Binder composition for secondary battery, functional layer, member, and secondary battery
By using a specific proportional composition of epoxy phosphate and bonding material in lithium-ion batteries, the problem of poor stability of the positive electrode slurry is solved, the circulation performance and adhesion of the secondary battery are significantly improved, and the excellent battery characteristics are ensured And reduce internal resistance.
Patent Information
- Application Number
- CN202310594958.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-03
AI Technical Summary
The positive electrode slurry of the existing lithium-ion batteries has poor stability, resulting in unstable adhesion, affecting battery performance, and it is difficult to significantly improve the circulation performance of the secondary battery.
Using an adhesive composition containing a bonding material and an epoxy phosphate, the mass ratio of the epoxy phosphate to the bonding material is 10-80, which is used to prepare a functional layer, enhance adhesion and improve the electrode composite material layer. Repressive.
The cycling performance and adhesion of the secondary battery is significantly improved, ensuring excellent battery characteristics, especially reducing internal resistance at high voltages.
Smart Images

Figure BDA0004248924910000161 
Figure BDA0004248924910000241 
Figure BDA0004248924910000251
Abstract
Description
Technical Field
[0001] The present application relates to a secondary battery, and in particular to a binder composition for a secondary battery, a functional layer for a secondary battery, a component for a secondary battery, and a secondary battery, belonging to the field of new energy technology. Background Art
[0002] With the implementation of the dual-carbon policy, the development of secondary batteries will be further promoted. In the manufacturing process of batteries, the stability of the slurry is one of the important indicators of the slurry properties, which directly affects the storage time of the slurry. The more stable the slurry is, the more it can provide sufficient continuity guarantee for production. At the same time, the stability of the slurry will also have a significant impact on the coating effect. The more stable the slurry is, the more stable the coating process is, the more stable the coating surface density is, and the prepared battery performance is stable and consistent. However, taking lithium-ion batteries as an example, the positive electrode slurry of lithium secondary batteries currently generally uses polyvinylidene fluoride as a bonding material, and the bonding between the polyvinylidene fluoride molecular chain and the positive electrode active particles is unstable, which will lead to a decrease in the stability of the slurry, and then cause gel, leakage and other undesirable phenomena, which will seriously affect the battery performance. Summary of the invention
[0003] Problem that the invention aims to solve
[0004] In the above-mentioned prior art, it is difficult to fully ensure the adhesion of the electrode composite material layer, and the secondary battery cannot exert excellent cycle performance. Therefore, in the above-mentioned prior art, there is still room for improvement in terms of giving excellent adhesion to the functional layer such as the electrode composite material layer and improving the cycle performance of the secondary battery.
[0005] In view of the above, one of the objects of the present application is to provide a binder composition for a secondary battery, which has excellent binding properties and can form a functional layer that can significantly improve the cycle performance of the secondary battery.
[0006] A second object of the present application is to provide a slurry composition for a functional layer for a secondary battery, which has excellent adhesiveness and can form a functional layer that can improve the cycle performance of the secondary battery.
[0007] A third object of the present application is to provide a functional layer for a secondary battery, which has excellent adhesion and can improve the cycle performance of the secondary battery.
[0008] A fourth object of the present application is to provide a secondary battery component, which includes the secondary battery functional layer and can improve the cycle performance of the secondary battery.
[0009] A fifth object of the present application is to provide a secondary battery having excellent cycle performance.
[0010] Solutions for solving problems
[0011] The applicant has conducted in-depth research to solve the above-mentioned problems and unexpectedly discovered that an adhesive composition containing an adhesive material and epoxy phosphate in a specified amount ratio has excellent adhesion. If the adhesive composition is used to form a functional layer, the adhesion of the functional layer can be improved, and the secondary battery with the functional layer can exhibit excellent cycle performance, thereby completing the present application.
[0012] That is, the purpose of the present application is to advantageously solve the above-mentioned problems. The main feature of the binder composition for secondary batteries of the present application is that it contains a binder and an epoxy phosphate, wherein the mass ratio of the epoxy phosphate to the binder is (0.1 to 0.8): 1, that is, the content of the epoxy phosphate is greater than 10 parts by mass and less than 80 parts by mass relative to 100 parts by mass of the binder. The binder composition containing a binder and a predetermined amount of epoxy phosphate relative to the binder has excellent adhesion, so if the binder composition is used, a functional layer with excellent adhesion can be obtained. Moreover, if a battery component having the functional layer is used, the secondary battery can exhibit excellent cycle performance.
[0013] Here, in the secondary battery binder composition of the present application, the above-mentioned binder material is preferably a polymer having at least one functional group selected from carboxylic acid group, hydroxyl group, amino group, epoxy group, oxazoline group, sulfonic acid group, nitrile group and amide group. If a polymer having any of the above functional groups is used as a binder material, the adhesion of the binder composition can be further improved, and the adhesion of the functional layer and the cycle performance of the secondary battery can be further improved.
[0014] In addition, the present application aims to solve the above-mentioned problems advantageously, and the main feature of the slurry composition for secondary battery functional layer of the present application is that it contains any of the above-mentioned secondary battery binder compositions. If a functional layer is formed by any of the above-mentioned slurry compositions, the adhesion of the functional layer can be improved. Moreover, if a battery component having the functional layer is used, the secondary battery can have excellent cycle performance.
[0015] Here, the slurry composition for secondary battery functional layer of the present application may further include electrode active material particles, etc. When the slurry composition includes electrode active material particles, the slurry composition can form an electrode composite material layer having excellent adhesion and enabling the secondary battery to exhibit excellent cycle performance.
[0016] In addition, the present application aims to solve the above-mentioned problems advantageously. The main feature of the functional layer for secondary batteries of the present application is that it is formed by using any of the above-mentioned slurry compositions for functional layers for secondary batteries. The functional layer formed by any of the above-mentioned slurry compositions has excellent adhesion. Moreover, if a battery component having the functional layer is used, the secondary battery can have excellent cycle performance.
[0017] In addition, the present application aims to solve the above-mentioned problems advantageously, and the secondary battery of the present application is also characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, and at least one of the positive electrode, the negative electrode and the separator has the above-mentioned functional layer for the secondary battery. The secondary battery including the battery component having the above-mentioned functional layer has excellent battery characteristics such as cycle performance.
[0018] In addition, the present application aims to solve the above-mentioned problems advantageously, and the secondary battery of the present application is also characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, and at least one of the positive electrode, the negative electrode and the separator has the above-mentioned functional layer for the secondary battery. In particular, when the above-mentioned electrolyte includes lithium difluorophosphate, succinonitrile or 1,3,6-hexanetrinitrile, and the secondary battery containing the battery component having the above-mentioned functional layer has excellent battery characteristics such as cycle performance and internal resistance.
[0019] It should be noted that in this specification, the functional layer containing a binding material and electrode active material particles is referred to as an "electrode composite material layer", the functional layer containing a binding material and non-conductive particles is referred to as a "porous membrane layer", and the functional layer containing a binding material but not containing any of the electrode active material particles and the non-conductive particles is referred to as an "adhesive layer".
[0020] Technical Effects
[0021] According to the present application, it is possible to provide a secondary battery binder composition that has excellent binding properties and can form a functional layer that can improve the cycle performance of a secondary battery.
[0022] Furthermore, according to the present application, it is possible to provide a slurry composition for a secondary battery functional layer that has excellent adhesiveness and can form a functional layer that can improve the cycle performance of a secondary battery.
[0023] Furthermore, according to the present application, it is possible to provide a functional layer for a secondary battery that has excellent adhesiveness and can improve the cycle performance of the secondary battery.
[0024] Furthermore, according to the present application, a secondary battery having excellent cycle performance, or excellent cycle performance and internal resistance characteristics can be provided. DETAILED DESCRIPTION
[0025] The following describes the implementation of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. The present application can also be implemented or applied through other different specific implementations, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application.
[0026] Here, the binder composition for secondary batteries of the present application is used for the manufacture of secondary batteries, for example, it can be used for the preparation of the slurry composition for the functional layer of secondary batteries of the present application. Moreover, the slurry composition for the functional layer of secondary batteries of the present application can be used to form any functional layer (such as an electrode composite material layer, a porous film layer, an adhesive layer, etc.) that bears the functions of electron transfer, enhancement, or bonding in the secondary battery. Furthermore, the functional layer for secondary batteries of the present application is formed by the slurry composition for the functional layer of secondary batteries of the present application. Moreover, the secondary battery of the present application has a battery component having a functional layer for secondary batteries of the present application.
[0027] Binder composition for secondary battery
[0028] The binder composition for secondary batteries of the present application is a composition formed by dissolving and / or dispersing a binder material and epoxy phosphate in a solvent. In addition, the binder composition for secondary batteries of the present application may also contain other ingredients other than the binder material, epoxy phosphate and solvent. Here, the binder composition for secondary batteries of the present application is characterized in that it contains more than 10 parts by mass and less than 80 parts by mass of epoxy phosphate relative to 100 parts by mass of the binder material.
[0029] Moreover, the binder composition for secondary batteries of the present application is inferred to be due to the interaction between epoxy phosphate and the binding material with abundant hydrogen bonds, etc., therefore, by containing more than 10 parts by mass of epoxy phosphate relative to 100 parts by mass of the binding material, thereby showing excellent adhesion. Moreover, if the binder composition of the present application is used, the obtained functional layer for secondary batteries can exert excellent adhesion and improve the battery characteristics of the secondary battery. In addition, the binder composition for secondary batteries of the present application is less than 80 parts by mass relative to 100 parts by mass of the binding material, so that the proportion of the binding material in the solid component is guaranteed, thereby fully maintaining the adhesion of the functional layer for secondary batteries, and the conductivity of the functional layer for secondary batteries will not be excessively decreased due to the excessive amount of epoxy phosphate, and the cycle performance of the secondary battery will not be impaired. In addition, it is speculated that the properties of epoxy phosphate as a lubricant are derived from epoxy phosphate. If the electrode composite material layer as a functional layer for secondary batteries is formed using the binder composition for secondary batteries of the present application, the electrode composite material layer can be easily densified by pressurization (i.e., the compressibility of the electrode composite material layer is improved). Therefore, by using the binder composition for secondary batteries of the present application, it is possible to impart excellent adhesiveness to the functional layer for secondary batteries, and to produce a secondary battery having excellent battery characteristics such as cycle performance.
[0030] Bonding material
[0031] The bonding material is a component that exhibits bonding properties in the secondary battery binder composition of the present application, and in a secondary battery functional layer formed on a substrate using a slurry composition containing the bonding material, components such as functional particles can be kept from detaching from the functional layer, and secondary battery components can be bonded to each other via the secondary battery functional layer.
[0032] Types of bonding materials
[0033] Here, as a binder, any binder that can be used in a secondary battery is not particularly limited. For example, as a binder, a polymer (synthetic polymer, such as an addition polymer obtained by addition polymerization) obtained by polymerizing a monomer composition containing a monomer that can exhibit adhesion can be used. As such polymers, there can be cited: aliphatic conjugated diene / aromatic vinyl copolymers (polymers mainly containing aliphatic conjugated diene monomer units and aromatic vinyl monomer units, such as styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-isopentadiene copolymers, etc.), acrylic polymers (polymers mainly containing (meth) acrylic acid ester monomer units, such as polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polymethyl methacrylate, polybutyl methacrylate), fluorine polymers (polymers mainly containing fluorine-containing monomer units, such as polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluoroethylene, etc.), acrylic acid / acrylamide copolymers (polymers mainly containing (meth) acrylic acid units and (meth) acrylamide units, such as acrylic acid-acrylamide methyl propane sulfonic acid copolymers, acrylic acid-acrylamide acrylic acid hydroxyethyl copolymers, etc.), acrylonitrile polymers (polymers mainly containing (meth) acrylonitrile units, such as polyacrylonitrile, polymethacrylonitrile, etc.), etc. These can be used alone or in combination of two or more at any ratio. Among these, preferred are aliphatic conjugated diene / aromatic vinyl copolymers, acrylic acid / acrylamide copolymers, and acrylonitrile polymers. For example, preferred are styrene-butadiene copolymers, polyvinylidene fluoride, and polyacrylonitrile.
[0034] Among them, with respect to the aliphatic conjugated diene monomer that can form the aliphatic conjugated diene monomer unit in the aliphatic conjugated diene / aromatic vinyl copolymer, the aromatic vinyl monomer that can form the aromatic vinyl monomer unit in the aliphatic conjugated diene / aromatic vinyl copolymer, the (meth)acrylate monomer that can form the (meth)acrylate monomer unit in the acrylic polymer, and the fluorine-containing monomer that can form the fluorine-containing monomer unit in the fluorine-based polymer, the corresponding compounds known in the art can be used.
[0035] Epoxy Phosphate
[0036] Epoxy phosphate is a component that improves the adhesiveness of the binder composition by adding it to the binder composition containing the binder material. In addition, if an electrode composite material layer as a functional layer is prepared using a binder composition containing epoxy phosphate, the compressibility of the resulting electrode composite material layer can also be improved.
[0037] Epoxy phosphate is generally obtained by adding a phosphoric acid compound to an epoxy resin, and has a hydroxyl group and a phosphoric acid group in its molecule.
[0038] Among them, examples of epoxy resins include bisphenol epoxy resins, novolac epoxy resins, and modified epoxy resins obtained by reacting epoxy groups or hydroxyl groups in these epoxy resins with a modifier. The bisphenol epoxy resin may be any of the following resins: a resin obtained by condensing epichlorohydrin and bisphenol in the presence of a catalyst such as an alkaline catalyst to obtain a high molecular weight resin; a resin obtained by condensing epichlorohydrin and bisphenol in the presence of a catalyst such as an alkaline catalyst to obtain a low molecular weight epoxy resin, and then subjecting the low molecular weight epoxy resin to a polyaddition reaction with bisphenol. The epoxy equivalent is 172 to 4,000, preferably 175 to 1,000, to obtain epoxy phosphate with better bonding effect.
[0039] Examples of the bisphenols include bis(4-hydroxyphenyl)methane [bisphenol F], 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane [bisphenol A], 2,2-bis(4-hydroxyphenyl)butane [bisphenol B], bis(4-hydroxyphenyl)-1,1-isobutane, bis(4-hydroxy-tert-butyl-phenyl)-2,2-propane, p-(4-hydroxyphenyl)phenol, oxybis(4-hydroxyphenyl), sulfonylbis(4-hydroxyphenyl), 4,4′-dihydroxybenzophenone, and bis(2-hydroxynaphthyl)methane. The bisphenols may be used alone or as a mixture of two or more.
[0040] Examples of the novolac epoxy resin include phenol-novolak epoxy resins, cresol-novolak epoxy resins, and novolac-glyoxal epoxy resins having a plurality of epoxy groups in the molecule.
[0041] Among them, the phosphoric acid compound includes orthophosphoric acid, pyrophosphoric acid, etc. The manufacture of epoxy phosphate ester is as follows: add a phosphoric acid compound to an epoxy resin, for example, in the presence of a catalyst such as imidazoles and salts, and react at a reaction temperature of 70 to 150°C, preferably 110 to 130°C for 1 to 8 hours, preferably 3 to 6 hours, so that the epoxy phosphate ester compound obtained has better adhesion. It should be noted that the H+ of the phosphoric acid compound preferably reacts with 1 mol of ethylene oxide groups of the epoxy resin in the range of H+ / ethylene oxide = 0.5 to 3, preferably 1 to 3.
[0042] The acid value of the epoxy phosphate thus obtained is in the range of 5 to 70 mgKOH / g, preferably 28 to 60 mgKOH / g, more preferably 35 to 57 mgKOH / g, which is preferred from the viewpoint of water-resistant adhesion and substrate adhesion.
[0043] Examples of commercially available epoxy phosphates include RKZ3008 from RKZ3032 from RKZ, ETERKYD 4901-B-72 from Changxing Chemical, Qingdao Shengshi 801 Phosphate, Guangdong Lisheng 6063A, and Suzhou Qingtian DH-7526. The epoxy phosphates may be used alone or in combination of two or more at any ratio.
[0044] Moreover, the content of the epoxy phosphate in the binder composition needs to be more than 10 parts by mass and less than 80 parts by mass relative to 100 parts by mass of the bonding material, preferably more than 12 parts by mass, more preferably more than 15 parts by mass, further preferably more than 20 parts by mass, particularly preferably more than 30 parts by mass, preferably less than 80 parts by mass, more preferably less than 60 parts by mass, and further preferably less than 50 parts by mass. When the content of the epoxy phosphate is less than 10 parts by mass relative to 100 parts by mass of the bonding material, the adhesion of the functional layer cannot be guaranteed. When the content of the epoxy phosphate is selected to be more than 30 parts and less than 50 parts, the interaction between the epoxy phosphate and the bonding material is more sufficient, further improving the adhesion. On the other hand, when the content of the epoxy phosphate exceeds 80 parts by mass relative to 100 parts by mass of the bonding material, the adhesion of the functional layer decreases, and the conductivity of the functional layer is impaired, and the cycle performance of the secondary battery decreases. Furthermore, when the content of the epoxy phosphate is 10 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the binder, the compressibility of the electrode composite material layer formed from the slurry composition containing the binder composition can be improved.
[0045] Solvents
[0046] The solvent contained in the adhesive composition is not particularly limited as long as it can dissolve or disperse the above-mentioned adhesive material and epoxy phosphate, and any one of water and organic solvents can be used. As the organic solvent, for example, acetonitrile, N-methyl-2-pyrrolidone, tetrahydrofuran, acetone, acetylpyridine, cyclopentanone, dimethylformamide, dimethyl sulfoxide, methylformamide, methyl ethyl ketone, furfural, ethylenediamine, dimethylbenzene (xylene), methylbenzene (toluene), cyclopentyl methyl ether and isopropyl alcohol can be used.
[0047] These solvents may be used alone or in combination of two or more at any mixing ratio.
[0048] Other ingredients
[0049] In addition to the above-mentioned adhesive material, epoxy phosphate and solvent, the adhesive composition of the present application may also arbitrarily contain other polymers, conductive materials, wetting agents, viscosity regulators, electrolyte additives, etc. that are different from the composition and properties of the above-mentioned adhesive material and can be added to functional layers such as electrode composite material layers, porous membrane layers and adhesive layers. Known additives.
[0050] Method for preparing adhesive composition
[0051] Here, the adhesive composition is prepared by a method without particular limitation, and is generally prepared by mixing an adhesive material, epoxy phosphate, and other components that may be used as required in a solvent. The mixing method is not particularly limited, and mixing is performed using a common stirrer or disperser.
[0052] Slurry composition for functional layer of secondary battery
[0053] The slurry composition of the present application is a composition for forming a functional layer, comprising the above-mentioned binder composition, and then arbitrarily containing functional particles and other components. That is, the slurry composition of the present application usually contains a bonding material, epoxy phosphate and a solvent, and then arbitrarily contains functional particles and other components. Moreover, the slurry composition of the present application is owing to comprising the above-mentioned binder composition, so by drying the slurry composition of the present application on, for example, a substrate, so as to obtain a functional layer with excellent adhesion. Moreover, if a battery component with the functional layer is used, the secondary battery can be made to exert excellent battery characteristics, especially excellent cycle performance.
[0054] Binder composition
[0055] As the adhesive composition, the adhesive composition of the present application described above containing at least an adhesive material and epoxy phosphate is used.
[0056] In addition, the amount of the binder composition in the slurry composition is not particularly limited. For example, when the slurry composition is a slurry composition for an electrode, the amount of the binder composition can be set to an amount of 0.5 parts by mass or more and 15 parts by mass or less of the amount of the binder material relative to 100 parts by mass of the electrode active material particles in terms of solid content conversion, that is, in terms of solid content conversion, the mass ratio of the binder composition to the electrode active material particles is (0.5 to 15): 100, which can further improve the compressibility of the electrode composite material layer.
[0057] In addition, in the case where the slurry composition is a slurry composition for a porous membrane layer, the amount of the binder composition can be set to an amount of 0.5 parts by mass or more and 30 parts by mass or less of the binder material calculated on a solid content basis relative to 100 parts by mass of the non-conductive particles, that is, when the mass ratio of the binder composition to the non-conductive particles is (0.5 to 30):100 calculated on a solid content basis, the insulation or support properties of the porous membrane layer can be improved.
[0058] Functional particles
[0059] Here, examples of functional particles for enabling the functional layer to exert a desired function include electrode active material particles when the functional layer is an electrode composite material layer, and non-conductive particles when the functional layer is a porous membrane layer.
[0060] Electrode active material particles
[0061] Moreover, the electrode active material particles are not particularly limited, and particles formed by known electrode active materials that can be used in secondary batteries can be cited. Specifically, for example, the electrode active material particles that can be used in the electrode composite material layer of a lithium ion battery as an example of a secondary battery are not particularly limited, and particles formed by electrode active materials such as the following positive electrode active materials and negative electrode active materials can be used.
[0062] Positive active material
[0063] As the positive electrode active material matched with the positive electrode composite material layer of the positive electrode of the lithium ion battery, for example, a compound containing a transition metal can be used, such as a transition metal oxide, a transition metal sulfide, a composite metal oxide of lithium and a transition metal, etc. Among them, as the transition metal, for example, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, etc. can be listed.
[0064] Specifically, as the positive electrode active material, there is no particular limitation, and examples thereof include lithium cobalt oxide (LiCoO2), lithium manganate (LiMn2O4), lithium nickel oxide (LiNiO2), Co-Ni-Mn lithium-containing composite oxides, Ni-Mn-Al lithium-containing composite oxides, Ni-Co-Al lithium-containing composite oxides, olivine lithium iron phosphate (LiFePO4), olivine lithium manganese phosphate (LiMnPO4), Li 1+x Mn 2-x O4 (0<X<2) represented by lithium-excess spinel compounds, Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O2、LiNi 0.5 Mn 1.5O4, etc.
[0065] The above-mentioned positive electrode active materials may be used alone or in combination of two or more.
[0066] Negative active material
[0067] Examples of the negative electrode active material to be blended in the negative electrode composite material layer of the negative electrode of the lithium ion battery include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials in combination thereof.
[0068] Here, the carbon-based negative electrode active material refers to an active material with carbon as the main skeleton that can embed lithium. In addition, as the carbon-based negative electrode active material, specific examples include: carbonaceous materials such as coke, mesoporous carbon microspheres (MCMB), mesophase pitch carbon fibers, pyrolysis vapor-grown carbon fibers, phenolic resin sintered bodies, polyacrylonitrile carbon fibers, quasi-isotropic carbon, furfuryl alcohol resin sintered bodies (PFA) and hard carbon, and graphite materials such as natural graphite and artificial graphite.
[0069] In addition, the metal-based negative electrode active material is an active material containing a metal, generally referring to an active material containing an element capable of embedding lithium in the structure, and having a theoretical capacity of 500 mAh / g or more per unit mass when lithium is embedded. Moreover, as metal-based active materials, for example, lithium metal, single metals capable of forming lithium alloys (such as Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.) and their oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. can be cited. Furthermore, oxides such as lithium titanate can also be cited.
[0070] The above-mentioned negative electrode active materials may be used alone or in combination of two or more.
[0071] Non-conductive particles
[0072] The non-conductive particles to be blended in the porous membrane layer are not particularly limited, and examples thereof include known non-conductive particles that can be used in secondary batteries.
[0073] Specifically, as non-conductive particles, both inorganic particles and organic particles can be used, and inorganic particles are usually used. Among them, as the material of non-conductive particles, it is preferred that the material is stably present and electrochemically stable under the use environment of the secondary battery. When the preferred examples of materials for non-conductive particles are listed from this point of view, oxide particles such as aluminum oxide (alumina), hydrated aluminum oxide (boehmite), silicon oxide, magnesium oxide (magnesia), calcium oxide, titanium oxide (Titania), BaTiO3, ZrO, aluminum oxide / silicon dioxide composite oxides, etc.; nitride particles such as aluminum nitride and boron nitride; covalently bonded crystal particles such as silicon and diamond; insoluble ionic crystal particles such as barium sulfate, calcium fluoride, and barium fluoride; clay particles such as talc and montmorillonite, etc. In addition, element replacement, surface treatment, solid solution, etc. can be implemented on these particles as needed.
[0074] In addition, the above-mentioned non-conductive particles may be used alone or in combination of two or more.
[0075] Preparation of slurry composition
[0076] The method for preparing the slurry composition is not particularly limited.
[0077] For example, when the slurry composition is a slurry composition for an electrode, the slurry composition can be prepared by mixing a binder composition, electrode active material particles, and other components used as necessary in the presence of a solvent.
[0078] When the slurry composition is a slurry composition for a porous membrane layer, the slurry composition can be prepared by mixing a binder composition, non-conductive particles, and other components used as necessary in the presence of a solvent.
[0079] When the slurry composition is a slurry composition for an adhesive layer, the binder composition may be used as the slurry composition directly or after being diluted with a solvent, or the binder composition and other components used as needed may be mixed in the presence of a solvent to prepare the slurry composition.
[0080] The solvent used in preparing the slurry composition also includes the solvent contained in the binder composition. The mixing method is not particularly limited, and for example, a common stirrer or disperser may be used for mixing.
[0081] Functional layer for secondary batteries
[0082] The functional layer of the present application is a layer that bears the functions of electron transfer, enhancement, or bonding in a secondary battery. As a functional layer, for example, an electrode composite material layer that performs electron transfer through an electrochemical reaction, a porous film layer that improves heat resistance and / or strength, an adhesive layer that improves adhesion, etc. can be cited. Moreover, the functional layer of the present application is formed by the above-mentioned slurry composition of the present application, and can be formed by, for example, the following manner, that is, after the above-mentioned slurry composition is applied to a suitable substrate surface to form a coating, the formed coating is dried, thereby forming. That is, the functional layer of the present application is formed by the dried product of the above-mentioned slurry composition, usually containing at least a bonding material and epoxy phosphate. In addition, since the components included in the functional layer are the components included in the above-mentioned slurry composition, the preferred existence ratio of these components is the same as the preferred existence ratio of the components in the slurry composition.
[0083] Since the functional layer of the present application is formed by the slurry composition of the present application containing the binder composition of the present application, it has excellent adhesion and can also enable the secondary battery having the battery component with the functional layer of the present application to exhibit excellent battery characteristics (cycle performance, etc.).
[0084] Substrate
[0085] Here, the substrate to which the slurry composition is applied is not limited. For example, a coating film of the slurry composition can be formed on the surface of a release substrate, the coating film can be dried to form a functional layer, and the release substrate can be peeled off from the functional layer. The functional layer peeled off from the release substrate can also be used as a self-supporting film to form a battery component of a secondary battery.
[0086] However, from the viewpoint of omitting the process of stripping the functional layer and improving the manufacturing efficiency of the battery component, as the substrate, it is preferred to use a current collector, a diaphragm substrate, or an electrode substrate. Specifically, when preparing the electrode composite material layer, the slurry composition is preferably applied to the current collector as the substrate. In addition, when preparing the porous film layer and the bonding layer, the slurry composition is preferably applied to the diaphragm substrate or the electrode substrate.
[0087] current collector
[0088] As the current collector, a material having conductivity and electrochemical durability can be used. Specifically, as the current collector, for example, a current collector comprising iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. Among them, as the current collector used in the negative electrode, copper foil is particularly preferred. In addition, as the current collector used in the positive electrode, aluminum foil is particularly preferred. In addition, the above-mentioned materials can be used alone, or two or more can be used in combination in any ratio.
[0089] Diaphragm substrate
[0090] As the diaphragm substrate, there is no particular limitation, and known diaphragm substrates such as organic diaphragm substrates can be cited. The organic diaphragm substrate is a porous member formed by an organic material. When the example of the organic diaphragm substrate is cited, microporous membranes or nonwoven fabrics containing polyolefin resins such as polyethylene and polypropylene, aromatic polyamide resins, etc. can be cited. From the aspect of excellent strength, microporous membranes, nonwoven fabrics, etc. made of polyethylene are preferred.
[0091] Electrode substrate
[0092] The electrode substrate (positive electrode substrate and negative electrode substrate) is not particularly limited, and examples thereof include an electrode substrate in which an electrode composite material layer including electrode active material particles and a binder is formed on the above-mentioned current collector.
[0093] The electrode active material particles and the binding material contained in the electrode composite material layer in the electrode substrate are not particularly limited, and the electrode active material particles described in the "Slurry composition for functional layer for secondary battery" project and the binding material described in the "Binder composition for secondary battery" project can be used. In addition, the electrode composite material layer in the electrode substrate may also contain epoxy phosphate. That is, as the electrode composite material layer in the electrode substrate, the functional layer of the present application can be used.
[0094] Method for forming functional layer
[0095] Examples of a method for forming a functional layer on a substrate such as the above-mentioned current collector, separator substrate, electrode substrate, etc. include the following methods.
[0096] 1) A method of applying the slurry composition of the present application to the surface of a substrate and then drying it;
[0097] Alternatively, 2) a method of immersing a substrate in the slurry composition of the present application and drying the slurry composition;
[0098] Alternatively, 3) a method in which the slurry composition of the present application is applied on a release substrate, dried to produce a functional layer, and the obtained functional layer is transferred to the surface of the substrate.
[0099] Among these methods, the method 1) is particularly preferred because the thickness of the functional layer can be easily controlled. The method 1) includes, in detail, a step of applying the slurry composition to a substrate (coating step) and a step of drying the slurry composition applied to the substrate to form a functional layer (drying step).
[0100] Coating process
[0101] In the coating step, the method for coating the slurry composition on the substrate is not particularly limited, and examples thereof include a doctor blade method, a reverse roll method, a direct roll method, a gravure printing method, an extrusion method, and a brush coating method.
[0102] Drying process
[0103] In addition, in the drying process, the method for drying the slurry composition on the substrate is not particularly limited, and a known method can be used. Examples of drying methods include drying using warm air, hot air, and low-humidity air; vacuum drying; and drying using irradiation with infrared rays, ultraviolet rays, and the like. In order to avoid the problem of thermal decomposition of the epoxy phosphate used, the drying temperature is preferably lower than 200°C, more preferably lower than 150°C, preferably higher than 50°C, and more preferably higher than 80°C.
[0104] In addition, in the case of preparing an electrode composite material layer as a functional layer, preferably after the drying process, the electrode composite material layer is subjected to pressure treatment using mold pressing or roll pressing. The electrode composite material layer as the functional layer of the present application has excellent compressibility because it contains epoxy phosphate in a specified amount. Therefore, by pressure treatment, it is possible to easily prepare an electrode composite material layer with high density and excellent adhesion to the current collector.
[0105] Battery component with functional layer
[0106] The battery components (diaphragms and electrodes) with functional layers of the present application may have structural elements other than the functional layers and substrates of the present application as long as they do not significantly affect the effects of the present application. Such structural elements are not particularly limited, and examples thereof include electrode composite material layers, porous membrane layers, and adhesive layers that do not belong to the functional layers of the present application.
[0107] In addition, the battery component may have a variety of functional layers of the present application. For example, the electrode may have an electrode composite material layer formed by the electrode slurry composition of the present application on the current collector, and on the electrode composite material layer, there is a porous film layer and / or bonding layer formed by the porous film layer and / or bonding layer slurry composition of the present application. In addition, for example, the diaphragm may have a porous film layer formed by the porous film layer slurry composition of the present application on the diaphragm substrate, and on the porous film layer, there is a bonding layer formed by the bonding layer slurry composition of the present application.
[0108] The battery member having the functional layer of the present application can be well bonded to an adjacent battery member and can also exhibit excellent battery characteristics of a secondary battery, such as excellent cycle performance.
[0109] Secondary battery
[0110] The secondary battery of the present application has the above-mentioned functional layer of the present application. More specifically, the secondary battery of the present application has a positive electrode, a negative electrode, a separator, and an electrolyte, and the above-mentioned functional layer for the secondary battery is included in at least one of the positive electrode, the negative electrode, and the separator as a battery component. Moreover, the secondary battery of the present application can exert excellent battery characteristics (such as cycle performance).
[0111] Positive electrode, negative electrode and separator
[0112] At least one of the positive electrode, negative electrode and separator used in the secondary battery of the present application is a battery component having the above-mentioned functional layer of the present application. In addition, the positive electrode, negative electrode and separator not having the functional layer of the present application are not particularly limited, and known positive electrodes, negative electrodes and separators can be used.
[0113] Electrolyte
[0114] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent is generally used. As a supporting electrolyte, a lithium salt is used in, for example, a lithium ion battery. As a lithium salt, for example: LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, because they are easily soluble in solvents and show a high degree of dissociation, LiPF6, LiClO4, and CF3SO3Li are preferred. In addition, the electrolyte can be used alone or in combination of two or more. Generally, the more a supporting electrolyte with a high degree of dissociation is used, the more the lithium ion conductivity tends to increase, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0115] As the organic solvent used in the electrolyte, there is no particular limitation as long as it can dissolve the supporting electrolyte. For example, in lithium ion batteries, it is preferred to use: carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC); esters such as γ-butyrolactone, methyl formate, ethyl acetate, ethyl propionate, and propyl propionate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, carbonates or carboxylates are preferred because of their high dielectric constant and wide stable potential region. Generally, the lower the viscosity of the solvent used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of solvent.
[0116] It should be noted that the concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. In addition, known additives may be added to the electrolytic solution.
[0117] In addition, the applicant unexpectedly discovered that when the electrolyte contains lithium difluorophosphate, succinonitrile or 1,3,6-hexanetrinitrile, the decomposition of epoxy phosphate at high voltage can be inhibited, thereby further improving the cycle performance of the secondary battery at high voltage and reducing the internal resistance.
[0118] The above-mentioned lithium difluorophosphate, succinonitrile or 1,3,6-hexanetricarbonitrile may be used alone or in combination of two or more.
[0119] The content of the above-mentioned lithium difluorophosphate (LiPO 2 F 2 ), succinonitrile (SN) or 1,3,6-hexanetricarbonitrile (HTCN) can be set to, for example, 8 parts by mass or less or 5 parts by mass or less, respectively, relative to 100 parts by mass of the electrolyte solution.
[0120] In some cases, the electrolyte may also be replaced by a gel electrolyte, a solid electrolyte, etc. These gel electrolytes and solid electrolytes may contain the aforementioned lithium salt and other additive components commonly used in the art.
[0121] In some cases, the secondary battery may also be a sodium ion battery, etc., and accordingly, the electrolyte may include sodium salt, etc.
[0122] Method for manufacturing secondary battery
[0123] The secondary battery of the present application can be manufactured by, for example, overlapping the positive electrode and the negative electrode via a diaphragm, winding and folding them as needed and placing them in a battery container, and injecting an electrolyte into the battery container for sealing. In addition, at least one of the positive electrode, the negative electrode, and the diaphragm is set as a battery component having a functional layer of the present application. In addition, metal mesh, fuse, PTC element and other anti-overcurrent elements, guide plates, etc. can be placed in the battery container as needed to prevent the internal pressure of the battery from rising and overcharging and discharging. The shape of the battery can be any shape such as a coin, button, sheet, cylindrical, square, flat, etc.
[0124] Example
[0125] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In addition, in the following description, "%" and "part" indicating the amount are based on mass unless otherwise specified.
[0126] In the following examples and comparative examples, the adhesiveness of the functional layer, the compressibility of the electrode composite material layer, and the cycle performance of the secondary battery were evaluated according to the following methods.
[0127] Bonding of functional layers
[0128] Adhesion of negative electrode composite material layer as functional layer
[0129] The negative electrode of the lithium ion battery produced is cut into a rectangle of 100mm in length and 10mm in width to make a test piece, with one side with the negative electrode composite material layer downward, the negative electrode composite material layer surface of the test piece is affixed to a test bench (SUS substrate) by a scotch tape (defined in J1SZ1522). Afterwards, one end of the current collector is stretched in the vertical direction at a tensile speed of 50mm / min and it is peeled off, and the stress (N / m) during peeling is measured (in addition, the scotch tape is fixed on the test bench). Carry out the same test as above 3 times, obtain its average value as peel strength, and evaluate according to the following benchmark. The larger the value of peel strength, the more firmly the negative electrode composite material layer and the current collector are in close contact, and the more excellent the adhesion of the negative electrode composite material layer.
[0130] A: Peel strength is 30N / m or more
[0131] B: Peel strength is 20 N / m or more and less than 30 N / m
[0132] C: Peel strength is 10 N / m or more and less than 20 N / m
[0133] D: Peel strength less than 10N / m
[0134] Adhesion of the positive electrode composite material layer as a functional layer
[0135] The positive electrode of the lithium ion battery produced is cut into a rectangle of 100mm in length and 10mm in width and made into a test piece, with one side with a positive electrode composite material layer downward, the positive electrode composite material layer surface of the test piece is affixed to a test bench (SUS substrate) by a scotch tape (defined in J1SZ1522). Afterwards, one end of the current collector is stretched in a vertical direction at a tensile speed of 50mm / min and it is peeled off, and the stress (N / m) during peeling is measured (in addition, the scotch tape is fixed on the test bench). Carry out 3 times of the same test as above, obtain its average value as peel strength, and evaluate according to the following benchmark. The larger the value of peel strength, the more firmly the positive electrode composite material layer and the current collector are in close contact, and the more excellent the adhesion of the positive electrode composite material layer.
[0136] A: Peel strength is 80N / m or more
[0137] B: Peel strength is 60 N / m or more and less than 80 N / m
[0138] C: Peel strength is 40 N / m or more and less than 60 N / m
[0139] D: Peel strength less than 40N / m
[0140] Adhesion of porous membrane layer as functional layer
[0141] The diaphragm with porous film layer made is cut into a rectangle of 100mm in length and 10mm in width and is made into test piece, with one side with porous film layer downward, the porous film layer surface of test piece is affixed on test bench (SUS substrate) by transparent tape (defined by JIS Z1522).Afterwards, one end of the diaphragm substrate is stretched with a tensile speed of 50mm / min in the vertical direction and it is peeled off, and the stress (N / m) (in addition, transparent tape is fixed on the test bench) during peeling is measured. Carry out 3 times of above-mentioned same tests, obtain its mean value as peel strength, evaluate according to the following benchmark.The value of peel strength is larger, represents that porous film layer and diaphragm substrate are more firmly close, and the adhesion of porous film layer is more excellent.
[0142] A: Peel strength is 50N / m or more
[0143] B: Peel strength is 40 N / m or more and less than 50 N / m
[0144] C: Peel strength is 30 N / m or more and less than 40 N / m
[0145] D: Peel strength less than 30N / m
[0146] Compressibility of electrode composite layers
[0147] Compressibility of negative electrode composite material layer
[0148] The negative electrode composite material layer side of the prepared negative electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 50 t (tons) to obtain a negative electrode composite material layer with a density of 1.80 g / cm 3 The negative electrode was then placed in an environment with a temperature of 25±3°C and a relative humidity of 50±5% for one week. The density of the negative electrode composite material layer (g / cm 3 ), and the evaluation was performed according to the following criteria. The higher the density of the negative electrode composite material layer after being placed, the less likely the negative electrode composite material layer will rebound, and the better the compressibility of the negative electrode composite material layer.
[0149] A: The density of the negative electrode composite material layer after placement is 1.70g / cm 3 above
[0150] B: The density of the negative electrode composite material layer after placement is 1.60g / cm 3 Above and less than 1.70g / cm 3
[0151] C: The density of the negative electrode composite material layer after placement is 1.50 g / cm 3Above and less than 1.60g / cm 3
[0152] D: The density of the negative electrode composite material layer after placement is less than 1.50g / cm 3
[0153] Compressibility of positive electrode composite material layer
[0154] The positive electrode composite material layer side of the prepared positive electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 70 t (tons) to obtain a positive electrode composite material layer with a density of 4.30 g / cm 3 The positive electrode was then placed in an environment with a temperature of 25±3°C and a relative humidity of 50±5% for one week. The density of the positive electrode composite material layer (g / cm 3 ), and the evaluation was performed according to the following criteria. The higher the density of the positive electrode composite material layer after being placed, the less likely the positive electrode composite material layer will rebound, and the better the compressibility of the positive electrode composite material layer.
[0155] A: The density of the positive electrode composite material layer after placement is 4.20g / cm 3 above
[0156] B: The density of the positive electrode composite material layer after placement is 4.10 g / cm 3 Above and less than 4.20g / cm 3
[0157] C: The density of the positive electrode composite material layer after placement is 4.00 g / cm 3 Above and less than 4.10g / cm 3
[0158] D: The density of the positive electrode composite material layer after placement is less than 4.00g / cm 3
[0159] Cycle characteristics of secondary batteries
[0160] The lithium ion batteries prepared in the examples and comparative examples were left to stand at 25°C for 5 hours. Then, they were charged at 25°C by a constant current method at 0.2C until the battery cell voltage was 3.85V, and then aged at 60°C for 12 hours. Then, they were discharged at 25°C by a constant current method at 0.2C until the battery cell voltage was 3.00V. Then, CC-CV charging was performed at a constant current method at 0.2C (upper limit battery cell voltage 4.60V), and CC discharge was performed at a constant current method at 0.2C until the battery cell voltage was 3.00V. This 0.2C charge and discharge was repeated 3 times.
[0161] Then, 100 cycles of charge and discharge were performed at a temperature of 10° C., a cell voltage of 4.60-3.00 V, and a charge and discharge rate of 1.0 C. At this time, the discharge capacity of the first cycle was defined as X1, and the discharge capacity of the 100th cycle was defined as X2.
[0162] Then, the capacity retention rate ΔC′=(X2 / X1)×100(%) was calculated using the discharge capacity X1 and the discharge capacity X2, and the evaluation was performed according to the following criteria: The larger the value of the capacity retention rate ΔC′, the better the cycle characteristics of the secondary battery.
[0163] A: Capacity retention rate ΔC′ is 95% or more
[0164] B: Capacity retention rate ΔC′ is 90% or more and less than 95%
[0165] C: Capacity retention rate ΔC′ is 85% or more and less than 90%
[0166] D: Capacity retention rate ΔC′ is 80% or more and less than 85%
[0167] E: Capacity retention rate ΔC′ is 80% or less
[0168] Internal resistance characteristics of secondary batteries
[0169] The lithium ion batteries prepared in the examples and comparative examples were charged at 10°C at 1C (C is a numerical value expressed as rated capacity (mA) / 1h (hour)) to 50% of the SOC (State Of Charge), and then charged and discharged for 15 seconds at 0.5C, 1.0C, 1.5C, and 2.0C, respectively, with 50% of the SOC as the center. The battery voltage after 10 seconds in each case (charging side and discharging side) was plotted against the current value, and the slope was divided by the area of the positive electrode of the prepared lithium ion battery. The obtained value was calculated as the IV resistance (Ω·cm2) (IV resistance during charging and IV resistance during discharging). For the value of the IV resistance (Ω·cm2) obtained 2 ), and evaluated according to the following criteria. The smaller the IV resistance value, the lower the internal resistance (the lower the DC resistance), and the better the internal resistance characteristics.
[0170] A: IV resistance is 22Ω·cm 2 the following
[0171] B: IV resistance greater than 22Ω·cm 2 and 25Ω·cm 2 the following
[0172] C: IV resistance greater than 25Ω·cm 2 and 28Ω·cm2 the following
[0173] D: IV resistance greater than 28Ω·cm 2
[0174] The bonding materials and epoxy phosphates used in the following examples are all commercially available, and their specific names and abbreviations are shown in Table 1 below.
[0175] Table 1 Sources of bonding materials and epoxy phosphates in the examples of this application
[0176]
[0177] Example 1
[0178] Preparation of binder composition for negative electrode composite material layer
[0179] 15 parts of epoxy phosphate P01 were mixed with 100 parts (in terms of solid content) of an aqueous dispersion of a styrene-butadiene copolymer (SBR) to prepare an adhesive composition.
[0180] Preparation of slurry composition for negative electrode composite material layer
[0181] In a double planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360mAh / g) as a negative electrode active material, 48.75 parts of natural graphite (theoretical capacity: 360mAh / g), and 1 part of carboxymethyl cellulose as a thickener were added in terms of solid content. The solid content concentration was further diluted to 60% using ion exchange water, and then stirred at a speed of 45rpm for 60 minutes. After that, 1.5 parts of the above-obtained binder composition for the negative electrode composite material layer were added in terms of solid content, and stirred at a speed of 40rpm for 40 minutes. After that, ion exchange water was added to make the viscosity 4000±500mPa·s (B-type viscometer, measured at 25°C and 60rpm), and a slurry composition for the negative electrode composite material layer was prepared.
[0182] Negative electrode manufacturing
[0183] The negative electrode composite material layer slurry composition was applied in an amount of 11±0.5 mg / cm 2 The copper foil with the negative electrode composite material layer was then conveyed in an oven at 80°C for 2 minutes at a speed of 400 mm / min, and then in an oven at 110°C for 2 minutes to dry the slurry composition on the copper foil, thereby obtaining a negative electrode raw material for forming a negative electrode composite material layer on the current collector. The compressibility of the negative electrode composite material layer was evaluated using the negative electrode raw material. The results are shown in Table 2.
[0184] Afterwards, the negative electrode composite material layer side of the prepared negative electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 50 t (tons) to obtain a negative electrode composite material layer with a density of 1.70 g / cm 3 The negative electrode was then placed in an environment of 25±3°C and 50±5% relative humidity for 1 week. The negative electrode after placement was used to evaluate the adhesion of the negative electrode composite material layer. The results are shown in Table 2.
[0185] Cathode Manufacturing
[0186] In a double planetary mixer, 96 parts of lithium cobalt oxide as a positive electrode active material, 2 parts of acetylene black as a conductive material, and 2 parts of polyvinylidene fluoride as a binding material were added. After the above powders were mixed and stirred for 10 minutes, N-methyl-2-pyrrolidone (NMP) as a dispersion medium was added to make the total solid content concentration become 70% and mixed to prepare a slurry composition for a positive electrode composite material layer.
[0187] Then, the obtained slurry composition for positive electrode composite material layer was applied in an amount of 20±0.5 mg / cm 2 It was coated on a 9 μm thick aluminum foil as the current collector.
[0188] Furthermore, the slurry composition on the aluminum foil was dried by conveying it in an oven at 90°C for 2 minutes at a speed of 200 mm / min and in an oven at 120°C for 2 minutes to obtain a positive electrode raw material having a positive electrode composite material layer formed on the current collector.
[0189] After that, the positive electrode composite material layer side of the prepared positive electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 70t (tons) to obtain a positive electrode with a positive electrode composite material layer density of 4.20g / cm3. The positive electrode was then placed in an environment of a temperature of 25±3°C and a relative humidity of 50±5% for 1 week.
[0190] Preparation of the diaphragm
[0191] As the separator, 7 μm polyethylene (Xingyuan Material) was used.
[0192] Lithium-ion battery manufacturing
[0193] Using the above-mentioned negative electrode, positive electrode and separator, a wound battery cell is prepared and placed in an aluminum-plastic film packaging material. Afterwards, a 12.5% LiPF6 solution as an electrolyte is filled into the packaging material [Solvent: ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC) / propyl propionate (PP) / =1 / 1 / 1 / 2 (mass ratio) mixed solvent, additive: containing 4% by mass of fluoroethylene carbonate]. Then, a heat seal at a temperature of 150°C is performed to seal the packaging material to manufacture a lithium-ion battery. The cycle performance is evaluated using the lithium-ion battery, and the results are shown in Table 2.
[0194] Example 2
[0195] When preparing the binder composition for the negative electrode composite material layer, the amount of P01 was changed to 30 parts, and the same method as in Example 1 was used to manufacture styrene-butadiene copolymer (SBR) as a binder, a binder composition for the negative electrode composite material layer, a slurry composition for the negative electrode composite material layer, a negative electrode, a positive electrode, a separator, and a lithium ion battery. Afterwards, the evaluation was performed in the same manner as in Example 1, and the results are shown in Table 2.
[0196] Example 3
[0197] When preparing the binder composition for the negative electrode composite material layer, P02 was used instead of P01. Otherwise, the same method as in Example 2 was used to manufacture styrene-butadiene copolymer (SBR) as a binder, a binder composition for the negative electrode composite material layer, a slurry composition for the negative electrode composite material layer, a negative electrode, a positive electrode, a separator and a lithium ion battery. Afterwards, the evaluation was performed in the same manner as in Example 1, and the results are shown in Table 2.
[0198] Example 4
[0199] When preparing the binder composition for negative electrode composite material layer, 75 parts of PO3 were used instead of 15 parts of PO1. In addition, the same method as in Example 1 was used to manufacture styrene-butadiene copolymer (SBR) as a binding material, a binder composition for negative electrode composite material layer, a slurry composition for negative electrode composite material layer, a negative electrode, a positive electrode, a separator and a lithium ion battery. Afterwards, the same method as in Example 1 was used to evaluate, and the results are shown in Table 2.
[0200] Example 5
[0201] When preparing the binder composition for the negative electrode composite material layer, P01 was used instead of P03. Otherwise, the same method as in Example 4 was used to manufacture styrene-butadiene copolymer (SBR) as a binder, a binder composition for the negative electrode composite material layer, a slurry composition for the negative electrode composite material layer, a negative electrode, a positive electrode, a separator and a lithium ion battery. Afterwards, the same method as in Example 1 was used to evaluate, and the results are shown in Table 2.
[0202] Example 6
[0203] Preparation of binder composition for negative electrode composite material layer
[0204] 30 parts of P01 were mixed with 100 parts (in terms of solid content) of an aqueous dispersion of an acrylic acid / acrylamide copolymer (AA / AAm) to prepare an adhesive composition.
[0205] Preparation of slurry composition for negative electrode composite material layer
[0206] Add 48.75 parts of artificial graphite (theoretical capacity: 360mAh / g) and 48.75 parts of natural graphite (theoretical capacity: 360mAh / g) as negative electrode active materials to a double planetary mixer. Further dilute the solid content concentration to 60% with ion exchange water, and then stir at a speed of 45rpm for 60 minutes. Then add 1.5 parts of the above-obtained binder composition for the negative electrode composite material layer in terms of solid content equivalent, and stir at a speed of 40rpm for 40 minutes. Then add ion exchange water to make the viscosity 4000±500mPa·s (B-type viscometer, measured at 25°C, 60rpm), and prepare a slurry composition for the negative electrode composite material layer.
[0207] Negative electrode manufacturing
[0208] The negative electrode raw material and the negative electrode were obtained in the same manner as in Example 1 except that the above-mentioned slurry composition for the negative electrode composite material layer was used. The compressibility of the negative electrode composite material layer was evaluated using the obtained negative electrode raw material, and the adhesion of the negative electrode composite material layer was evaluated using the obtained negative electrode. The results are shown in Table 2.
[0209] Manufacturing of positive electrodes, separators, and lithium-ion batteries
[0210] A positive electrode, a separator, and a lithium ion battery were produced in the same manner as in Example 1 except that the negative electrode obtained above was used. The cycle performance was evaluated using the obtained lithium ion battery. The results are shown in Table 2.
[0211] Example 7
[0212] Preparation of binder composition for negative electrode composite material layer
[0213] 30 parts of P01 were mixed with 100 parts (in terms of solid content) of an aqueous emulsion of polyvinylidene fluoride (PVDF) to prepare an adhesive composition.
[0214] Preparation of slurry composition for negative electrode composite material layer
[0215] 48.75 parts of artificial graphite (theoretical capacity: 360mAh / g) as the negative electrode active material and 48.75 parts of natural graphite (theoretical capacity: 360mAh / g) were added with 2.5 parts of the above-mentioned negative electrode composite material layer binder composition in terms of solid content, and the solid content concentration was further diluted to 50% with water, and stirred at 3000rpm for 1 hour with a disperser. NMP was then added to make the viscosity 4000±500mPa·s (B-type viscometer, measured at 25°C, 60rpm), and a slurry composition for a negative electrode composite material layer was prepared.
[0216] Negative electrode manufacturing
[0217] The negative electrode composite material layer slurry composition was applied in an amount of 11±0.5 mg / cm 2 The copper foil coated with the negative electrode composite material layer slurry composition was then transported in an oven at 90°C for 2 minutes at a speed of 200 mm / min, and then in an oven at 120°C for 2 minutes to dry the slurry composition on the copper foil, thereby obtaining a negative electrode raw material for forming a negative electrode composite material layer on the current collector. The compressibility of the negative electrode composite material layer was evaluated using the negative electrode raw material. The results are shown in Table 2.
[0218] Afterwards, the negative electrode composite material layer side of the prepared negative electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 50 t (tons) to obtain a negative electrode composite material layer with a density of 1.70 g / cm 3 The negative electrode was then placed in an environment of 25±3°C and 50±5% relative humidity for 1 week. The negative electrode after placement was used to evaluate the adhesion of the negative electrode composite material layer. The results are shown in Table 2.
[0219] Manufacturing of positive electrodes, separators, and lithium-ion batteries
[0220] A positive electrode, a separator, and a secondary battery were produced in the same manner as in Example 1 except that the negative electrode obtained above was used. The cycle performance of the produced lithium ion battery was then evaluated. The results are shown in Table 2.
[0221] Example 8
[0222] In the same manner as in Example 7, an NMP solution (solid content concentration: 8%) of polyvinylidene fluoride (PVDF) as a binder was prepared.
[0223] Preparation of binder composition for positive electrode composite material layer
[0224] 30 parts of P01 were mixed with 100 parts (in terms of solid content) of a PVDF NMP solution to prepare an adhesive composition.
[0225] Preparation of slurry composition for positive electrode composite material layer
[0226] For 96 parts of lithium cobalt oxide, a positive electrode active material, 2 parts of acetylene black as a conductive material and 2 parts of the above-mentioned positive electrode composite material layer binder composition in terms of solid content were added. After the above-mentioned powder was mixed and stirred for 10 minutes, the solid content concentration was diluted to 70% with NMP and stirred for 1 hour at 3000rpm with a disperser. After that, ion exchange water was added to make the viscosity 4000±500mPa·s (B-type viscometer, measured at 25°C and 60rpm), thereby preparing a slurry composition for a positive electrode composite material layer.
[0227] Cathode Manufacturing
[0228] A positive electrode material and a positive electrode were prepared in the same manner as in Example 1 except that the above-obtained positive electrode material layer slurry composition was used. The compressibility of the positive electrode material layer was evaluated using the obtained positive electrode material, and the adhesiveness of the positive electrode material layer was evaluated using the obtained positive electrode.
[0229] Negative electrode manufacturing
[0230] In a double planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360mAh / g) as a negative electrode active material, 48.75 parts of natural graphite (theoretical capacity: 360mAh / g), and 1 part of carboxymethyl cellulose as a thickener were added in terms of solid content. Ion exchange water was then added to dilute the solid content concentration to 60%, and then stirred at a speed of 45rpm for 60 minutes. Then, 1.5 parts of polymer A obtained in the same manner as in Example 1 were added in terms of solid content, and stirred at a speed of 40rpm for 40 minutes. After that, ion exchange water was added to make the viscosity 4000±500mPa·s (B-type viscometer, measured at 25°C and 60rpm) to prepare a slurry composition for a negative electrode composite material layer.
[0231] The negative electrode composite material layer slurry composition was applied in an amount of 11±0.5 mg / cm 2 The copper foil coated with the negative electrode composite material layer slurry composition was then transported in an oven at 80°C for 2 minutes at a speed of 400 mm / min, and then transported in an oven at 110°C for 2 minutes to dry the slurry composition on the copper foil, thereby obtaining a negative electrode raw material for forming a negative electrode composite material layer on the current collector.
[0232] Afterwards, the negative electrode composite material layer side of the prepared negative electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 50 t (tons) to obtain a negative electrode composite material layer with a density of 1.70 g / cm3 The negative electrode was then placed in an environment with a temperature of 25±3°C and a relative humidity of 50±5% for 1 week.
[0233] <Manufacturing of separators and lithium-ion batteries>
[0234] A separator was prepared and a lithium ion battery was produced in the same manner as in Example 1 except that the positive electrode and negative electrode obtained above were used. The cycle performance of the obtained lithium ion battery was then evaluated. The results are shown in Table 2.
[0235] Example 9
[0236] Preparation of binder composition for positive electrode composite material layer
[0237] 30 parts of P01 were mixed with 100 parts (in terms of solid content) of an NMP solution of polyacrylonitrile (PAN) to prepare an adhesive composition.
[0238] Slurry composition for positive electrode composite material layer, positive electrode, negative electrode, separator, and production of lithium ion battery
[0239] A slurry composition for a positive electrode material layer, a positive electrode, a negative electrode, a separator, and a lithium ion battery were produced in the same manner as in Example 8 except that the binder composition for a positive electrode material layer obtained above was used. Thereafter, evaluation was performed in the same manner as in Example 8. The results are shown in Table 2.
[0240] Example 10
[0241] When preparing the binder composition for the positive electrode composite material layer, the same method as in Example 9 is used to manufacture the binder composition for the positive electrode composite material layer, the slurry composition for the positive electrode composite material layer, the positive electrode, the negative electrode, the separator, and the lithium ion battery. The electrolyte is adjusted as follows: as the electrolyte, the concentration of the LiPF6 solution is 12.5% [solvent: ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC) / propyl propionate (PP) / =1 / 1 / 1 / 2 (mass ratio) mixed solvent, additives: containing 4% by mass of fluoroethylene carbonate and 0.8% by mass of lithium difluorophosphate], and then the same evaluation as in Example 8 is carried out, and the results are shown in Table 2.
[0242] Embodiment 11
[0243] When preparing the binder composition for the positive electrode composite material layer, the same method as in Example 9 is used to manufacture the binder composition for the positive electrode composite material layer, the slurry composition for the positive electrode composite material layer, the positive electrode, the negative electrode, the separator, and the lithium ion battery. The electrolyte is adjusted as follows: as the electrolyte, a LiPF6 solution with a concentration of 12.5% [solvent: ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC) / propyl propionate (PP) / =1 / 1 / 1 / 2 (mass ratio) mixed solvent, additives: containing 4% by mass of fluoroethylene carbonate and 4% by mass of succinonitrile] is used, and then the evaluation is carried out in the same manner as in Example 8, and the results are shown in Table 2.
[0244] Example 12
[0245] When preparing the binder composition for the positive electrode composite material layer, the same method as in Example 9 is used to manufacture the binder composition for the positive electrode composite material layer, the slurry composition for the positive electrode composite material layer, the positive electrode, the negative electrode, the separator, and the secondary battery. The electrolyte is adjusted as follows: as the electrolyte, the concentration of the LiPF6 solution is 12.5% [solvent: ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC) / propyl propionate (PP) / =1 / 1 / 1 / 2 (mass ratio) mixed solvent, additives: containing 4% by mass of fluoroethylene carbonate, containing 2% by mass of l,3,6-hexane trinitrile], and then the same evaluation as in Example 8 is carried out, and the results are shown in Table 2.
[0246] Example 13
[0247] Preparation of adhesive composition for porous membrane layer
[0248] 30 parts of P01 were mixed with 100 parts (in terms of solid content) of an aqueous dispersion of polyacrylic acid (ACR) to prepare an adhesive composition.
[0249] Preparation of slurry composition for porous membrane
[0250] A ball mill is used to mix 100 parts of aluminum oxide as non-conductive particles in terms of solid content, 5 parts of the above-mentioned binder composition for the porous membrane layer in terms of solid content, 1.5 parts of polyacrylamide as a thickener, and 0.8 parts of polyacrylic acid as a dispersant, and ion exchange water is added to make the solid content concentration become 40% to obtain a slurry composition for the porous membrane layer.
[0251] Diaphragm manufacturing
[0252] The porous film layer slurry composition obtained above is applied to an organic diaphragm substrate (7μm polyethylene, Xingyuan material) as a substrate in a manner that the coating thickness of the porous film layer slurry composition becomes 2μm, and dried at 50°C for 10 minutes to obtain a diaphragm having a porous film layer on one side of the organic diaphragm substrate. The adhesion of the porous film layer is evaluated using the diaphragm having a porous film layer on one side. The results are shown in Table 2. In addition, by performing the above-mentioned coating and drying operations on both sides, a diaphragm having a porous film layer on both sides of the organic diaphragm substrate is obtained.
[0253] Negative electrode manufacturing
[0254] A negative electrode was produced in the same manner as in Example 8.
[0255] Cathode Manufacturing
[0256] A positive electrode was produced in the same manner as in Example 1.
[0257] Lithium-ion battery manufacturing
[0258] Using the above-mentioned negative electrode, positive electrode and separator, a wound battery cell is prepared and placed in an aluminum-plastic film packaging material. Afterwards, a 12.5% LiPF6 solution as an electrolyte is filled into the packaging material [Solvent: ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC) / propyl propionate (PP) / =1 / 1 / 1 / 2 (mass ratio) mixed solvent, additive: containing 4% by mass of fluoroethylene carbonate]. Then, a heat seal at a temperature of 150°C is performed to seal the packaging material to manufacture a lithium-ion battery. The cycle performance is evaluated using the lithium-ion battery, and the results are shown in Table 2.
[0259] Comparative Example 1
[0260] When preparing the binder composition for the negative electrode composite material layer, epoxy phosphate was not added. Otherwise, the same method as in Example 1 was used to manufacture styrene-butadiene copolymer (SBR) as a binder, a binder composition for the negative electrode composite material layer, a slurry composition for the negative electrode composite material layer, a negative electrode, a positive electrode, a separator, and a lithium ion battery. Afterwards, the same method as in Example 1 was used to evaluate, and the results are shown in Table 2.
[0261] Comparative Example 2
[0262] When preparing the binder composition for the negative electrode composite material layer, the amount of P01 was changed to 200 parts, and the same method as in Example 6 was used to manufacture acrylic acid / acrylamide copolymer (AA / AAm) as a binder, a binder composition for the negative electrode composite material layer, a slurry composition for the negative electrode composite material layer, a negative electrode, a positive electrode, a separator, and a lithium ion battery. Afterwards, the evaluation was carried out in the same manner as in Example 1, and the results are shown in Table 2.
[0263] Comparative Example 3
[0264] When preparing the binder composition for the positive electrode composite material layer, epoxy phosphate was not added. Otherwise, polyvinylidene fluoride (PVDF) as a binder material, a binder composition for the positive electrode composite material layer, a slurry composition for the positive electrode composite material layer, a positive electrode, a negative electrode, a separator, and a lithium ion battery were manufactured in the same manner as in Example 8. Thereafter, the evaluation was performed in the same manner as in Example 8, and the results are shown in Table 2.
[0265] Comparative Example 4
[0266] When preparing the binder composition for the positive electrode composite material layer, epoxy phosphate was not added. Otherwise, polyacrylonitrile (PAN) as a binder, a binder composition for the positive electrode composite material layer, a slurry composition for the positive electrode composite material layer, a positive electrode, a negative electrode, a separator, and a lithium ion battery were manufactured in the same manner as in Example 9. Evaluation was then performed in the same manner as in Example 8, and the results are shown in Table 2.
[0267] Comparative Example 5
[0268] When preparing the porous membrane layer binder composition, epoxy phosphate was not added. Otherwise, polyacrylic acid (ACR) as a binder material, a porous membrane layer binder composition, a porous membrane layer slurry composition, a separator, a positive electrode, a negative electrode, and a lithium ion battery were manufactured in the same manner as in Example 13. Evaluation was then performed in the same manner as in Example 13, and the results are shown in Table 2.
[0269] Comparative Example 6
[0270] The results are shown in Table 2. The same procedures as in Comparative Example 2 were carried out except that the epoxy phosphate P01 was changed to 5 parts when preparing the binder composition for the negative electrode material layer.
[0271] Table 2 Comparison of secondary battery performance of the present embodiment and the comparative example
[0272]
[0273]
[0274] As shown in Table 2, in Examples 1 to 13 using a binder composition comprising a binder and an epoxy phosphate ester, wherein the amount of the epoxy phosphate ester relative to the binder is within a specific range, the functional layer can exhibit excellent adhesion and the cycle performance of the lithium ion battery can be improved. In addition, as shown in Table 2, in Examples 1 to 12 using a binder composition comprising a binder and an epoxy phosphate ester, wherein the amount of the epoxy phosphate ester relative to the binder is within a specific range and an electrode composite material layer is prepared, an electrode composite material layer with excellent compressibility can be obtained.
[0275] On the other hand, it can be seen from Table 2 that in Comparative Examples 1, 3 to 5 using a binder composition containing a binder but not epoxy phosphate, both the adhesion of the functional layer and the cycle performance of the lithium ion battery cannot be fully ensured. In addition, it can be seen from Table 2 that in Comparative Examples 1, 3, and 4 in which an electrode composite material layer is prepared using a binder composition containing a binder but not epoxy phosphate, the compressibility of the electrode composite material layer is impaired. Moreover, it can be seen from Table 2 that in Comparative Examples 2 and 6 in which an electrode composite material layer (functional layer) is prepared using a binder composition containing a binder and epoxy phosphate, but the amount of epoxy phosphate relative to the binder exceeds a specific range, the adhesion of the functional layer and the cycle performance of the lithium ion battery cannot be fully ensured, and the compressibility of the electrode composite material layer is also impaired.
[0276] On the other hand, it can be seen from Table 2 that when using an electrolyte containing a binding material and epoxy phosphate, and including lithium difluorophosphate, succinonitrile or 1,3,6-hexanetrinitrile, the decomposition of epoxy phosphate under high voltage can be suppressed, thereby further improving the cycle performance of the lithium ion battery under high voltage and reducing the internal resistance.
[0277] Industrial Applicability
[0278] According to the present application, it is possible to provide a secondary battery binder composition that has excellent binding properties and can form a functional layer that can improve the cycle performance of a secondary battery.
[0279] Furthermore, according to the present application, it is possible to provide a slurry composition for a secondary battery functional layer that has excellent adhesiveness and can form a functional layer that can improve the cycle performance of a secondary battery.
[0280] Furthermore, according to the present application, it is possible to provide a functional layer for a secondary battery that has excellent adhesiveness and can improve the cycle performance of the secondary battery.
[0281] Furthermore, according to the present application, a secondary battery having excellent cycle performance can be provided.
[0282] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.
Claims
1. A binder composition for secondary batteries, characterized in that The invention comprises a bonding material and epoxy phosphate ester, and the mass ratio of the epoxy phosphate ester to the bonding material is (0.1-0.8):
1.
2. The binder composition for secondary batteries according to claim 1, characterized in that: The mass ratio of the epoxy phosphate and the bonding material contained in the composition is (0.1-0.6):
1.
3. The binder composition for secondary batteries according to claim 1 or 2, characterized in that: The acid value of the epoxy phosphate is 5 to 70 mgKOH / g, preferably 28 to 60 mgKOH / g, and more preferably 35 to 57 mgKOH / g; And / or, the bonding material comprises a combination of one or more of aliphatic conjugated diene / aromatic vinyl copolymers, acrylic polymers, fluorine polymers, acrylic acid / acrylamide copolymers and acrylonitrile polymers, preferably a combination of one or more of styrene-butadiene copolymers, polyvinylidene fluoride and polyacrylonitrile.
4. The binder composition for secondary batteries according to claim 1, characterized in that The invention also comprises a solvent and additives which may be added or not added, wherein the solvent is used to dissolve and / or disperse the bonding material and the epoxy phosphate ester. 5 . Use of the binder composition for secondary batteries according to claim 1 in preparing a slurry composition for a functional layer for secondary batteries, a functional layer for secondary batteries, a member for secondary batteries or a secondary battery.
6. A slurry composition for a functional layer of a secondary battery, characterized in that A secondary battery binder composition comprising the binder composition according to any one of claims 1 to 5.
7. The slurry composition for a functional layer for a secondary battery according to claim 6, characterized in that: The slurry composition is a slurry composition for an electrode containing an electrode active material, and the mass ratio of the binder composition to the electrode active material particles is (0.5-15):100 in terms of solid content conversion; Alternatively, the slurry composition is a slurry composition for a porous membrane layer containing non-conductive particles, and the mass ratio of the binder composition to the non-conductive particles is (0.5 to 30):100 in terms of solid content.
8. A functional layer for a secondary battery, characterized in that: The secondary battery functional layer is formed from the slurry composition for a secondary battery functional layer according to any one of claims 6 to 7.
9. A secondary battery component, characterized in that The secondary battery functional layer according to claim 8 is included.
10. A secondary battery, characterized in that The secondary battery functional layer according to claim 8 or the secondary battery member according to claim 9 is included.
11. The secondary battery according to claim 10, characterized in that The invention comprises a positive electrode, a negative electrode, a separator and an electrolyte; at least one of the positive electrode, the negative electrode and the separator comprises the functional layer for the secondary battery.
12. The secondary battery according to claim 10, characterized in that: The secondary battery includes a lithium ion battery or a sodium ion battery.
13. The secondary battery according to claim 11, characterized in that: The electrolyte includes at least one of lithium difluorophosphate, succinonitrile or 1,3,6-hexanetrinitrile.