Modified solid electrolyte and application thereof in solid-state battery
By combining garnet solid electrolyte with anti-perovskite, a dense body phase morphology and fast lithium ion transmission path is formed, the thermal stability and energy density of lithium ion batteries are solved, and high energy density and safety are achieved solid state battery.
Patent Information
- Application Number
- CN202411250970.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The existing lithium-ion batteries have limited the application time and safety of the battery due to poor thermal stability, high flammability and leakage problems of liquid electrolytes, and insufficient energy density of graphite anode and transition metal oxide positive electrodes.
The garnet-type solid electrolyte is combined with antiperovskite modifications, and Li2OHCl antiperovskite is generated through ultrasonic treatment and vacuum sintering, forming a dense body phase morphology and a fast lithium ion transmission pathway, blocking electron injection, and passing anticalcium The lithium-philicity of titanium ore achieves uniform wetting of the lithium anode interface.
It significantly improves the electrochemical cycling performance of solid-state batteries, enhances lithium ion conductivity and electron blocking capabilities, reduces dendrite formation, achieves high energy density and safety, and extends the service life of the battery.
Smart Images

Figure CN119069779A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a modified solid electrolyte and application thereof in solid-state batteries. Background Art
[0002] With the rapid growth in sales of electronic devices and electric vehicles, higher requirements are also placed on battery safety and energy density. Lithium-ion batteries are recognized as one of the most important energy storage systems due to their high energy density and have been widely studied and achieved great success. Lithium-ion batteries based on liquid electrolytes are approaching their theoretical energy limits and are no longer sufficient to power electric vehicles due to a variety of reasons such as energy density, cost, life, and safety. Although liquid electrolytes have high ionic conductivity and good electrode wettability, they still have safety issues such as poor thermal stability, high flammability, and leakage problems. In addition, lithium-ion batteries based on graphite anodes and transition metal oxide positive electrodes typically exhibit energy densities below 260Whkg -1 The mass energy density of batteries limits the operating time of battery-powered devices.
[0003] The development of batteries with higher specific energy, no explosion risk and long service life is essential to meet the stringent requirements of large-scale energy storage devices and various consumer electronic products. Solid-state batteries have become the pioneers of the transformation of lithium-ion battery technology. Solid-state rechargeable batteries using solid electrolytes instead of flammable liquid electrolytes have the inherent advantage of improving the safety and stability of state-of-the-art battery technology. Its unique safety and higher energy density. Among the many candidate materials in the field of solid-state electrolytes, garnet-type solid electrolytes stand out due to their excellent ionic conductivity, shear modulus and chemical stability. However, the poor contact between the solid electrolyte and the positive electrode and anode has become a major obstacle to the practical application of solid-state batteries.
[0004] Therefore, it is urgent to find a modification method to make up for the intrinsic defects of garnet-type solid electrolytes, such as high sintering temperature, high interface resistance, pore cracks, etc., and realize dendrite-free solid electrolytes. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention proposes a modified solid electrolyte and its application in solid-state batteries. The antiperovskite modification provided by the present invention makes up for the multiple intrinsic defects of the garnet-type solid electrolyte. The antiperovskite coating at the surface and grain boundary provides a dense bulk morphology, constructs a fast lithium ion transmission path in situ, and blocks electron injection. On the other hand, the lithium affinity of the antiperovskite makes the lithium anode interface uniformly wetted. The solid-state battery containing the solid electrolyte exhibits excellent electrochemical cycle performance.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A modified solid electrolyte comprises a garnet-type solid electrolyte and an antiperovskite as a grain boundary filler. Specifically, the garnet-type solid electrolyte is immersed in an antiperovskite precursor solution for ultrasonic treatment for 30 minutes, and then vacuum sintered at 350°C for 6 hours. During the vacuum sintering process, LiOH and LiCl react to generate Li2OHCl antiperovskite to obtain the modified solid electrolyte. The precursor solution is prepared by adding 0.15 mol LiOH and 0.1-0.25 mol LiCl into deionized water to prepare a 100 mL solution, adding a stirring magnet, and stirring on a magnetic stirrer until fully dissolved.
[0008] As an improvement, the garnet-type solid electrolyte includes but is not limited to Li7La3Zr2O 12 (LLZO), Li 6.4 LqCy 1.4 Ta 0.6 O 12 (LLZTO), Li 6.75 La 2.9 Ga 0.1 Nb 0.25 Zr 1.75 O 12 (LLGNZO), Li 6.5 LqCy 1.5 Nb 0.5 O 12 (LLZNO).
[0009] A further improvement is that when the general formula of the garnet-type solid electrolyte is Li 6.4 LqCy 1.4 Ta 0.6 O 12 When using Li2CO3, La2O3, ZrO2, and Ta2O5, they are added in a stoichiometric ratio and then sintered. The amount of Li2CO3 added needs to be 20% in excess to ensure that the amount is insufficient due to volatilization. The particle size of the obtained garnet-type solid electrolyte is 0.5-15μm, the diameter of the disc is 13-14mm, and the thickness is 1mm.
[0010] A further improvement is that the garnet-type solid electrolyte Li 6.4 LqCy 1.4 Ta 0.6 O 12The preparation process is as follows: Li2CO3, La2O3, ZrO2, Ta2O5 and ZrO2 ball milling beads are mixed with the ball-to-material mass ratio of 2:1, ball milled at 1200rpm for 2 hours, and then calcined in a magnesium oxide crucible at 900℃ for 6 hours to obtain pre-burned powder, 1.2wt% Al2O3 is added to the pre-burned powder as a sintering aid, and ball milling is continued for 2 hours to obtain prefabricated powder, the prefabricated powder is cold pressed into a green embryo at 500MPa, and a small amount of prefabricated powder is sprinkled on the green embryo, and after sintering in N2 at 1180℃ for 16 hours, the disc is polished with 800 and 1000 mesh sandpaper in turn, washed with anhydrous ethanol and dried.
[0011] As an improvement, the added amount of LiCl is 0.15 mol.
[0012] Application of the above modified solid electrolyte in the preparation of solid-state batteries.
[0013] A solid-state battery is assembled from the modified solid electrolyte, a positive electrode and a negative electrode.
[0014] As an improvement, the positive electrode is LiNi 0.928 Co 0.072 O2 and acetylene black were added to a solution of polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP), and then stirred evenly using a centrifugal mixer, coated on a carbon-coated aluminum foil, and dried overnight in a vacuum oven at 110°C, and finally cut into discs with a diameter of 8 mm. The mass fraction of polyvinylidene fluoride in N-methyl-2-pyrrolidone was 6 wt%, and LiNi 0.928 Co 0.072 O2, acetylene black and polyvinylidene fluoride are mixed in a weight ratio of 8:1:1.
[0015] As an improvement, the negative electrode is prepared by placing a clean lithium sheet in a nickel crucible, heating it to melt at 320°C on a heating table in an argon glove box, carefully scraping off the oxide film on the surface of the lithium liquid with tweezers and a stainless steel spoon, and then clamping the modified solid electrolyte described in claim 1 in the lithium liquid with tweezers and scraping it so that one side is completely wetted and covered by the molten lithium. After cooling, the edge is polished so that the lithium is retained only on one side.
[0016] The assembly method of the above-mentioned solid-state battery is as follows: in an argon glove box, 7 μL of electrolyte (1.0 M LiPF6, the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) is added to the other side of the modified solid electrolyte of the above-mentioned negative electrode to ensure good contact between the modified solid electrolyte and the positive electrode, and then it is bonded with the above-mentioned positive electrode; nickel foam is placed on the outside of the negative electrode and the positive electrode to act as a buffer to prevent the modified solid electrolyte from breaking during the battery packaging process. Finally, it is loaded into a CR2032 button battery and maintained at a pressure of 500 psi for 10 seconds on a battery sealing machine to obtain a solid-state battery.
[0017] The modified solid electrolyte of the present invention comprises a garnet-type solid electrolyte and an antiperovskite modified layer filled at the grain boundary of the garnet-type solid electrolyte, wherein the antiperovskite modified layer is formed by immersing the garnet-type solid electrolyte in an antiperovskite precursor solution by ultrasound and then vacuum sintering reaction. The antiperovskite modified material formed during the sintering process well compensates for the multiple intrinsic defects of the garnet-type solid electrolyte, and the low-melting-point antiperovskite material melts and infiltrates the garnet-type solid electrolyte through capillary action, and is formed in situ at the grain boundary, providing a dense bulk morphology, constructing a fast lithium ion transmission path in situ, and blocking electron injection. On the other hand, the lithium affinity of the antiperovskite makes the lithium anode interface uniformly wetted, effectively improving the electrochemical performance of the solid-state battery assembled by the solid electrolyte.
[0018] Beneficial Effects
[0019] Compared with the prior art, the present invention discloses a modified solid electrolyte and its application in a solid-state battery. A garnet-type solid electrolyte is selected to be immersed in an antiperovskite precursor solution. During the vacuum sintering process, LiOH and LiCl react to form Li2OHCl antiperovskite. The antiperovskite as a modified product shows the highest lithium concentration among all lithium-based solid electrolytes to date, and has a wide voltage window, ultra-high ionic conductivity, high electron blocking, special structural tunability and mechanical flexibility. At the same time, it makes up for the intrinsic defects of the garnet-type solid electrolyte. The low melting point characteristics of the antiperovskite enable it to be formed in situ during the vacuum sintering process at 360°C, and melt and penetrate through capillary action to fill the pores and grain boundaries of the solid electrolyte. The antiperovskite on the surface and grain boundaries provides fast lithium ion transport kinetics during the cycle, blocks electron injection, and inhibits dendrite formation. In addition, the lithium affinity of the antiperovskite allows the lithium anode interface to be uniformly wetted, while improving the interface stability and reducing the influence of the grain boundary energy barrier of the garnet-type solid electrolyte, thereby realizing a low-temperature sintered dendrite-free solid electrolyte. The solid-state battery prepared using the modified solid-state electrolyte of the present invention exhibits excellent electrochemical cycle performance and has good market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1The XRD patterns of Example 2, Comparative Examples 1, 2, Comparative Example 6 and Comparative Example 9 are shown;
[0021] Figure 2 Surface SEM images of Example 2, Comparative Examples 2, 4, and Comparative Example 5;
[0022] Figure 3 The cross-sectional SEM images of Example 2 and Comparative Example 2;
[0023] Figure 4 The electrochemical impedance test results of Examples 1 to 4, Comparative Example 2 and Comparative Example 5 are shown;
[0024] Figure 5 This is the cycle performance of Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to more clearly demonstrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with embodiments.
[0027] The testing method of the present invention is as follows:
[0028] The electrochemical impedance test (EIS) was measured using an electrochemical workstation (WonATech ZIVE SP2) in the frequency range of 1 Hz to 7 MHz, with an AC amplitude of 50 mV. The test method is: prepare the negative electrode on both sides of the solid electrolyte according to the method described in the sixth aspect. After cooling, use 400 mesh sandpaper to grind the lithium on the edge of the disc to block the connection between the two poles. And assemble the battery according to the method described in the sixth aspect, except for the steps of adding electrolyte and attaching the positive electrode.
[0029] The constant current charge and discharge test uses Blue Power (CT3002A), and the specific test steps are: let it stand for 2 hours, charge at 0.1C to a voltage of 4.3V, let it stand for 1 minute, discharge at 0.1C to a voltage of 2.7V, let it stand for 1 minute, and cycle test.
[0030] It should be noted that all embodiments of the present invention and comparative examples use the same garnet-type solid electrolyte.
[0031] Example 1
[0032] 0.1 mol LiOH and 0.1 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0033] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0034] Example 2
[0035] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0036] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0037] Example 3
[0038] 0.2 mol LiOH and 0.2 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0039] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0040] Example 4
[0041] 0.25 mol LiOH and 0.25 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0042] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0043] Comparative Example 1
[0044] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0045] The solution was placed in an oven at 60°C for drying, and the obtained product was ground and then sintered in a tube furnace at 350°C for 6 hours in vacuum to obtain antiperovskite.
[0046] Comparative Example 2
[0047] The garnet-type solid electrolyte is directly synthesized without any modification.
[0048] Comparative Example 3
[0049] 0.3 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0050] The garnet-type solid electrolyte was placed in a precursor solution and ultrasonically treated for 30 minutes using an ultrasonic cleaner. The treated solid electrolyte was vacuum sintered at 350° C. in a tubular furnace for 6 hours to obtain a comparative solid electrolyte.
[0051] Comparative Example 4
[0052] 0.15 mol LiOH and 0.3 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0053] The garnet-type solid electrolyte was placed in a precursor solution and ultrasonically treated for 30 minutes using an ultrasonic cleaner. The treated solid electrolyte was vacuum sintered at 350° C. in a tubular furnace for 6 hours to obtain a comparative solid electrolyte.
[0054] Comparative Example 5
[0055] 0.3 mol LiOH and 0.3 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0056] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0057] Comparative Example 6
[0058] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0059] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaner. The treated solid electrolyte was vacuum sintered in a tubular furnace at 250° C. for 6 hours to obtain a modified solid electrolyte.
[0060] Comparative Example 7
[0061] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0062] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered in a tubular furnace at 450° C. for 6 hours to obtain a modified solid electrolyte.
[0063] Comparative Example 8
[0064] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0065] The garnet-type solid electrolyte was placed in a precursor solution, and ultrasonically treated for 30 minutes using an ultrasonic cleaner. The treated solid electrolyte was vacuum sintered at 550° C. in a tubular furnace for 6 hours to obtain a modified solid electrolyte.
[0066] Comparative Example 9
[0067] 0.15 mol LiOH and 0.15 mol LiCl were added into deionized water to prepare 100 mL of solution, a stirring magnet was added, and the mixture was stirred on a magnetic stirrer until fully dissolved to obtain a precursor solution.
[0068] The garnet-type solid electrolyte was placed in a precursor solution and ultrasonically treated for 30 minutes using an ultrasonic cleaning machine. The treated solid electrolyte was vacuum sintered at 650° C. in a tubular furnace for 6 hours to obtain a modified solid electrolyte.
[0069] Comparative Example 10
[0070] The garnet-type solid electrolyte was placed in deionized water without additives, and ultrasonically treated for 30 minutes using an ultrasonic cleaner. The treated solid electrolyte was vacuum sintered in a tubular furnace at 350° C. for 6 hours to obtain a modified solid electrolyte.
[0071] Figure 1The XRD patterns of Example 2, Comparative Examples 1, 2, 6 and 9 are shown in Table 1. Comparative Example 1 is an antiperovskite obtained by vacuum sintering the precursor. Its XRD diffraction pattern is consistent with the standard diffraction pattern of antiperovskite Li3OBr and has no impurity peaks, indicating that this method successfully prepares pure antiperovskite. Comparative Example 2 is an unmodified garnet-type solid electrolyte. Its diffraction peak shape is consistent with that of cubic garnet phase Li5La3Nb2O 12 The standard diffraction card is in good agreement, and the cubic phase has higher lithium ion conductivity than the tetragonal garnet phase. Example 2 is a solid electrolyte modified with antiperovskite, and its diffraction spectrum shows a new peak at 21.9° and a broadening of the LLZO peak at 31.2°, corresponding to the (100) and (110) crystal planes of the antiperovskite, which indicates the successful doping and coating of the antiperovskite. Comparative Examples 6 and 9 have unsuitable sintering temperatures, resulting in residual reactants LiOH and LiCl raw materials, while Example 2 uses 350°C, slightly higher than the melting point of the antiperovskite, so that LiOH and LiCl fully react to form Li2OHCl antiperovskite without decomposition and volatilization due to excessively high temperatures.
[0072] Figure 2 The surface SEM images of Example 2, Comparative Examples 2, 4, and Comparative Example 5. Comparative Example 2 shows the surface micromorphology of the original LLZO, whose inherent porous skeleton leads to poor grain boundaries and high resistance. In contrast, Example 2 presents a dense and uniform morphology, which is due to the pores and grain boundaries of the LLZO ceramic skeleton being filled with molten infiltrated antiperovskite. The illustration in the upper right corner is a photograph of the bright surface of the modified garnet electrolyte. The surface of Comparative Example 4 shows many impurity particles, corresponding to excess, incompletely reacted LiCl; while there is no such phenomenon in Example 2, indicating that the reaction is complete and no excess raw materials remain. Comparative Example 5 shows an overly thick coating layer, and the excess antiperovskite crystallizes on the surface of the solid electrolyte to form an uneven shell; while there is no such phenomenon in Example 2, indicating that the concentration of the precursor solution is appropriate and the doping is uniform.
[0073] Figure 3The cross-sectional SEM images of Example 2 and Comparative Example 2 are shown, with a solid electrolyte on the top and a lithium metal negative electrode on the bottom, which is prepared by the method for preparing the negative electrode described in the sixth aspect. The interface contact between the solid electrolyte and the molten lithium metal anode is shown. In Comparative Example 2, many isolated pores are distributed along the interface. This is because the original LLZO surface has poor lithium affinity and the molten lithium liquid cannot fully wet it, which reduces the contact surface area, resulting in uneven lithium ion transport and charge distribution, causing high interface resistance and premature lithium dendrite growth. Example 2 presents a compact interface contact without voids or gaps. At the same time, the upper part presents a dense internal bulk morphology of the modified solid electrolyte, which indicates that the molten antiperovskite uniformly penetrates the grain boundaries of the solid electrolyte to form a flexible and dense internal morphology. The antiperovskite connects the LLZO grains, constructs a three-dimensional lithium ion transmission channel in situ, and reduces the resistance of the grain boundary barrier. At the same time, the electron blocking properties of the antiperovskite can inhibit dendrite growth and bring significantly improved cycle performance.
[0074] Figure 4 The electrochemical impedance test (EIS) results of Examples 1 to 4, Comparative Examples 2 and Comparative Examples 5. For Comparative Examples 6 to 9, Comparative Examples 3 and 4, the molten lithium liquid cannot wet the surface of the solid electrolyte, resulting in excessive impedance. The results are as follows: The melting point of the antiperovskite is about 320°C. The sintering temperature of Example 2 using 350°C ensures that the reaction is complete and the antiperovskite is fully melted and infiltrated. The sintering temperature of Comparative Example 6 is too low and the reaction cannot proceed. The sintering temperature of Comparative Examples 7 to 9 is too high, and the hydroxyl (–OH) in the antiperovskite is hydrolyzed and decomposed into raw materials again. Excessive single reactants remain in Comparative Examples 3 and 4. All of the above result in the lithium-phobic LiOH and LiCl raw materials remaining on the surface of the solid electrolyte, making it impossible for the molten lithium liquid to wet, resulting in the inability to prepare the negative electrode. The Nyquist plot shows a low-frequency straight line (ion blocking behavior) and two semicircular capacitive behaviors. By fitting an appropriate equivalent circuit, the total conductivity is calculated, and the specific results are shown in Table 1.
[0075] Table 1 EIS test results of solid electrolytes of Examples 1 to 4 and Comparative Examples 2 to 5
[0076]
[0077] The high-frequency semicircle is the sum of the bulk and grain boundary resistances of the solid electrolyte, and the medium-frequency semicircle represents the impedance of the interface between the solid electrolyte and the lithium anode. The ionic conductivity of Comparative Example 2 is 1.8×10 – 4 S cm -1, and exhibits a large interface resistance. This is because the original garnet-type solid electrolyte surface has insufficient lithium affinity and is easy to react with water and carbon dioxide in the atmosphere to generate a high-impedance impurity interface phase. Among Examples 1 to 5, Example 2 shows the lowest interface resistance and the highest ionic conductivity, reaching 6.2×10 – 4 S cm -1 , indicating that the appropriate concentration of the precursor solution brings the best modification effect. The molten infiltrated antiperovskite reduces the high grain boundary energy barrier of the original LLZO, constructs a three-dimensional fast lithium ion transmission path in situ, and significantly improves the ionic conductivity of the solid electrolyte. In addition, the antiperovskite-modified lithium-philic interface fully wets the molten lithium anode, brings about a compact interface contact, and optimizes the interface impedance. The results of Comparative Example 10 are similar to those of Comparative Example 2, indicating that the negative impact caused by immersion in deionized water is small.
[0078] Figure 5 The cycle performance of Example 2 and Comparative Example 2 was tested by constant current charge and discharge using a blue electric test system, with a current density of 0.1C and a voltage range of 4.3 to 2.7V. 0.928 Co 0.072 O2 high-voltage positive electrode to demonstrate its potential for application in high-voltage and high-energy-density new solid-state batteries. Comparative Example 2 decays rapidly after 50 cycles, which is attributed to the rapid penetration of lithium dendrites caused by electron injection along the grain boundaries. The modified solid electrolyte of Example 2 retains 77.9% of its capacity after 200 cycles, and its average Coulomb efficiency is 97.3%. The excellent electrochemical performance is due to the lithium-philic interface of the modified solid electrolyte and the three-dimensional fast lithium ion transport pathway formed by the antiperovskite at the LLZO grain boundary, which can well regulate the lithium stripping / plating behavior, accelerate bulk and interfacial charge transfer, and inhibit the formation of lithium dendrites.
[0079] In summary, under the same conditions, the solid-state battery assembled using the modified solid-state electrolyte provided by the present invention has better cycle performance, higher capacity retention rate, and lower bulk and interface resistance than the solid-state battery assembled using the unmodified solid-state electrolyte.
[0080] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A modified solid electrolyte, characterized in that: The modified solid electrolyte includes a garnet-type solid electrolyte and an antiperovskite as a grain boundary filler. Specifically, the garnet-type solid electrolyte is immersed in an antiperovskite precursor solution and ultrasonically treated for 30 minutes, and then vacuum sintered at 350° C. for 6 hours. During the vacuum sintering process, LiOH and LiCl react to generate Li2OHCl antiperovskite to obtain the modified solid electrolyte. The precursor solution is prepared by adding 0.15 mol LiOH and 0.1-0.25 mol LiCl into deionized water to prepare a 100 mL solution, adding a stirring magnet, and stirring on a magnetic stirrer until fully dissolved.
2. The modified solid electrolyte according to claim 1, characterized in that The garnet-type solid electrolyte includes but is not limited to Li7La3Zr2O 12 , Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 , Li 6.75 La 2.9 Ga 0.1 Nb 0.25 Zr 1.75 O 12 , Li 6.5 Ln3Z 1.5 Nb 0.5 O 12 .
3. The modified solid electrolyte according to claim 1, characterized in that When the general formula of garnet-type solid electrolyte is Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 When using Li2CO3, La2O3, ZrO2, and Ta2O5, they are added in a stoichiometric ratio and then sintered. The amount of Li2CO3 added needs to be 20% in excess to ensure that the amount is insufficient due to volatilization. The particle size of the obtained garnet-type solid electrolyte is 0.5-15μm, the diameter of the disc is 13-14mm, and the thickness is 1mm.
4. The modified solid electrolyte according to claim 3, characterized in that The garnet-type solid electrolyte Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 The preparation process is as follows: Li2CO3, La2O3, ZrO2, Ta2O5 and ZrO2 ball milling beads are mixed with the ball-to-material mass ratio of 2:1, ball milled at 1200rpm for 2 hours, and then calcined in a magnesium oxide crucible at 900℃ for 6 hours to obtain pre-burned powder, 1.2wt% Al2O3 is added to the pre-burned powder as a sintering aid, and the ball milling is continued for 2 hours to obtain a prefabricated powder, the prefabricated powder is cold pressed into a green embryo at 500MPa, and a small amount of prefabricated powder is sprinkled on the green embryo, and after sintering in N2 at 1180℃ for 16 hours, the disc is polished with 800 and 1000 mesh sandpaper in turn, washed with anhydrous ethanol and dried.
5. The modified solid electrolyte according to claim 1, characterized in that The added amount of LiCl is 0.15 mol.
6. Use of the modified solid electrolyte according to claim 1 in the preparation of solid-state batteries.
7. A solid-state battery, characterized in that: The modified solid electrolyte, a positive electrode and a negative electrode are assembled from the modified solid electrolyte according to claims 1 to 5.
8. The solid-state battery according to claim 7, characterized in that: The positive electrode is LiNi 0.928 Co 0.072 O2 and acetylene black are added to the N-methyl-2-pyrrolidone solution of polyvinylidene fluoride, and then stirred evenly with a centrifugal mixer, coated on a carbon-coated aluminum foil, and vacuum dried at 110°C overnight, and finally cut into discs with a diameter of 8 mm, wherein the mass fraction of polyvinylidene fluoride in N-methyl-2-pyrrolidone is 6wt%, wherein LiNi 0.928 Co 0.072 O2, acetylene black and polyvinylidene fluoride are mixed in a weight ratio of 8:1:
1.
9. The solid-state battery according to claim 7, characterized in that: The negative electrode is prepared by placing a clean lithium sheet in a nickel crucible, heating it to melt at 320°C on a heating table in an argon glove box, carefully scraping off the oxide film on the surface of the lithium liquid with tweezers and a stainless steel spoon, and then clamping the modified solid electrolyte described in claim 1 in the lithium liquid with tweezers and scraping it so that one side is completely wetted and covered by the molten lithium. After cooling, the edge is polished so that the lithium is retained only on one side.
10. The method for assembling a solid-state battery according to claim 9, characterized in that: In an argon glove box, 7 μL of electrolyte was dripped on the other side of the modified solid electrolyte of the negative electrode described in claim 9 to ensure good contact between the modified solid electrolyte and the positive electrode, and then bonded with the positive electrode described in claim 8; nickel foam was placed on the outside of both the negative electrode and the positive electrode to act as a buffer to prevent the modified solid electrolyte from breaking during the battery packaging process. Finally, it was loaded into a CR2032 button battery and maintained at a pressure of 500 psi for 10 seconds on a battery sealing machine to obtain a solid-state battery.
Citation Information
Patent Citations
Oxide solid electrolytes based on lithium halide-doping and low-temperature sintering method thereof
CN107732295A
Lithium-rich anti-perovskite oxide composite electrolyte and preparation method and application thereof
CN112993389A
Composite solid electrolyte material and preparation method thereof, preparation method of solid electrolyte sheet and all-solid-state battery
CN113054244A
Garnet-based mixed ion / electron conductive interface modified solid-state battery and preparation method thereof
CN118472411A