Solid electrolyte and preparation method thereof, positive electrode material, battery and electric device
Through spray pyrolysis method and high entropy doping technology, the low conductivity problem of NASICON type solid electrolyte is solved, and solid electrolyte with high ion and electron conductivity is prepared, which improves the performance of solid-state batteries.
Patent Information
- Application Number
- CN202411391506.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing NASICON type solid electrolyte has low ionic conductivity and cannot be used alone in all solid state batteries. In addition, traditional solid phase reactions are sensitive to temperature, easy to generate heterogeneous phases, and difficult to prepare fine crystal dense sintered bodies, which affects the energy density of the battery. .
The NASICON type solid electrolyte was prepared by spray pyrolysis method, and the lattice constant was regulated through high entropy doping, reducing crystallinity, and constructing a 3D fast ion transmission channel to improve ionic conductivity, and covering the surface with a carbon layer to improve electron conductivity.
The high ionic conductivity and electronic conductivity are improved, the preparation process is simplified, the sintering temperature is reduced, and the energy density and rate performance of the battery are improved.
Smart Images

Figure CN119069781A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and more specifically, to a solid electrolyte and a preparation method thereof, a positive electrode material, a battery and an electrical device. Background Art
[0002] In the solid-state battery system, one of the most critical materials is the solid electrolyte. Solid electrolytes include organic polymers, sulfides, halides, perovskites, NASICONs, garnets and other types. Among them, NASICON solid electrolytes have the advantages of high conductivity, good thermal stability, and a wide electrochemical window, making them one of the solid electrolytes with the greatest industrialization potential. At present, the ionic conductivity of NASICON solid electrolytes is still relatively low and cannot be used alone in all-solid-state batteries.
[0003] Therefore, the current solid electrolyte related technologies still need to be improved. Summary of the invention
[0004] This application is based on the inventor's discovery and understanding of the following facts and problems:
[0005] At present, the ionic conductivity of solid electrolytes is one of the main factors limiting their practical application. In order to effectively improve its ionic conductivity, researchers often use wet chemical reaction methods such as hydrothermal method and sol-gel method to improve performance, but they cannot produce at low cost and on a large scale. Although traditional solid-phase reactions are widely used, NASICON solid electrolytes are sensitive to temperature and are prone to the problem of impurity generation due to uneven mixing of raw materials. It is difficult to prepare fine-grained and dense sintered bodies through solid-phase reactions, which in turn affects the energy density of solid-state batteries.
[0006] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention provides a solid electrolyte which is easy to operate, highly controllable, easy to mass produce or has high ion conductivity, and a preparation method thereof, a positive electrode material, a battery and an electrical device.
[0007] In a first aspect of the present application, the present application provides a solid electrolyte. According to an embodiment of the present application, the solid electrolyte comprises a NASICON solid electrolyte; in an X-ray diffraction spectrum of the solid electrolyte, a crystal plane along <012> Preferred orientation, the peak intensity ratio of (012) peak to (113) peak I (012) / I (113) The half-peak width F of the strongest peak (113) is 22% to 25%. (113) It is 0.3°~0.6°.
[0008] Specifically, when the above peak intensity ratio is achieved, it indicates that the diffraction peak of the dominant crystal plane (012) for active ion diffusion is stronger, that is, the solid electrolyte has a dominant crystal plane for active ion diffusion, thereby significantly improving the ionic conductivity of the solid electrolyte. The half-peak width of the strongest peak (113) is within the above range, indicating that the characteristic peak has been broadened, and the solid electrolyte has a high degree of amorphization, which can construct a large number of 3D fast ion transmission channels in the lattice, shorten the distance between active ion transmission sites, and thus improve the ionic conductivity of the solid electrolyte.
[0009] According to an embodiment of the present application, in the X-ray diffraction spectrum of the solid electrolyte, the peak intensity of the strongest peak (113) is 300 to 900. In the X-ray diffraction spectrum of the solid electrolyte, the peak intensity of the strongest peak (113) is within the above range, and the peak intensity value is relatively low, indicating that the solid electrolyte has a high degree of amorphization, which is conducive to constructing active ion transmission channels, thereby improving the ionic conductivity of the solid electrolyte.
[0010] According to an embodiment of the present application, the lattice constant range of the solid electrolyte is The above lattice constants also indicate that the material has obvious amorphous characteristics and can effectively improve its ionic conductivity.
[0011] According to an embodiment of the present application, the solid electrolyte comprises: a core, the core comprising the NASICON solid electrolyte; and a carbon layer, the carbon layer coated on at least a portion of the surface of the core. Coating the carbon layer on the surface of the NASICON solid electrolyte can achieve the construction of an electron transmission channel on the surface of the solid electrolyte, thereby improving the electronic conductivity of the solid electrolyte.
[0012] According to an embodiment of the present application, the solid electrolyte satisfies at least one of the following conditions:
[0013] Carbon content is 0.2% to 1.5%;
[0014] The specific surface area is 30m 2 / g~100m 2 / g;
[0015] The electronic conductivity is 5×10 -4 S / cm~7×10 -4 S / cm;
[0016] The ionic conductivity is 2×10 -3 S / cm~8×10 -3 S / cm.
[0017] According to an embodiment of the present application, the NASICON solid electrolyte includes a compound represented by the following formula 1 or a compound represented by the following formula 2:
[0018] Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 Formula 1
[0019] Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 @vC formula 2
[0020] Among them, M 1 including at least one alkali metal other than lithium;
[0021] M 2 including at least one metal element having a valence state of +3;
[0022] M 3 including at least one metal element having a valence state of +4;
[0023] M 4 including at least one metal element having a valence state of +5;
[0024] R comprises at least one polyanionic element having a valence state of +4;
[0025] 0.05≤x<1, 1≤y<1.5, 0.05≤z<0.5, 0.01≤v≤2, 0.1≤u≤1.
[0026] According to the embodiments of the present application, M 1 including at least one of Na and K;
[0027] M 2 Including at least one of Al, Ga, In, Y, and Sc;
[0028] M 3 Includes at least one of Ti, Zr, Hf, and Ge;
[0029] M4 Includes at least one of V, Nb, Ta, and Bi;
[0030] R includes at least one of Si and S.
[0031] With the above chemical formula, element M 1 For Li doping, element M 2 、M 4 To M 3 By doping the element R at the P site to achieve high entropy doping, the crystallinity of the solid electrolyte can be reduced in the crystal structure, the amorphous characteristics become obvious, and the production of advantageous crystal planes for ion diffusion can be induced, thereby effectively improving the ionic conductivity of the solid electrolyte.
[0032] The second aspect of the present application provides a method for preparing the solid electrolyte described above. According to an embodiment of the present application, the method comprises: 2 Source, M 3 Source, M 4 The R source and the first solvent are mixed, and the obtained raw material mixture is spray pyrolyzed to obtain a precursor; the precursor is mixed with M 1 The precursor mixture is sintered to obtain a NASICON solid electrolyte.
[0033] The preparation method of the high entropy solid electrolyte provided in the present application does not require the use of complexing agents and chelating agents. The raw material elements of the high entropy solid electrolyte are uniformly mixed at the atomic level in the solution, and the solvent is quickly removed and a chemical reaction occurs at a high temperature to avoid the segregation of the elements. The obtained precursor has uniform composition, stable phase and high reaction activity. This method is simpler and more efficient, the sintering temperature is greatly reduced, and the obtained solid electrolyte has a higher ionic conductivity.
[0034] According to an embodiment of the present application, the spray pyrolysis satisfies at least one of the following conditions: the spray feed rate is 2 mol / min to 5 mol / min; the nozzle pressure is 0.4 MPa to 0.6 MPa; the inlet air temperature is 800°C to 1000°C; and the outlet air temperature is 700°C to 900°C.
[0035] According to an embodiment of the present application, the particle size of the precursor is 0.5 micrometer to 1 micrometer.
[0036] According to an embodiment of the present application, the sintering temperature is 600°C to 850°C, preferably 650°C to 750°C; the sintering duration is 4 hours to 12 hours, preferably 6 hours to 8 hours; and the sintering atmosphere is an oxygen-containing atmosphere.
[0037] According to an embodiment of the present application, the method for preparing a solid electrolyte further includes: mixing the NASICON solid electrolyte, a carbon source and a second solvent to obtain a slurry; and drying and dissociating the slurry to obtain the solid electrolyte.
[0038] According to an embodiment of the present application, the method satisfies at least one of the following conditions: the carbon source includes at least one of carbon nanotubes and graphene; and the particle size of the carbon source is 50 nm to 200 nm.
[0039] According to an embodiment of the present application, the second solvent includes at least one of acetone, cyclohexane, toluene, and ethanol.
[0040] According to the embodiment of the present application, the average particle size D of the slurry is V 50 is 5 nm to 500 nm, preferably 10 nm to 100 nm.
[0041] According to an embodiment of the present application, the method satisfies at least one of the following conditions: 1 Source, M 2 Source, M 3 Source, M 4 The source and R source independently include at least one of chloride, nitrate, oxalate, organic alcohol salt, and carbonate; the first solvent includes at least one of water, N-methyl-2-pyrrolidone, ethanol, isopropanol, acetonitrile, etc.; the lithium-containing raw material includes at least one of lithium hydroxide, lithium carbonate, lithium chloride, and lithium nitrate.
[0042] In the third aspect of the present application, a positive electrode material is provided. According to an embodiment of the present application, the positive electrode material includes a substrate; a coating layer, the coating layer is coated on at least part of the outer surface of the substrate, and the coating layer includes the solid electrolyte described above. The surface of the positive electrode material is constructed with a high-entropy solid electrolyte with a stable structure, and at the same time, an electron transmission channel is taken into account, so the powder resistance and DC internal resistance DCR are lower, and the capacity and rate performance in the solid-state battery are better.
[0043] According to an embodiment of the present application, based on the mass of the matrix, the mass percentage of the solid electrolyte is 0.05% to 1.00%.
[0044] According to an embodiment of the present application, the matrix layered oxide positive electrode material is at least one of a layered oxide positive electrode material and a phosphate positive electrode material; the layered oxide positive electrode material includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese base and their derivatives; the phosphate positive electrode material includes at least one of lithium iron phosphate and lithium iron manganese phosphate.
[0045] The present application also provides a method for preparing the aforementioned positive electrode material. According to an embodiment of the present application, the method comprises: mixing the aforementioned solid electrolyte with a matrix, and heat treating the obtained mixture to obtain the positive electrode material. The method is easy to operate and fast, and the obtained positive electrode material powder resistance and DC internal resistance DCR are low, and the capacity and rate performance in the solid-state battery are better.
[0046] According to an embodiment of the present application, the temperature of the heat treatment is 300° C. to 600° C.; the duration of the heat treatment is 4 hours to 10 hours; and the atmosphere of the heat treatment is a non-oxygen-containing atmosphere.
[0047] In a fourth aspect of the present application, a battery is provided. According to an embodiment of the present application, the battery includes the solid electrolyte described above, or the positive electrode material described above. The battery has all the features and advantages of the solid electrolyte described above or the positive electrode material described above, and has a higher energy density, better rate performance and cycle performance.
[0048] In a fifth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the battery described above. The electric device has all the features and advantages of the battery described above, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is the XRD spectrum of the precursors prepared in Example 1 and Comparative Example 2 of the present application.
[0050] Figure 2 It is the XRD spectra of the solid electrolytes prepared in Example 1 and Comparative Example 2 of the present application.
[0051] Figure 3 This is a SEM photograph of the solid electrolyte prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0052] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0053] In a first aspect of the present application, the present application provides a solid electrolyte. According to an embodiment of the present application, the solid electrolyte comprises a NASICON solid electrolyte; in an X-ray diffraction spectrum of the solid electrolyte, a crystal plane along <012> Preferred orientation, the peak intensity ratio of (012) peak to (113) peak I (012) / I (113) The half-peak width F of the strongest peak (113) is 22% to 25%. (113)is 0.3°~0.6°. Specifically, I (012) / I (113) It can be 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, etc. The above peak intensity ratio indicates that the diffraction peak of the dominant crystal plane (012) for active ion diffusion is stronger, that is, the solid electrolyte has a dominant crystal plane for active ion diffusion, so that the ionic conductivity of the solid electrolyte is significantly improved. Specifically, the half-peak width F of the strongest peak (113) is (113) It can be 0.3°, 0.31°, 0.32°, 0.33°, 0.34°, 0.35°, 0.36°, 0.37°, 0.38°, 0.39°, 0.4°, 0.41°, 0.42°, 0.43°, 0.44°, 0.45°, 0.46°, 0.47°, 0.48°, 0.49°, 0.5°, 0.51°, 0.52°, 0.53°, 0.54°, 0.55°, 0.56°, 0.57°, 0.58°, 0.59°, 0.6°, etc. The half-width of the strongest peak (113) is within the above range, indicating that the characteristic peak has been broadened. The solid electrolyte has a high degree of amorphization, and a large number of 3D fast ion transport channels can be constructed in the lattice, shortening the distance between active ion transport sites, thereby improving the ionic conductivity of the solid electrolyte.
[0054] According to an embodiment of the present application, in the X-ray diffraction spectrum of the solid electrolyte, the peak intensity I of the strongest peak (113) is (113) is 300 to 900. Specifically, the peak intensity I of the strongest peak (113) is (113) It can be 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900 and so on.
[0055] In the X-ray diffraction spectrum of the solid electrolyte, the peak intensity of the strongest peak (113) is within the above range. The peak intensity value is relatively low, indicating that the solid electrolyte has a high degree of amorphization, which is conducive to the construction of active ion transmission channels, thereby improving the ionic conductivity of the solid electrolyte.
[0056] According to an embodiment of the present application, the lattice constant range of the solid electrolyte is The above lattice constants also indicate that the material has obvious amorphous characteristics and can effectively improve its ionic conductivity.
[0057] In this paper, the X-ray diffraction spectrum of the solid electrolyte can be detected by the following method: put the sample powder into the glass sample preparation table, put the glass into the Rigaku device, use the Cu target Kα spectrum, set the sample 2θ angle scanning range to 10°-70° at a scanning speed of 0.02° / min, and read the scanning value. Among them, the (013) peak is the strongest peak, and the corresponding 2θ is generally about 24.5°. The (012) crystal plane is the dominant crystal plane for active ion diffusion, and the corresponding 2θ is generally about 14.7°. The peak intensity and half-peak width of the (013) peak and the (012) peak, as well as the lattice constant, can be obtained by reading the XRD test raw data using jade software.
[0058] According to an embodiment of the present application, the solid electrolyte includes: a core, the core including the NASICON-type solid electrolyte; and a carbon layer, the carbon layer coating at least a portion of the surface of the core.
[0059] According to the embodiments of the present application, a carbon layer is coated on the outer surface of a NASICON-type solid electrolyte, so that an electron transmission channel can be constructed on the surface of the solid electrolyte, thereby improving the electronic conductivity of the solid electrolyte; at the same time, the carbon layer coating can also improve the surface morphology of the solid electrolyte, so that it has a more suitable specific surface area.
[0060] In some embodiments, the solid electrolyte satisfies at least one of the following conditions: the carbon content is 0.2% to 1.5%. The specific surface area is 30m 2 / g~100m 2 / g; the electronic conductivity is 5×10 -4 S / cm~7×10 -4 S / cm; ionic conductivity is 2×10 -3 S / cm~8×10 -3 S / cm.
[0061] In this article, the surface morphology of the solid electrolyte can be observed by a transmission electron microscope to verify whether there is a carbon layer on the surface of the solid electrolyte; the presence of a carbon layer and the carbon content in the solid electrolyte can also be detected using a carbon-sulfur analyzer.
[0062] In this article, the specific surface area of the solid electrolyte can be tested by the nitrogen adsorption-desorption method, and the specific test can be carried out in accordance with GBT19587-2004.
[0063] In this paper, the electronic conductivity of solid electrolytes can be measured in a compaction density meter using the four-terminal method.
[0064] In this paper, the ionic conductivity of the solid electrolyte can be detected by pressing the solid electrolyte into a ceramic sheet using an electrochemical workstation using the EIS method.
[0065] In some specific embodiments, the carbon content of the solid electrolyte can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc. With the above carbon content, the coating effect is better, and the conductivity of the solid electrolyte can be effectively improved. When the solid electrolyte is used to coat the positive electrode material or coated on the diaphragm, the interface resistance between the positive electrode material or the diaphragm and the solid electrolyte can be significantly reduced, and the solid-state battery rate performance can be improved. When the coating amount is too low, the effect is not obvious. When the carbon coating is too high, the carbon layer may hinder the transmission of lithium ions, which in turn affects the performance of the solid-state battery.
[0066] In some specific embodiments, the specific surface area of the solid electrolyte can be 30 m 2 / g, 40m 2 / g, 50m 2 / g, 60m 2 / g, 70m 2 / g, 80m 2 / g, 90m 2 / g、100m 2 / g, etc. With the above specific surface area, the activity of the solid electrolyte can be improved. When coating the positive electrode material or coating on the separator, a small amount of solid electrolyte can achieve uniform and dense coating. When the specific surface area is too low, the activity may be low. When coating or coating, the amount of solid electrolyte used may be too large, resulting in a decrease in battery energy density; when the specific surface area is too large, the dispersibility and processing performance of the solid electrolyte may deteriorate.
[0067] In some specific embodiments, the electronic conductivity of the solid electrolyte can be 5×10 -4 S / cm, 5.2×10 -4 S / cm, 5.5×10 -4 S / cm, 5.8×10 -4 S / cm, 6×10 -4 S / cm, 6.2×10 -4 S / cm, 6.5×10 -4 S / cm, 6.8×10 - 4 S / cm, 7×10 -4 S / cm, etc. With the above electronic conductivity, the conductivity of the solid electrolyte can be effectively improved. When the solid electrolyte is used to coat the positive electrode material or coated on the diaphragm, the interface resistance between the positive electrode material or the diaphragm and the solid electrolyte can be significantly reduced, and the rate performance of the solid-state battery can be improved. When the electronic conductivity is low, the effect is not obvious. When the electronic conductivity is too high, it may mean that the carbon layer is too thick, which will hinder the transmission of lithium ions and affect the performance of the solid-state battery.
[0068] In some specific embodiments, the ionic conductivity of the solid electrolyte may be 2×10 -3 S / cm, 2.5×10 -3 S / cm, 3×10 -3 S / cm, 3.5×10 -3 S / cm, 4×10 -3 S / cm, 4.5×10 -3 S / cm, 5×10 -3 S / cm, 5.5×10 -3 S / cm, 6×10 -3 S / cm, 6.5×10 -3 S / cm, 7×10 -3 S / cm, 7.5×10 -3 S / cm, 8×10 -3 S / cm, etc. With the above ionic conductivity, when the solid electrolyte is used in batteries, coated with positive electrode materials or coated on separators, it can effectively improve the capacity and rate performance of positive electrode materials in solid-state batteries, effectively reduce interface impedance, improve battery temperature rise, and improve solid-state battery cycle performance.
[0069] According to an embodiment of the present application, the solid electrolyte includes a compound represented by the following formula 1 or a compound represented by the following formula 2:
[0070] Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 Formula 1
[0071] Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 @vC formula 2
[0072] Among them, M 1 including at least one alkali metal other than lithium;
[0073] M 2including at least one metal element having a valence state of +3;
[0074] M 3 including at least one metal element having a valence state of +4;
[0075] M 4 including at least one metal element having a valence state of +5;
[0076] R comprises at least one polyanionic element having a valence state of +4;
[0077] 0.05≤x<1, 1≤y<1.5, 0.05≤z<0.5, 0.01≤v≤2, 0.1≤u≤1.
[0078] In some specific embodiments, in the above formula 1 and formula 2, M 1 Including at least one of Na and K; M 2 Includes at least one of Al, Ga, In, Y, and Sc; M 3 Includes at least one of Ti, Zr, Hf, and Ge; M 4 Includes at least one of V, Nb, Ta, and Bi; R includes at least one of Si and S.
[0079] In some specific embodiments, in the above formula 1 and formula 2, x can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, etc.; y can be 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.49, etc.; z can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0. 3, 0.4, 0.5, etc.; v can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, etc.; u can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, etc.
[0080] According to the solid electrolyte of the embodiment of the present application, high entropy elements are introduced into the solid electrolyte to adjust the lattice constant, wherein the element M 1 For Li doping, element M 2 、M 4 To M 3Site doping, element R doping on P site, that is, introducing a variety of high entropy cations inside the lattice, the solid electrolyte is replaced by ions of different radii at different ion sites, making the unit cell of the original orderly distribution structure of each element appear microscopically ordered but macroscopically disordered, thereby reducing the crystallinity of the solid electrolyte in the crystal structure, and the amorphous characteristics become obvious; in the microstructure, the unit cell is distorted due to the substitution of ions of different radii, shortening the distance between active ion transport sites, inducing the generation of advantageous crystal planes that are conducive to active ion transport, thereby effectively reducing the active ion migration energy barrier, and constructing a large number of 3D fast ion transport channels in the lattice, enabling it to quickly percolate along energy-favorable paths, thereby achieving the purpose of improving ionic conductivity.
[0081] In a second aspect of the present application, a method for preparing the solid electrolyte described above is provided. According to an embodiment of the present application, the method comprises:
[0082] S10: Phosphorus source, M 2 Source, M 3 Source, M 4 The source, R source and the first solvent are mixed, and the obtained raw material mixture is spray pyrolyzed to obtain a precursor.
[0083] Spray pyrolysis is a method in which a metal salt solution is sprayed into a high-temperature atmosphere in a mist form to directly obtain metal or oxide powders through evaporation of the solvent and thermal decomposition of the metal salt.
[0084] In this step, the spray pyrolysis method allows the elements in the raw material mixture to be uniformly mixed at the atomic level, achieving multi-site doping of the solid electrolyte, thereby constructing a large number of 3D fast ion transmission channels in the lattice, so that the prepared solid electrolyte has uniform composition, an average particle size of nanometers, a high degree of amorphization, and a stronger diffraction peak of the dominant crystal plane of ion diffusion, thereby improving ionic conductivity. And this method is simple to operate, highly controllable, and easy to mass produce.
[0085] According to the embodiments of the present application, the spray feed rate of spray pyrolysis is 2 mol / min to 5 mol / min, such as 2 mol / min, 2.5 mol / min, 3 mol / min, 3.5 mol / min, 4 mol / min, 4.5 mol / min, 5 mol / min and the like.
[0086] According to the embodiments of the present application, the nozzle pressure of spray pyrolysis is 0.4MPa~0.6MPa, specifically 0.4MPa, 0.41MPa, 0.42MPa, 0.43MPa, 0.44MPa, 0.45MPa, 0.46MPa, 0.47MPa, 0.48MPa, 0.49MPa, 0.5MPa, 0.51MPa, 0.52MPa, 0.53MPa, 0.54MPa, 0.55MPa, 0.56MPa, 0.57MPa, 0.58MPa, 0.59MPa, 0.6MPa and the like.
[0087] According to the embodiments of the present application, the inlet temperature of spray pyrolysis is 800°C to 1000°C; the outlet temperature is 700°C to 900°C; specifically, the inlet temperature can be 800°C, 850°C, 900°C, 950°C, 1000°C, etc.; the outlet temperature can be 700°C, 750°C, 800°C, 850°C, 900°C, etc.
[0088] Specifically, the above-mentioned feed rate and nozzle pressure mainly affect the size of the droplets sprayed by the nozzle. The faster the feed rate and the smaller the nozzle pressure, the larger the droplets sprayed by the nozzle, and vice versa. If the droplets are too large, the drying speed will be slower, and problems such as component segregation, internal structure collapse, particle breakage, relatively poor strength and sphericity may occur. The above-mentioned inlet temperature and outlet temperature mainly affect the drying speed of the droplets sprayed by the nozzle. Similarly, if the drying speed is too slow, problems such as component segregation, internal structure collapse, particle breakage, relatively poor strength and sphericity may occur.
[0089] The present application controls the parameters of spray pyrolysis within the above range, and can obtain droplets of suitable size, which can be quickly dried after being sprayed from the nozzle, so that the obtained solid electrolyte has uniform composition and better performance.
[0090] According to an embodiment of the present application, the temperature of the spray pyrolysis reaction is 450°C to 1000°C. In some embodiments, the temperature of the spray pyrolysis reaction is 500°C to 900°C. In other embodiments, the temperature of the spray pyrolysis reaction is 600°C to 800°C. Specifically, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, etc.
[0091] It should be noted that the temperature of the above-mentioned spray pyrolysis reaction refers to the temperature in the pyrolysis chamber, which depends on the feed rate, air inlet temperature and air outlet temperature. Within the above-mentioned temperature range, it is conducive to obtaining a solid electrolyte with obvious amorphous characteristics and a crystal surface with obvious active ion diffusion advantages.
[0092] According to the embodiment of the present application, the particle size of the precursor is 0.5 micron to 1 micron, specifically 0.5 micron, 0.6 micron, 0.7 micron, 0.8 micron, 0.9 micron, 1 micron, etc. In this particle size range, the precursor has a high reactivity, which is conducive to the subsequent steps; at the same time, it is conducive to the uniform mixing of the elements in the solid electrolyte, and a solid electrolyte with obvious amorphous characteristics and a clear active ion diffusion advantage crystal surface is obtained.
[0093] In this paper, the particle size of the precursor refers to D v The 50 particle size, i.e. the volume distribution particle size, refers to the particle size corresponding to 50% of the cumulative volume, which can be specifically detected by a laser particle size analyzer.
[0094] It can be understood that in this step, the specific raw materials in the raw material mixture can be flexibly selected and adjusted according to the specific composition of the solid electrolyte, and the specific raw material compound can be selected according to the chemical formula of the target solid electrolyte, and the corresponding raw materials can be weighed according to the stoichiometric ratio in the chemical formula. For example, the specific raw materials can be chlorides, nitrates, oxalates, organic alcohol salts or carbonates of the corresponding elements in the solid electrolyte.
[0095] In some embodiments, the M 1 Source, M 2 Source, M 3 Source, M 4 The source and R source each independently include at least one of chloride, nitrate, oxalate, organic alcohol salt, and carbonate. In some embodiments, the raw material mixture includes M 2 、M 3 、M 4 , chloride, nitrate, oxalate, organic alcohol salt or carbonate of R element; wherein M 2 、M 3 、M 4 , R are consistent with the previous description and will not be described in detail here.
[0096] As mentioned above, spray pyrolysis is performed on a salt solution, and the raw material mixture is provided in the form of a solution, that is, the raw material mixture includes a first solvent. In some embodiments, the first solvent includes at least one of water, N-methyl-2-pyrrolidone, ethanol, isopropanol, acetonitrile, etc. Thus, the corresponding raw materials can be well dispersed, which is conducive to obtaining a solid electrolyte with uniform composition and better performance.
[0097] In some specific embodiments, this step can be performed by the following steps:
[0098] S11: Phosphorus source, M 2 Source, M 3 Source, M 4Source and R source are dissolved in a first solvent according to the chemical formula ratio of the solid electrolyte described above to obtain a mixture A;
[0099] S12: Spraying the mixed material A into a pyrolysis chamber at 450° C. to 1000° C. through a spray gun of a spray pyrolysis device to react and obtain a high entropy solid electrolyte precursor B.
[0100] Thus, the obtained precursor has obvious crystallization diffraction characteristic peaks at 2θ of 29.5±0.1°, 31.0±0.1°, and 48.1±0.1°, indicating that it has a better active ion diffusion dominant crystal plane.
[0101] In this step, the doping elements are introduced during the mixing process of the raw material solution to make the doping more uniform. In addition, by adjusting the raw material ratio, different positions of Li, P and transition metals in the solid electrolyte are doped with different degrees of elements. The obtained solid electrolyte has obvious amorphous characteristics and has obvious active ion diffusion advantage crystal plane, and the ion conductivity is significantly improved.
[0102] S20: mixing the precursor with M 1 The precursor mixture is sintered to obtain a NASICON solid electrolyte.
[0103] According to an embodiment of the present application, the lithium-containing raw material may specifically include at least one of lithium hydroxide, lithium carbonate, lithium chloride, and lithium nitrate.
[0104] According to the embodiments of the present application, the amount of lithium-containing raw material added can be calculated based on the chemical calculation ratio in the chemical formula of the solid electrolyte, which will not be elaborated here.
[0105] According to an embodiment of the present application, the sintering temperature may be 600°C to 850°C; in some embodiments, the sintering temperature may be 650°C to 750°C, such as 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, etc.
[0106] According to an embodiment of the present application, the sintering duration may be 4 to 12 hours; in some embodiments, the sintering duration may be 6 to 8 hours; specifically, such as 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, etc.
[0107] According to an embodiment of the present application, the sintering atmosphere is an oxygen-containing atmosphere, such as air or oxygen.
[0108] Under the above sintering conditions, the reaction is fully carried out and the reaction efficiency is high. At the same time, the obtained NASICON solid electrolyte has high ion conductivity.
[0109] In some embodiments, this step can be performed by:
[0110] The solid electrolyte precursor B is mixed with lithium-containing raw materials, M 1 Source according to M 3 :Li:M 1 =y:(3-xy-2z+u):x, and the mixture is uniformly mixed to obtain a powder, which is then sintered in a certain atmosphere and temperature to obtain a micron-sized high-entropy NASICON solid electrolyte. 1 、M 3 , x, y, z, and u are consistent with the previous description and will not be described in detail here.
[0111] According to an embodiment of the present application, the NASICON type solid electrolyte may also be carbon coated, and thus, the above method for preparing the solid electrolyte may further include:
[0112] S30: mixing the NASICON solid electrolyte, the carbon source and the second solvent to obtain a slurry, and drying and dissociating the slurry to obtain the solid electrolyte.
[0113] In this step, by introducing a carbon source during the nano-scaling process of the high-entropy solid electrolyte, an electron transmission channel can be constructed on the surface of the solid electrolyte, effectively improving the electronic conductivity of the solid electrolyte.
[0114] According to an embodiment of the present application, the carbon source includes at least one of carbon nanotubes and graphene; the particle size of the carbon source is 50nm to 200nm (specifically, 50nm, 80nm, 100nm, 120nm, 150nm, 180nm, 200nm, etc.). Thus, a dense and uniform coating of the solid electrolyte can be achieved with a small amount.
[0115] According to an embodiment of the present application, the second solvent includes at least one of acetone, cyclohexane, toluene, and ethanol. Thus, the slurry can minimize the degree of agglomeration during the drying process and achieve better dispersibility.
[0116] According to the embodiment of the present application, the average particle size D of the slurry is v 50 is 5 nm to 500 nm; in some embodiments, the average particle size D of the slurry v 50 is 10 nm to 100 nm, such as 5 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 50 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, etc. Thus, a solid electrolyte with a small particle size and uniform composition can be obtained.
[0117] According to the embodiments of the present application, the drying can be performed by at least one of spray drying, blast drying, vacuum drying and freeze drying, thereby achieving high efficiency and good drying effect.
[0118] According to the embodiments of the present application, the dissociation specifically includes separating the single nanoparticles in the agglomerated particles by using at least one device selected from the group consisting of a colloid mill, a mechanical mill, and a jet mill to achieve better dispersibility. That is, in this step, the secondary particles formed by the agglomeration of multiple primary particles can be disaggregated to form primary particles that are substantially not agglomerated.
[0119] The preparation method of the high entropy solid electrolyte provided in the present application is a spray pyrolysis method. Compared with the sol-gel method, the spray pyrolysis method does not require the use of complexing agents and chelating agents. The raw material elements of the high entropy solid electrolyte are uniformly mixed at the atomic level in the solution, and the solvent is quickly removed and a chemical reaction occurs under high temperature conditions to avoid element segregation. The resulting precursor has uniform composition, stable phase and high reaction activity.
[0120] Compared with the solid-state reaction method, this method is simpler and more efficient, and the phase composition of the powder can be adjusted by the proportion of the precursor. Based on the nano-particle size, the sintering temperature is greatly reduced, and fine-grained and dense bulk and thin-film solid electrolytes can be prepared at a sintering temperature 100℃ to 200℃ lower than that of the solid-state reaction method.
[0121] According to the method of the embodiment of the present application, the spray pyrolysis process reduces the size of the precursor particle size by controlling parameters such as temperature, pressure and feed rate, thereby increasing the activity of the grains and reducing the difficulty of phase formation, thereby forming crystals with advantageous crystal faces in the precursor stage, effectively reducing the solid electrolyte phase formation temperature, which also contributes to the amorphization in the solid electrolyte synthesis stage, and improves the ionic conductivity by the formation of an amorphous structure. In addition, the introduction of a carbon coating layer during the nano-process of the solid electrolyte can further improve its electronic conductivity. Thus, the prepared solid electrolyte has both good ionic conductivity and electronic conductivity.
[0122] In the third aspect of the present application, a positive electrode material is provided. According to an embodiment of the present application, the positive electrode material includes a substrate; a coating layer, the coating layer is coated on at least part of the outer surface of the substrate, and the coating layer includes the solid electrolyte described above. The surface of the positive electrode material is constructed with a high-entropy solid electrolyte with a stable structure, and at the same time, an electron transmission channel is taken into account, so the powder resistance and DC internal resistance DCR are lower, and the capacity and rate performance in the solid-state battery are better.
[0123] According to an embodiment of the present application, based on the mass of the substrate, the mass percentage of the solid electrolyte is 0.05% to 1.00%, specifically 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc. Within this content range, the substrate can be well coated without causing the coating layer to be too thick and easy to fall off or affect the capacity.
[0124] According to an embodiment of the present application, the matrix includes at least one of a layered oxide positive electrode material and a phosphate positive electrode material; specifically, the layered positive electrode material includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese base and their derivatives; the phosphate positive electrode material includes at least one of lithium iron phosphate and lithium iron manganese phosphate.
[0125] In some embodiments, the aforementioned positive electrode material can be prepared by the following method: mixing the aforementioned solid electrolyte with a matrix, and subjecting the obtained mixture to a heat treatment to obtain the positive electrode material.
[0126] According to the embodiments of the present application, the specific method of mixing the aforementioned solid electrolyte with the matrix is not particularly limited and can be selected according to actual needs. In some embodiments, the aforementioned solid electrolyte and the aforementioned solid electrolyte matrix can be mixed in a mass ratio of 0.05:100 to 1:100 using at least one mixing device selected from a ball mill, a high mixer, a vertical mixer, a horizontal mixer, and an oblique mixer. As a result, the mixing is more uniform and the efficiency is higher.
[0127] According to the embodiments of the present application, the temperature of the heat treatment is 300°C to 600°C (specifically 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc.); the duration of the heat treatment is 4 hours to 10 hours (specifically 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, etc.); the atmosphere of the heat treatment is a non-oxygen atmosphere (specifically nitrogen, argon, etc.). Under the above conditions, the solid electrolyte can be well coated on the surface of the substrate to obtain a positive electrode material with low powder resistance and DC internal resistance DCR, and good capacity and rate performance in solid-state batteries.
[0128] According to the embodiments of the present application, the heat treatment can be performed in any heating device of a tubular furnace, an atmosphere furnace, a muffle furnace and a roller kiln, thereby making the operation convenient and fast, and facilitating large-scale production.
[0129] In a fourth aspect of the present application, a battery is provided. According to an embodiment of the present application, the battery comprises the solid electrolyte described above, or the positive electrode material described above. The battery has a high energy density, good rate performance and cycle performance.
[0130] It can be understood that there is no particular limitation on the specific type of the above-mentioned battery, which may be a solid-state battery, a semi-solid-state battery or a liquid battery; and the above-mentioned battery includes but is not limited to a lithium-ion battery, a lithium metal battery, and the like.
[0131] In some embodiments, the above-mentioned battery is a solid-state battery, which includes the solid electrolyte described above. In this case, the solid electrolyte can be used as an electrolyte in the battery, for example, it can be arranged between the positive electrode and the negative electrode to isolate the positive electrode and the negative electrode while allowing active ions to pass through.
[0132] In some other embodiments, the battery includes the positive electrode material described above. In this case, the electrolyte in the battery may be a solid electrolyte, a semi-solid electrolyte or an electrolyte.
[0133] It is understood that the battery generally includes an outer package and an electrode assembly and an electrolyte contained in the outer package, wherein the electrode assembly generally includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet (the separator in the solid-state battery can be replaced with a solid electrolyte). The positive electrode sheet generally includes a positive electrode collector and a positive electrode film layer located on at least one surface of the positive electrode collector, and the positive electrode film layer includes the positive electrode material, conductive agent, binder, and optional functional additives described above. In some embodiments, the negative electrode sheet may include a negative electrode collector and a negative electrode film layer located on at least one surface of the negative electrode collector, and the negative electrode film layer includes a negative electrode material, conductive agent, binder, and optionally functional additives. In other embodiments, the negative electrode sheet may also be a lithium metal sheet, or a structure in which a lithium metal foil is loaded on the surface of the substrate.
[0134] In a fifth aspect of the present application, an electric device is provided. According to an embodiment of the present application, the electric device includes the battery described above. The electric device has all the features and advantages of the battery described above, which will not be described in detail here.
[0135] According to an embodiment of the present application, the battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0136] The embodiments of the present application are described in detail below.
[0137] Example 1
[0138] AlCl3, TiOCl2, NbOCl3, H2SiO3, and NH4H2PO4 were weighed according to the stoichiometric ratio of Al:Ti:Nb:Si:P=0.6:1.3:0.1:1:2, and a certain amount of pure water was added to dissolve and form a stable aqueous solution A;
[0139] The aqueous solution A was sprayed into the pyrolysis chamber through the spray gun of the spray pyrolysis device for reaction, and the spray feed rate was controlled to be 4 mol / min, the nozzle pressure was controlled to be 0.5 MPa, the inlet temperature was controlled to be 1000°C, and the outlet temperature was controlled to be 900°C. The average particle size D was collected. v 50 is a solid electrolyte precursor B powder with a particle size of 0.5 microns.
[0140] Li2CO3 and Na2CO3 were weighed according to the stoichiometric ratio of Li:Na:P=1.7:0.8:2, and the solid electrolyte precursor B was ground and mixed with the weighed lithium carbonate and sodium carbonate in a sand mill to obtain D v The powder obtained after spray drying was sintered at 800°C for 6h in air atmosphere to obtain a high entropy NASICON solid electrolyte with the chemical formula of Li 1.7 Na 0.8 Al 0.6 Ti 1.3 Nb 0.1 SiP2O 12 The obtained solid electrolyte was mixed with graphene in acetone at a ratio of 99:1 and ground to obtain a slurry, which was then dried and dissociated to obtain a slurry with a chemical formula of Li 1.7 Na 0.8 Al 0.6 Ti 1.3 Nb 0. 1SiP2O 12 @0.01C high entropy NASICON type solid electrolyte.
[0141] The solid electrolyte Li 1.7 Na 0.8 Al 0.6 Ti 1.3 Nb 0.1 SiP2O 12 @0.01C powder with positive electrode material LiNi 0.93 Co 0.05 Mn 0.02 O2 was weighed in a mass ratio of 0.8:100 and put into a high-speed mixer for uniform mixing; the obtained mixture was heat treated at 500°C in a nitrogen atmosphere furnace for 6 hours to obtain Li 1.7Na 0.8 Al 0.6 Ti 1.3 Nb 0.1 SiP2O 12 @0.01C powder coated LiNi 0.93 Co 0.05 Mn 0.02 O2 material.
[0142] The above-mentioned positive electrode material coated with the solid electrolyte was mixed with conductive carbon black, PVDF, and LiTFSI in a mass ratio of 90:3:5:2, and an appropriate amount of NMP was added. After stirring evenly, it was scraped on aluminum foil, dried in a 120℃ forced air oven for 1 hour, and punched into a positive electrode sheet with a diameter of 11mm; PEO (polyethylene oxide) and LiTFSI (substance ratio EO:Li=12:1) were dissolved in acetonitrile, stirred for 12 hours, and the obtained slurry was cast in a polytetrafluoroethylene mold. After vacuum drying in an oven at 50℃ for 10 hours, the PEO electrolyte membrane was placed in a press and hot-pressed for 5 minutes, and then taken out to punch into a circular PEO electrolyte membrane with a diameter of 19mm. With a metallic lithium negative electrode, the prepared positive electrode sheet and PEO electrolyte membrane were assembled into a 2025 button-type all-solid-state battery in an Ar gas glove box with a water content and an oxygen content of less than 5ppm.
[0143] Example 2
[0144] Same as Example 1, except that the doping element Ti is replaced by Hf.
[0145] Example 3
[0146] Same as Example 1, except that the doping element Al is replaced by Y, as shown in Table 1.
[0147] Example 4
[0148] Same as Example 1, except that the doping element Nb is replaced by V, as shown in Table 1.
[0149] Example 5
[0150] Same as Example 1, except that the spray pyrolysis parameters are different, as shown in Table 1.
[0151] Example 6
[0152] Same as Example 1, except that the spray pyrolysis parameters are different, as shown in Table 1.
[0153] Example 7
[0154] Same as Example 1, except that no carbon coating was performed.
[0155] Example 8
[0156] Same as Example 1, except that the PEO electrolyte membrane in the 2025 button-type all-solid-state battery is replaced with the Li 1.7 Na 0.8 Al 0.6 Ti 1.3 Nb 0.1 SiP2O 12 Electrolyte membrane.
[0157] Example 9
[0158] Same as Example 1, except that the sintering parameters are different, see Table 1 for details.
[0159] Example 10
[0160] Same as Example 1, except that the sintering parameters are different, see Table 1 for details.
[0161] Comparative Example 1 (Preparation of a Li 1.3 Al 0.3 Ti 1.7 (PO4)3 solid electrolyte)
[0162] The compounds of Li2CO3, Al2O3, TiO2 and NH4H2PO4 were weighed according to the stoichiometric ratio, mixed in a ball mill mixer at 900 rpm for 6 hours to obtain a mixture; the obtained mixture was pre-sintered at 700°C in a muffle furnace for 2 hours, and the sintered product was crushed at the highest level in a wall breaker for 5 minutes to obtain a powdery solid electrolyte precursor.
[0163] The obtained solid electrolyte precursor was sintered in a muffle furnace at 950°C for 6 hours, and the sintered product was crushed in a jet mill to obtain a powdered solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3.
[0164] The obtained nanoscale solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder with positive electrode material LiNi 0.93 Co 0.05 Mn 0.02 O2 was weighed in a mass ratio of 0.8:100 and put into a high-speed mixer for mixing. The obtained mixture was heat treated at 500°C for 6 hours in an atmosphere furnace to obtain Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder coated LiNi 0.93 Co 0.05 Mn 0.02 O2 material.
[0165] Comparative Example 2 (Preparation of Precursor by High-Temperature Solid Phase Method)
[0166] The same as Example 1, except that the high temperature solid phase method of Comparative Example 1 is adopted for preparation, and there is no carbon coating.
[0167] Comparative Example 3 (Preparation of Li 1.3 Al 0.3 Ti 1.7 (PO4)3 solid electrolyte)
[0168] AlCl3, TiOCl3, and NH4H2PO4 were weighed according to the stoichiometric ratio of Al:Ti:P=0.3:1.7:3, and a certain amount of pure water was added to dissolve and form a stable aqueous solution A; the aqueous solution A was sprayed into the pyrolysis chamber through the spray gun of the spray pyrolysis device for reaction, and the spray feed rate range was controlled to be 6 mol / min, the nozzle pressure range was controlled to be 0.3 MPa, the inlet temperature range was controlled to be 700°C, and the outlet temperature range was controlled to be 500°C. The solid electrolyte precursor B powder with an average particle size Dv50 of 30 microns was collected.
[0169] Li2CO3 was weighed according to the stoichiometric ratio of Li:P=2:1, and the solid electrolyte precursor B and the weighed lithium carbonate were mixed evenly in a high-speed mixer. The obtained powder was sintered at 800°C in an air atmosphere to obtain a high-entropy NASICON solid electrolyte with a chemical formula of Li 1.3 Al 0.3 Ti 1.7 P3O 12 .
[0170] The obtained solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO 4)3 Powder with positive electrode material LiNi 0.93 Co 0.05 Mn 0.02 O2 was weighed in a mass ratio of 0.8:100 and put into a high-speed mixer for mixing. The obtained mixture was heat treated at 500°C for 6 hours in an atmosphere furnace to obtain Li 1.3 Al 0.3 Ti 1.7 P3O 12 Solid electrolyte coated LiNi 0.93 Co 0.05 Mn 0.02 O2 material.
[0171] Comparative Example 4
[0172] Different from Example 1, the doping element does not contain Na.
[0173] Comparative Example 5
[0174] Different from Example 1, the doping element does not contain Nb.
[0175] Comparative Example 6
[0176] Different from Example 1, the doping element does not contain Si.
[0177] Comparative Example 7
[0178] The difference from Example 1 is that the inlet air temperature and outlet air temperature of the spray drying are specifically shown in Table 1.
[0179] Comparative Example 8
[0180] The difference from Example 1 is that the pressure and feed rate of spray drying are shown in Table 1.
[0181] Performance Test:
[0182] 1. XRD test: Place the sample powder on a glass sample preparation table, place the glass sample on the Rigaku device, use the Cu target Kα spectrum, set the sample 2θ angle scanning range to 10°~70° at a scanning speed of 0.02° / min, and read the scanning value.
[0183] 2. Ionic conductivity test: Take 10 grams of each solid electrolyte sample prepared in the above comparative example and embodiment, of which 2 grams are placed in a mold with a diameter of 11 mm, and pressed into a dense disc under a pressure of 100 MPa. The pressed disc is placed in an alumina crucible with a lid, and the disc is evenly covered with the remaining 8 grams of sample powder. Sintered at 1200°C for 8 hours, the disc is taken out and polished to obtain a sintered dense solid electrolyte ceramic sheet. The prepared solid electrolyte ceramic sheet is placed in an electrochemical workstation to test the AC impedance at room temperature, and the frequency is set to 0.01MPa~10MPa. According to the impedance data obtained by the test, the ionic conductivity corresponding to the sample is calculated according to the formula σ=L / RS (σ is conductivity, L is the thickness of the ceramic sheet, R is the impedance value, and S is the area of the ceramic sheet). The test results are shown in Table 2.
[0184] 3. Ionic conductivity test: After the solid electrolyte is pressed into a ceramic sheet, it is tested using the EIS method using an electrochemical workstation.
[0185] 4. Carbon content test: Place the sample in a carbon-sulfur analyzer and heat it to 800°C to burn the carbon in the sample. Analyze the carbon-containing gas content in the combustion product to obtain the carbon content in the sample.
[0186] 5. Specific surface area test: Nitrogen adsorption and desorption method is used, referring to GBT19587-2004 for detection.
[0187] 6. Morphology observation: Place the sample in SEM to characterize the surface morphology of the solid electrolyte.
[0188] 7. Battery performance test:
[0189] The solid-state batteries in the above embodiments and comparative examples were tested for charge and discharge capacity at 3.0V-4.3V, 0.1C, and 60°C. The charge and discharge cycle performance was tested by charging and discharging 50 times at 3.0V-4.3V, 1C, and 60°C. The test results are shown in Table 4.
[0190] Table 1: Solid electrolyte preparation parameters
[0191]
[0192]
[0193]
[0194]
[0195] Table 3: Cathode material parameters
[0196]
[0197]
[0198] Table 4: Battery performance test results
[0199] 0.1C discharge specific capacity / mAh / g 1C cycle 50 weeks capacity retention rate / % Example 1 215 92.9 Example 2 220 93.4 Example 3 214 92.0 Example 4 213 92.1 Example 5 210 90.0 Example 6 212 92.8 Example 7 211 90.3 Example 8 215 92.9 Example 9 210 90.1 Example 10 211 90.2 Comparative Example 1 207 87.8 Comparative Example 2 209 89.2 Comparative Example 3 205 88.6 Comparative Example 4 207 89.0 Comparative Example 5 206 88.7 Comparative Example 6 208 89.2 Comparative Example 7 206 87.5 Comparative Example 8 205 87.2
[0200] From the above test data, it can be seen that by introducing a variety of high entropy doping elements, the solid electrolyte can have obvious amorphous characteristics and <012> The half-width of the (113) peak and I (012) / I (113) The requirements specified in right 1 are met; by comparing examples 1 to 8 with examples 9 to 10, it can be seen that the process conditions of spray pyrolysis have a greater influence on the performance of the product; by comparing example 1 and example 7, it can be seen that carbon coating can significantly improve the electronic conductivity of the solid electrolyte; by comparing the various examples and comparative examples, it can be seen that the doping elements in the solid electrolyte, the precursor preparation process and the process parameters of spray pyrolysis all have a certain influence on the degree of amorphization of the solid electrolyte. The solid-phase sintering method cannot achieve high-entropy doping, the degree of amorphization of the solid electrolyte is low, the number of doping elements is small and the process parameters of spray pyrolysis are not suitable, which is not conducive to achieving high-entropy doping, and the degree of amorphization of the solid electrolyte will also be reduced, and then the ionic conductivity of the solid electrolyte is low, which is not conducive to improving battery performance.
[0201] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0202] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0203] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A solid electrolyte, characterized in that Including NASICON type solid electrolyte; In the X-ray diffraction spectrum of the solid electrolyte, the crystal plane <012> Preferred orientation, the peak intensity ratio of (012) peak to (113) peak I (012) / I (113) The half-peak width F of the strongest peak (113) is 22% to 25%. (113) It is 0.3°~0.6°.
2. The solid electrolyte according to claim 1, characterized in that In the X-ray diffraction spectrum of the solid electrolyte, the lattice constant of the solid electrolyte satisfies:
3. The solid electrolyte according to any one of claims 1 to 2, characterized in that include: A core, the core comprising the NASICON type solid electrolyte; and A carbon layer is coated on at least a portion of the surface of the inner core.
4. The solid electrolyte according to claim 3, characterized in that Satisfy at least one of the following conditions: Carbon content is 0.2% to 1.5%; The specific surface area is 30m 2 / g~100m 2 / g; The electronic conductivity is 5×10 -4 S / cm~7×10 -4 S / cm; The ionic conductivity is 2×10 -3 S / cm~8×10 -3 S / cm.
5. The solid electrolyte according to claim 1, characterized in that Including the compound represented by the following formula 1 or the compound represented by the following formula 2: Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 Formula 1 Li 3-x-y-2z+u M 1 x M 2 2-y-z M 3 y M 4 z P 3-u R u O 12 @vC type 2 Among them, M 1 including at least one alkali metal other than lithium; M 2 including at least one metal element having a valence state of +3; M 3 including at least one metal element having a valence state of +4; M 4 including at least one metal element having a valence state of +5; R comprises at least one polyanionic element having a valence state of +4; 0.05≤x<1, 1≤y<1.5, 0.05≤z<0.5, 0.1≤u≤1, 0.01≤v≤2.
6. The solid electrolyte according to claim 5, characterized in that M 1 including at least one of Na and K; M 2 Including at least one of Al, Ga, In, Y, and Sc; M 3 Includes at least one of Ti, Zr, Hf, and Ge; M 4 Includes at least one of V, Nb, Ta, and Bi; R includes at least one of Si and S.
7. A method for preparing the solid electrolyte according to any one of claims 1 to 6, characterized in that: include: The phosphorus source, M 2 Source, M 3 Source, M 4 The source, the R source and the first solvent are mixed, and the obtained raw material mixture is spray pyrolyzed to obtain a precursor; The precursor and M 1 A source and a lithium-containing raw material are mixed, and the obtained precursor mixture is sintered to obtain the NASICON type solid electrolyte; Among them, M 1 、M 2 、M 3 、M 4 , R as defined in claim 5 or 6.
8. The method according to claim 7, characterized in that The spray pyrolysis satisfies at least one of the following conditions: The spray feed rate is 2mol / min~5mol / min; The nozzle pressure is 0.4MPa~0.6MPa; The air inlet temperature is 800℃~1000℃; The air outlet temperature is 700℃~900℃.
9. The method according to claim 7, characterized in that: The particle size of the precursor is 0.5 micrometer to 1 micrometer; and / or, The sintering temperature is 600°C to 850°C, preferably 650°C to 750°C; and / or, The sintering duration is 4 to 12 hours, preferably 6 to 8 hours; and / or, The sintering atmosphere is an oxygen-containing atmosphere.
10. The method according to any one of claims 7 to 9, characterized in that: Also includes: Mixing the NASICON solid electrolyte, a carbon source and a second solvent to obtain a slurry; The slurry is dried and dissociated to obtain the solid electrolyte.
11. The method according to claim 10, characterized in that Satisfy at least one of the following conditions: The carbon source includes at least one of carbon nanotubes and graphene; The particle size of the carbon source is 50nm to 200nm; The second solvent comprises at least one of acetone, cyclohexane, toluene and ethanol; The average particle size D of the slurry v 50 is 5 nm to 500 nm, preferably 10 nm to 100 nm.
12. The method according to claim 7, characterized in that Satisfy at least one of the following conditions: The M 1 Source, M 2 Source, M 3 Source, M 4 The sources independently include at least one of chloride, nitrate, oxalate, organic alcohol salt, and carbonate; The first solvent includes at least one of water, N-methyl-2-pyrrolidone, ethanol, isopropanol, acetonitrile, etc.; The lithium-containing raw material includes at least one of lithium hydroxide, lithium carbonate, lithium chloride and lithium nitrate.
13. A positive electrode material, characterized in that: include: matrix; A coating layer is coated on at least a portion of the outer surface of the substrate, and the coating layer comprises the solid electrolyte according to any one of claims 1 to 6.
14. The positive electrode material according to claim 13, characterized in that Based on the mass of the matrix, the mass percentage of the solid electrolyte is 0.05% to 1.00%, and / or, The substrate includes at least one of a layered oxide positive electrode material and a phosphate positive electrode material; The layered oxide positive electrode material comprises at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese-based and derivatives thereof; The phosphate positive electrode material includes at least one of lithium iron phosphate and lithium manganese iron phosphate.
15. A battery, characterized in that: The invention comprises the solid electrolyte according to any one of claims 1 to 6, or the positive electrode material according to any one of claims 13 to 14.
16. An electrical device, characterized in that: Comprising the battery as claimed in claim 15.