturally cooling to room temperature.
5. The method for preparing the ultra-folded lithium-ion battery electrode material according to claim 1, characterized in that: in, The ultra-folded lithium-ion battery electrode material is an ultra-folded positive electrode material, In step S50, the carbonization process is as follows: in a nitrogen atmosphere, the temperature is raised to 250-300°C at a heating rate of 2-5°C / min and kept for 1 hour, and then the temperature is raised to 650-750°C at a heating rate of 0.5-1.5°C / min and kept for 2 hours.
6. The method for preparing an ultra-folded lithium-ion battery electrode material according to claim 1, characterized in that: in, The ultra-folded lithium-ion battery electrode material is an ultra-folded negative electrode material, In step S50, the carbonization process is as follows: in a nitrogen atmosphere, the temperature is raised to 250-300°C at a heating rate of 2-5°C / min and kept for 1 hour, and then the temperature is raised to 760-850°C at a heating rate of 0.5-1.5°C / min and kept for 2 hours.
7. An ultra-folded lithium-ion battery electrode material, characterized in that: The ultra-folded lithium-ion battery electrode material is prepared by the preparation method of any one of claims 1 to 6.
8. An ultra-foldable full battery, characterized in that: Contains the ultra-folded lithium-ion battery electrode material according to claim 7.
9. An ultra-foldable full battery, characterized in that: include: The super-folded positive electrode material is prepared by the method for preparing the super-folded lithium-ion battery electrode material according to claim 5; and The super-folded negative electrode material is prepared by the method for preparing the super-folded lithium-ion battery electrode material described in claim 6.
10. The ultra-folded full battery according to claim 9, characterized in that: The method for preparing the ultra-folded full battery comprises the following steps: The first step is to take two sheets of the super-folded positive electrode material and two sheets of the super-folded negative electrode material, soak them in a 1% lithium naphthalene solution, and perform a pre-lithiation treatment to obtain a lithiated super-folded positive electrode material and a lithiated super-folded negative electrode material; The second step is to use the lithiated superfolded positive electrode material as a self-supporting positive electrode, use the lithiated superfolded negative electrode material as a self-supporting negative electrode, select Celgard series diaphragm as a porous diaphragm, lithium salt organic system as an electrolyte, insulating polymer film as an outer packaging material, ultra-thin aluminum foil and copper foil as positive and negative ears respectively, and stack and assemble them into a full battery. The porous diaphragm includes any one or more of Celgard series diaphragms, thin layers of glass fiber, and paper diaphragms. The connection between the tabs and the self-supporting positive electrode and the self-supporting negative electrode is bonding with a configured PVDF glue mixed with carbon nanotubes.
Citation Information
Patent Citations
Method for preparing cathode material of lithium iron phosphate without coating of pole piece
CN103236544A
Preparation method for carbon-based lithium ion battery electrode material
CN105355872A
Lithium pre-doping method for electrode plate of lithium-ion battery
CN105489841A
Electrostatic spinning-carbonization preparation method of foldable flexible pure nanometer carbon fiber
CN107083584A
Arbitrarily and repeatedly foldable ultra-flexible carbon material and preparation method thereof
CN109208121A