Electrolyte solution, electrochemical device, and electronic device

By adding lithium tetrafluoroborate and compound of formula I to the electrolyte, a passivation layer rich in S and F elements is formed, which solves the problem of poor stability of the electrolyte for the positive and negative interface protective film, and significantly improves the electrochemical device Low temperature performance and conductivity.

CN119069804APending Publication Date: 2024-12-03NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208219.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The electrolyte has poor stability to the protective film of the positive and negative electrode interface, which affects the high and low temperature performance of the electrochemical device.

Method used

By adding lithium tetrafluoroborate and a specific compound of formula I to the electrolyte, the mass content is adjusted to form a passivation layer rich in S and F elements, improving the stability and ionic conductivity of the electrode plate interface, thereby improving electricity Low temperature discharge performance of chemical devices.

Benefits of technology

It effectively improves the interface stability of the electrode plate and the low-temperature discharge performance of the electrochemical device, improves the impedance and conductivity of the electrochemical device, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069804A_ABST
    Figure CN119069804A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte, an electrochemical device and an electronic device. The electrolyte comprises lithium tetrafluoroborate and a compound # imgabs0 # lithium tetrafluoroborate shown in the formula I, the mass percentage A of the lithium tetrafluoroborate is larger than or equal to 0.1% and smaller than or equal to 2%, the mass percentage B of the compound shown in the formula I is larger than or equal to 0.01% and smaller than or equal to 20%, the lithium tetrafluoroborate and the compound shown in the formula I can form a passivation layer which comprises organic components and inorganic components and is rich in at least one element of B, P or F, the passivation layer is thin and firm, and the passivation layer is not prone to deformation. And the passivation layer exists on a positive electrode interface and / or a negative electrode interface, so that the stability of a corresponding pole piece interface can be effectively improved, the low-temperature impedance of the electrochemical device is improved, and the low-temperature discharge performance of the electrochemical device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrochemical devices, and in particular to an electrolyte, an electrochemical device and an electronic device. Background Art

[0002] Electrochemical devices have the advantages of high energy storage density, high open circuit voltage, low self-discharge rate, long cycle life, and good safety. They are widely used in various fields such as portable energy storage, electronic devices, and electric vehicles. However, higher requirements are also placed on the comprehensive performance of electrochemical devices, such as high energy density, good high-temperature storage performance, and cycle performance. Among them, by improving the components of the electrolyte, the stability of the protective film formed at the interface of the positive and negative electrodes can be improved, thereby improving the high and low temperature performance of the electrochemical device. However, in the related art, the effect of the electrolyte on improving the stability of the protective film at the interface of the positive and negative electrodes is still poor. Therefore, the components of the electrolyte need to be optimized. Summary of the invention

[0003] The embodiments of the present application provide an electrolyte, an electrochemical device, and an electronic device, which can solve the problem of poor stability of the protective film of the electrolyte on the positive and negative electrode interfaces.

[0004] In a first aspect, the present application provides an electrolyte comprising lithium tetrafluoroborate and a compound of formula I;

[0005]

[0006] Wherein, in the compound of formula I, R is selected from C2-C6 alkyl which is unsubstituted or substituted by Ra, C2-C6 alkenyl which is unsubstituted or substituted by Ra, C2-C6 alkynyl which is unsubstituted or substituted by Ra, C2-C6 nitrogen-containing heteroaryl which is unsubstituted or substituted by Ra, C6-C 12 Aryl, the substituents Ra of each group are independently selected from fluorine or C1-C6 fluoroalkyl;

[0007] Based on the total mass of the electrolyte, the mass percentage of the lithium tetrafluoroborate is A, and the mass percentage of the compound of formula I is B, wherein 0.1%≤A≤2%, 0.01%≤B≤20%. By regulating the mass percentage of the compound of formula I and lithium tetrafluoroborate in the electrolyte, the compound of formula I and lithium tetrafluoroborate are within the scope of the present application, which can effectively improve the stability of the electrode interface, improve the impedance of the electrochemical device, and improve the low-temperature discharge performance of the electrochemical device.

[0008] In some exemplary embodiments, the electrolyte satisfies at least one of the following conditions:

[0009] (1) 0.2% ≤ A ≤ 1.5%;

[0010] (2)2.0%≤B≤10%.

[0011] In some exemplary embodiments, 15≤B / A≤70. By selecting the contents of lithium tetrafluoroborate and the compound of formula I to meet the above range, the synergistic effect of lithium tetrafluoroborate and the compound of formula I is more obvious, which can improve the interface impedance of the positive and negative electrodes, form a thinner passivation layer, and effectively improve the ionic conductivity of the electrode interface.

[0012] In some exemplary embodiments, the compound of formula I includes at least one of the following compounds:

[0013]

[0014] The above-mentioned compound of formula I is selected, and the compound of formula I can form a positive electrode interface passivation layer and / or a negative electrode interface passivation layer of a lithium-containing inorganic compound rich in S and F elements at the electrode interface, thereby improving the stability of the positive and negative electrode interfaces, improving the impedance of the electrochemical device, and improving the ionic conductivity, thereby improving the low-temperature discharge performance of the electrochemical device.

[0015] In some exemplary embodiments, the electrolyte further comprises a compound of formula II, wherein the compound of formula II comprises at least one of the following compounds:

[0016]

[0017] In some exemplary embodiments, based on the total mass of the electrolyte, the mass percentage of the compound of formula II is C, wherein 0.1%≤C≤20%. The compound of formula II is a carboxylic acid ester compound having a lower viscosity, a lower melting point, and a higher dielectric constant. By adjusting the mass percentage of the compound of formula II in the electrolyte to meet the above range and using it as a co-solvent with the compound of formula I, the ionic conductivity of the electrolyte at low temperature can be improved, thereby further improving the low temperature performance of the electrochemical device.

[0018] In some exemplary embodiments, the electrolyte further includes a fluorocarbonate, and the fluorocarbonate includes at least one of fluoroethylene carbonate, difluoroethylene carbonate or 3,3,3-trifluoropropylene carbonate; based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate is F, wherein 0.01%≤F≤5%, 0.005≤F / (A+B)≤0.5. By selecting the mass percentage of the fluorocarbonate within the above range, the fluorocarbonate can further improve the interface impedance of the negative electrode and improve the low-temperature discharge performance of the electrochemical device. In addition, the fluorocarbonate works together with the compound of formula I and lithium tetrafluoroborate, and based on the high dielectric constant of the fluorocarbonate and the compound of formula I, the dissociation degree of lithium tetrafluoroborate can be increased, thereby improving the low-temperature discharge performance of the electrochemical device.

[0019] In some exemplary embodiments, the electrolyte further includes a cyclic sulfur-oxygen double bond compound, the cyclic sulfur-oxygen double bond compound includes at least one of 1,3-propane sultone, ethylene sulfate or methane disulfonic acid methylene ester; based on the total mass of the electrolyte, the mass percentage of the cyclic sulfur-oxygen double bond compound is S, wherein 0.01%≤S≤5.0%, 0.003≤S / (A+B)≤0.5. By selecting the mass percentage of the cyclic sulfur-oxygen double bond compound to meet the above range, the cyclic sulfur-oxygen double bond compound can further enrich the positive and negative electrode interface components during the charge and discharge process and improve the density of the purification layer. In addition, the cyclic sulfur-oxygen double bond compound works together with the compound of formula I and lithium tetrafluoroborate, and based on the solvation structure formed by the cyclic sulfur-oxygen double bond compound and the compound of formula I for lithium ions, the ionic conductivity of the electrolyte at low temperature can be improved.

[0020] In a second aspect, the present application provides an electrochemical device, comprising the electrolyte as described above.

[0021] In a third aspect, the present application provides an electronic device, comprising the electrochemical device as described above.

[0022] Based on the electrolyte, electrochemical device and electronic device of the embodiments of the present application, by adding lithium tetrafluoroborate and the compound of formula I to the electrolyte, and selecting the mass percentage A of lithium tetrafluoroborate to satisfy 0.1%≤A≤2%, and the mass percentage B of the compound of formula I to satisfy 0.01%≤B≤20%, lithium tetrafluoroborate can form a passivation layer with the compound of formula I, which includes organic components and inorganic components and is rich in at least one element of B, P or F. The passivation layer is thin and strong, and the passivation layer exists at the positive electrode interface and / or the negative electrode interface, which can effectively improve the stability of the electrode interface, improve the impedance of the electrochemical device, and improve the low-temperature discharge performance of the electrochemical device.

[0023] The passivation layer in the present application also refers to the protective film layer formed at the interface of the positive electrode and / or the negative electrode. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. All other embodiments obtained by those skilled in the art based on the present application are within the scope of protection of the present application.

[0025] It should be noted that in the following content, lithium-ion batteries are used as an example of electrochemical devices to explain the present application, but the electrochemical devices of the present application are not limited to lithium-ion batteries. The specific technical solution is as follows:

[0026] In a first aspect, the present application provides an electrolyte for an electrochemical device, the electrolyte comprising lithium tetrafluoroborate and a compound of formula I, wherein the mass percentage A of the lithium tetrafluoroborate satisfies 0.1%≤A≤2%, and the mass percentage B of the compound of formula I satisfies 0.01%≤B≤20%, based on the total mass of the electrolyte, so that a thin and strong passivation layer can be formed at the interface between the positive and negative electrodes, thereby improving the interface impedance of the positive and negative electrodes and the low-temperature discharge performance.

[0027] The compound of formula I included in the electrolyte of the present application is as follows:

[0028]

[0029] Wherein, in Formula I, R is selected from C2-C6 alkyl which is unsubstituted or substituted by Ra, C2-C6 alkenyl which is unsubstituted or substituted by Ra, C2-C6 alkynyl which is unsubstituted or substituted by Ra, C2-C6 nitrogen-containing heteroaryl which is unsubstituted or substituted by Ra, C6-C 12 Aryl, the substituents Ra of each group are independently selected from fluorine or C1-C6 fluoroalkyl.

[0030] In the embodiment of the present application, by adding the compound of formula I to the electrolyte, the compound of formula I can form a positive electrode interface passivation layer and / or a negative electrode interface passivation layer of a lithium-containing inorganic compound rich in S and F elements at the electrode interface, thereby improving the stability of the positive and negative electrode interfaces, improving the impedance of the electrochemical device, and improving the ionic conductivity, thereby improving the low-temperature discharge performance of the electrochemical device.

[0031] Based on the mass of the electrolyte, the mass percentage of the compound of formula I is B. In some embodiments, 0.01%≤B≤20%. In some embodiments, 1.0%≤B≤15%. In some embodiments, 2.0%≤B≤10%. In some embodiments, 2.0%≤B≤5%, in some embodiments, 0.05%≤B≤10%, in some embodiments, the value of B is 0.01%, 0.03%, 0.05%, 0.07%, 1.0%, 8.0%, 10.0%, 13.0%, 18%, 20% or a value in the range of any two of these values. By selecting B in the above range, the content of the compound of formula I is appropriate, which helps to promote the uniform deposition of compounds containing elements such as S and F at the positive electrode interface, while improving the ionic conductivity of the positive electrode interface and improving the positive electrode interface impedance. When B exceeds the upper limit of 20%, the thickness of the passivation layer formed at the positive electrode interface will increase, the ionic conductivity will decrease, and the impedance will deteriorate, thereby reducing the ionic conductivity of the positive electrode interface. When B is lower than the lower limit of 0.01%, it will be difficult to play a role in improving the interface impedance.

[0032] In some embodiments, the compound of Formula I includes at least one of the following compounds:

[0033]

[0034] The electrolyte also includes lithium tetrafluoroborate, which can form a passivation layer including organic components and inorganic components and rich in at least one element of B, P or F with the compound of formula I. The passivation layer is thin and strong, and the passivation layer exists at the positive electrode interface or the negative electrode interface, which can effectively improve the stability of the electrode interface, improve the impedance of the electrochemical device, and improve the low-temperature discharge performance of the electrochemical device.

[0035] Based on the mass of the electrolyte, the mass percentage of lithium tetrafluoroborate is A. In some embodiments, 0.1%≤A≤2%. In some embodiments, the value of A is 0.1%, 0.2%, 0.3%, 0.5%, 0.7%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0% or a value in the range composed of any two of these values. In some embodiments, 0.3%≤A≤2%. In some embodiments, 0.4%≤A≤1.8%. In some embodiments, 0.5%≤A≤2%. In some embodiments, 1.8%≤A≤2%. In the present application, A satisfies the above range, and the content of lithium tetrafluoroborate is further optimized, so that lithium tetrafluoroborate and the compound of formula I can jointly optimize the positive and negative electrode interface morphology while reducing the increase in positive and negative electrode impedance caused by excessive decomposition of lithium tetrafluoroborate itself. When A exceeds the upper limit of 10%, lithium tetrafluoroborate will not be completely ionized, which will reduce the conductivity of the electrolyte. When A is lower than the lower limit of 0.3%, the B content in the film-forming component will be insufficient and it will be difficult to play a role in improving the interface.

[0036] In some embodiments, 15≤B / A≤70. In some embodiments, 15≤B / A≤65.0. In some embodiments, 20.0≤B / A≤60.0. In some embodiments, 25.0≤B / A≤60.0. In some embodiments, 20.0≤B / A≤65.0. In some embodiments, the value of B / A is 0.005, 5.0, 15.0, 26.8, 31.8, 41.0, 52.7, 73.4, 84.5, 95.0 or a value in the range composed of any two of these values. The present application regulates the value of B / A within the above range, and the synergistic effect of the two compounds of lithium tetrafluoroborate and the compound of formula I is more obvious, which can improve the interface impedance of the positive and negative electrodes, form a thinner passivation layer, and effectively improve the ionic conductivity of the electrode interface.

[0037] In some embodiments, the electrolyte further comprises a compound of formula II, wherein the compound of formula II comprises at least one of the following compounds:

[0038]

[0039] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the compound of formula II is C, and C satisfies: 0.1%≤C≤20%. In some embodiments, 0.1%≤C≤10%. In some embodiments, 0.5%≤C≤15.0%. In some embodiments, 0.5%≤C≤12.0%. In some embodiments, 1.0%≤C≤15.0%. In some embodiments, the value of C is 0.1%, 0.5%, 1.5%, 8.8%, 9.8%, 10.0%, 12.8%, 13.6%, 15.5%, 20.0% or a value in the range of any two of these values. The compound of formula II is a carboxylic acid ester compound with a lower viscosity, a low melting point, and a higher dielectric constant. By adjusting the mass percentage of the compound of formula II in the electrolyte to meet the above range, and using it as a co-solvent with the compound of formula I, the ionic conductivity of the electrolyte at low temperature can be improved, thereby further improving the low temperature performance of the electrochemical device.

[0040] In some embodiments, the electrolyte further includes a fluorocarbonate, and the fluorocarbonate includes at least one of fluoroethylene carbonate, difluoroethylene carbonate, or 3,3,3-trifluoropropylene carbonate.

[0041] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate is F, and F satisfies: 0.01%≤F≤5.0%. In some embodiments, 0.1%≤F≤5.0%. In some embodiments, 0.5%≤F≤4.0%. In some embodiments, 0.9%≤F≤3.5%. In some embodiments, 0.1%≤F≤3.5%. In some embodiments, 0.9%≤F≤3%. In some embodiments, the value of F is 0.01%, 0.05%, 0.25%, 1.0%, 2.0%, 3.0%, 3.1%, 3.8%, 4.5%, 5.0% or a value in the range of any two of these values. Fluorinated carbonate has good reduction performance. By selecting the content of fluorocarbonate in the above range, fluorocarbonate can further improve the interface impedance of the negative electrode and improve the low temperature discharge performance of the electrochemical device. In addition, the fluorocarbonate works together with the compound of formula I and lithium tetrafluoroborate to increase the dissociation degree of lithium tetrafluoroborate based on the high dielectric constant of the fluorocarbonate and the compound of formula I, thereby improving the low-temperature discharge performance of the electrochemical device.

[0042] In some embodiments, F, A and B satisfy the conditional formula: 0.005≤F / (A+B)≤0.5. In some embodiments, 0.01≤F / (A+B)≤0.4. In some embodiments, 0.05≤F / (A+B)≤0.3. In some embodiments, 0.06≤F / (A+B)≤0.2. In some embodiments, 0.06≤F / (A+B)≤0.2. In some embodiments, the value of F / (A+B) is 0.005, 0.007, 0.03, 0.09, 0.12, 0.15, 0.2, 0.25, 0.45, 0.5 or a value in the range consisting of any two of these values. By adjusting the fluorinated carbonate, lithium tetrafluoroborate and the compound of formula I in the electrolyte to meet the above conditional formula, the elements S, B, F, P and the like contained in the passivation layer formed at the electrode interface are distributed more evenly, which can further improve the ionic conductivity of the electrochemical device and make the positive and negative electrode interfaces more stable.

[0043] In some embodiments, the electrolyte further includes a cyclic sulfur-oxygen double bond compound, and the cyclic sulfur-oxygen double bond compound includes at least one of 1,3-propane sultone, ethylene sulfate, or methylene methane disulfonate.

[0044] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the cyclic sulfur-oxygen double bond compound is S, and S satisfies the condition 0.01%≤S≤5.0%. In some embodiments, 0.2%≤S≤5.0%. In some embodiments, 0.4%≤S≤4.5%. In some embodiments, 0.3%≤S≤4.5%. In some embodiments, 0.2%≤S≤3.0%. In some embodiments, 3.0%≤S≤5.0%. In some embodiments, the value of S is 0.01%, 0.15%, 0.75%, 2.5%, 2.8%, 3.0%, 3.6%, 4.1%, 4.5%, 5.0%, or a value in the range of any two of these values. By selecting a cyclic sulfur-oxygen double bond compound to meet the above range, the cyclic sulfur-oxygen double bond compound can further enrich the positive and negative electrode interface components during the charge and discharge process and improve the density of the passivation layer. In addition, the cyclic sulfur-oxygen double bond compound works together with the compound of formula I and lithium tetrafluoroborate. Based on the solvation structure formed by the cyclic sulfur-oxygen double bond compound and the compound of formula I for lithium ions, the ionic conductivity of the electrolyte at low temperatures can be improved.

[0045] In some embodiments, S, A and B satisfy the conditional formula: 0.003≤S / (A+B)≤0.5. In some embodiments, 0.005≤S / (A+B)≤0.4. In some embodiments, 0.01≤S / (A+B)≤0.3. In some embodiments, 0.01≤S / (A+B)≤0.2. In some embodiments, 0.008≤S / (A+B)≤0.2. In some embodiments, the value of S / (A+B) is 0.003, 0.004, 0.008, 0.01, 0.05, 0.3, 0.35, 0.5 or a value in the range consisting of any two of these values. By adjusting the cyclic sulfur-oxygen double bond compound, lithium tetrafluoroborate and the compound of formula I in the electrolyte to meet the above conditional formula, the solvation structure formed by the cyclic sulfur-oxygen double bond compound, the compound of formula I and lithium tetrafluoroborate can improve the migration ability of lithium ions and improve the conductivity of the electrolyte, thereby improving the low-temperature discharge performance of the electrochemical device.

[0046] The electrolyte also includes a lithium salt. The present application does not particularly limit the type of lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonyl imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(oxalate borate) (LiBOB) or lithium difluorooxalate borate (LiDFOB). Based on the total mass of the electrolyte, the mass percentage of the lithium salt may be 8% to 15%, for example, the mass percentage of the lithium salt may be 8%, 9%, 10%, 11%, 12.5%, 13%, 15% or a range consisting of any two of the values.

[0047] The electrolyte may also include a non-aqueous solvent. The present application does not particularly limit the type of non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds or cyclic carbonate compounds. The above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate, propylene carbonate, ethylene carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or methyl ethyl carbonate. The above-mentioned cyclic carbonate compounds may include but are not limited to at least one of butylene carbonate or ethylene ethylene carbonate. The above-mentioned carboxylate compounds may include but are not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, γ-butyrolactone, decalactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of ethylene glycol dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0048] In a second aspect, the present application provides an electrochemical device, the electrochemical device comprising the electrolyte as described above, and the electrochemical device further comprising a positive electrode, a negative electrode and a separator.

[0049] The present application does not specifically limit the materials, structures and processing methods of the positive electrode, negative electrode and separator of the electrochemical device. The positive electrode, negative electrode and separator that can be used in the art are applicable to the present application.

[0050] Ⅰ Positive electrode

[0051] The positive electrode in the electrochemical device of the present application includes a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector. The positive electrode active material layer can be coated on one side of the positive electrode current collector or on both sides of the positive electrode current collector.

[0052] The positive electrode material layer disposed on the same side of the positive electrode current collector may be one or more layers, and each layer of the multiple positive electrode material layers may contain the same or different positive electrode active materials. As the positive electrode active material used in the electrochemical device, the positive electrode active material may include but is not limited to lithium nickel cobalt manganese oxide (e.g., NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate.

[0053] The cathode material layer of the present application also includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the cathode material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black, carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers. The above-mentioned conductive carbon black may include but is not limited to Super P, acetylene black or Ketjen black. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The binder may include, but is not limited to, polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene butadiene copolymer (styrene-butadiene rubber, SBR), sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose (CMC-Na), potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose or potassium hydroxymethyl cellulose. The present application does not particularly limit the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved.

[0054] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, it may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The present application has no particular restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm, preferably 6μm to 18μm. The present application has no particular restrictions on the thickness of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the single-sided positive electrode material layer is 30μm to 120μm.

[0055] Optionally, the positive electrode may further include a conductive layer, which is located between the positive electrode current collector and the positive electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be at least one of the above conductive agent and the above binder. The present application has no particular restrictions on the mass ratio of the conductive agent and the binder in the conductive layer, and those skilled in the art may select according to actual needs, as long as the purpose of the present application can be achieved.

[0056] In the present application, the electrochemical device also includes a negative electrode, which includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode material layer disposed on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be disposed on one surface of the negative electrode current collector along its own thickness direction, or on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a partial area of ​​the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the negative electrode current collector, as long as the purpose of this application can be achieved. For example, it can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector, etc.

[0057] The negative electrode material layer of the present application includes a negative electrode active material. The present application has no particular limitation on the negative electrode active material, as long as the purpose of the present application can be achieved. For example, the negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0.5<x<1.6), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12 , Li-Al alloy or metallic lithium, etc. The negative electrode material layer of the present application also includes a binder. The present application has no special restrictions on the binder in the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the binder can be at least one of the above binders. The negative electrode material layer of the present application also includes a conductive agent. The present application has no special restrictions on the conductive agent in the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent can be at least one of the above conductive agents. The present application has no special restrictions on the mass ratio of the negative electrode active material, the binder and the conductive agent in the negative electrode material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.

[0058] The present application has no particular limitation on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode current collector is 5 μm to 16 μm. The present application has no particular limitation on the thickness of the negative electrode material layer, as long as the purpose of the present application can be achieved, for example, the thickness of the single-sided negative electrode material layer is 30 μm to 120 μm.

[0059] Optionally, the negative electrode may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be at least one of the above conductive agent and the above binder. The present application has no particular restrictions on the mass ratio of the conductive agent and the binder in the conductive layer, and those skilled in the art may choose according to actual needs, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the thickness of the conductive layer, as long as the purpose of the present application can be achieved, for example, the thickness of the conductive layer is 1 μm to 10 μm.

[0060] In the present application, the electrochemical device also includes a diaphragm, which is used to separate the positive electrode plate and the negative electrode, prevent the internal short circuit of the electrochemical device, allow the electrolyte ions to pass freely, and do not affect the electrochemical charge and discharge process. The present application has no special restrictions on the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (for example, polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid at least one; the type of diaphragm may include woven membranes, non-woven membranes, microporous membranes, composite membranes, rolled membranes or spun membranes at least one. The present application has no special restrictions on the thickness of the diaphragm, as long as the purpose of the present application can be achieved, for example, the thickness of the diaphragm is 3μm to 30μm.

[0061] In the present application, the diaphragm may include a substrate and a surface treatment layer. The substrate may be a non-woven fabric or a composite film having a porous structure, and the material of the substrate may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used. Optionally, the thickness of the base film is 3 μm to 25 μm. Optionally, a surface treatment layer is provided on at least one surface of the substrate, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the present application has no particular restrictions on the above-mentioned inorganic particles, for example, it may include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the above-mentioned binder, for example, it can be at least one of the aforementioned binders. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene). Optionally, the thickness of the surface treatment layer is 1 μm to 10 μm.

[0062] The electrochemical device of the present application also includes a packaging bag for containing a positive electrode sheet, a separator, a negative electrode and an electrolyte, as well as other components known in the art in the electrochemical device, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0063] The present application does not particularly limit the type of electrochemical device, which may include any device that undergoes an electrochemical reaction. In the present application, the electrochemical device may include, but is not limited to: a lithium metal electrochemical device, a lithium ion electrochemical device (lithium ion battery), a lithium polymer electrochemical device or a lithium ion polymer electrochemical device (lithium ion polymer battery), etc.

[0064] The preparation process of the electrochemical device of the present application is well known to those skilled in the art, and the present application has no particular limitation. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode in order, and winding, folding and other operations as needed to obtain an electrode assembly of a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device; or stacking the positive electrode sheet, the separator and the negative electrode in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0065] The present application also provides an electronic device, which includes the electrochemical device in any of the above embodiments. Therefore, the electronic device provided by the present application has good performance.

[0066] The present application does not particularly limit the type of electronic device, which can be any electronic device known in the prior art. In some embodiments, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0067] The preparation of the electrochemical device is described below in conjunction with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0068] Example

[0069] Hereinafter, taking lithium-ion batteries as an example, examples and comparative examples are given to more specifically describe the implementation of the electrochemical device of the present application. Those skilled in the art will understand that the preparation method described in the present application is only an example, and any other suitable preparation method is within the scope of the present application. Various tests and evaluations are carried out according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0070] Test Method

[0071] 1. -10℃50%SOC impedance test method

[0072] At 25°C, discharge the lithium-ion battery to 3.0V at a current of 0.5C. After standing for 5 minutes, charge it to 4.5V at a current of 0.5C, and keep the voltage constant at 0.025C at 4.5V. After standing for 5 minutes, discharge it to 3.0V at a current of 0.1C, and mark the capacity released at this time as C1. Charge it to 4.5V with a capacity of 0.5C1, keep the voltage constant at 0.025C1 at 4.5V, and stand for 5 minutes. Then, at -10°C, discharge the lithium-ion battery with a current of 0.1C1 for 5h, and the battery voltage at this time is recorded as V1. Then, discharge it with a current of 1C for 1 second, and the battery voltage at this time is recorded as V2.

[0073] -10℃50%SOC impedance=(V1-V2) / (1C-0.1C1).

[0074] 2. Low temperature discharge performance test method

[0075] Place the lithium-ion battery in a 25℃ constant temperature environment and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature of 25℃. Charge to 4.5V at a constant current of 0.5C, charge to a current of 0.025C at a constant voltage of 4.5V, discharge to 3.0V at a constant current of 0.2C, and record the discharge capacity at 25℃ as C2. Then charge to 4.5V at a constant current of 0.5C, charge to a current of 0.025C at a constant voltage of 4.5V, transfer the lithium-ion battery to a -10℃ constant temperature test box, let it stand for 60 minutes to allow the lithium-ion battery to reach a constant temperature of -10℃, and then discharge to 3.0V at a constant current of 0.2C, and record the discharge capacity at -10℃ as C3.

[0076] -10℃ low temperature discharge capacity retention rate = C3 / C2×100%.

[0077] Example 1-1

[0078] 1. Preparation of positive electrode

[0079] The positive electrode active material LiCoO2, the positive electrode conductive agent conductive carbon black (Super P), the positive electrode binder polyvinylidene fluoride (PVDF, Mw = 7 × 10 6) are mixed in a mass ratio of 97.5:1:1.5, N-methylpyrrolidone (NMP) is added as a solvent, and stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, dried and cold pressed at 85°C to obtain a positive electrode sheet with a single-sided coating of a positive electrode material layer with a thickness of 50μm. Thereafter, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of a positive electrode material layer. After cutting and welding the positive electrode aluminum pole ears, a positive electrode sheet with a specification of 74mm×851mm is obtained for standby use, and the compaction density of the positive electrode material layer is 4.15g / cm 3 .

[0080] 2. Preparation of negative electrode sheet

[0081] The negative electrode active material artificial graphite, negative electrode conductive agent Super P, thickener carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5 ), negative electrode binder styrene butadiene rubber (SBR, Mw = 5 × 10 6 ) are mixed in a mass ratio of 97.5:1:0.5:1, and then deionized water is added as a solvent, and stirred evenly under the action of a vacuum mixer to obtain a negative electrode slurry with a solid content of 50wt%. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 8μm, dried and cold pressed at 85°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer with a thickness of 60μm. Thereafter, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of a negative electrode material layer. After cutting and welding the negative electrode ear nickel ear, a negative electrode sheet with a specification of 76mm×867mm is obtained for standby use, and the compaction density of the negative electrode material layer is 1.75g / cm 3 .

[0082] 3. Preparation of electrolyte

[0083] In an argon atmosphere glove box with a water content of less than 10 ppm, dimethyl carbonate: propylene carbonate: ethylene carbonate are mixed in a mass ratio of 60:30:10 to obtain a base solvent, and then lithium tetrafluoroborate, a compound of formula I and lithium hexafluorophosphate (LiPF6) are dissolved in the base solvent to obtain an electrolyte. Wherein, based on the total mass of the electrolyte, the mass percentage of LiPF6 is 12.5%.

[0084] The mass percentages of lithium tetrafluoroborate and the compound of formula I are shown in Table 1, and the rest are base solvents.

[0085] 4. Isolation film

[0086] A polyethylene (PE) porous membrane with a thickness of 15 μm was used.

[0087] 5. Preparation of lithium-ion batteries

[0088] The prepared separator, positive electrode sheet, separator and negative electrode sheet are stacked and wound in sequence to obtain an electrode assembly with a wound structure. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation (charging at a constant current of 0.2°C to 3.5V, and then charging at a constant current of 1C to 3.9V), capacity, degassing, trimming and other processes.

[0089] Examples 1-2 to 1-17 are the same as Example 1-1 except that the type of compound of formula I, the content B of compound of formula I and the content A of lithium tetrafluoroborate are adjusted in the preparation of the electrolyte as shown in Table 1. The mass percentage of the base solvent changes accordingly, and the mass percentage of the lithium salt remains unchanged.

[0090] Comparative Example 1-1 is the same as Example 1-1 except that the compound of Formula I is not added to the electrolyte, wherein the mass percentage of the base solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged.

[0091] Comparative Example 1-2 is the same as Example 1-1 except that lithium tetrafluoroborate is not added to the electrolyte, wherein the mass percentage of the base solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged.

[0092] Comparative Examples 1-3 to Comparative Examples 1-6 are the same as Example 1-1 except that the content B of the compound of Formula I and the content A of lithium tetrafluoroborate in the preparation of the electrolyte are adjusted as shown in Table 1. The mass percentage of the base solvent is changed accordingly, and the mass percentage of the lithium salt remains unchanged.

[0093] Examples 2-1 to 2-7 are the same as Example 1-4 except that the compound of Formula II is added in the preparation of the electrolyte as shown in Table 2. The mass percentage of the base solvent changes accordingly, while the mass percentage of the lithium salt remains unchanged.

[0094] Examples 3-1 to 3-6 are the same as Examples 1-4 except that fluorocarbonate is added in the preparation of the electrolyte as shown in Table 3. The mass percentage of the base solvent changes accordingly, while the mass percentage of the lithium salt remains unchanged.

[0095] Examples 3-7 to 3-8 are the same as Examples 1-4 except that the compound of Formula II and fluorocarbonate are added in the preparation of the electrolyte as shown in Table 3. The mass percentage of the base solvent changes accordingly, while the mass percentage of the lithium salt remains unchanged.

[0096] Example 4-1 to Example 4-4 are the same as Example 1-4 except that a cyclic sulfur-oxygen double bond compound is added in the preparation of the electrolyte as shown in Table 4. The mass percentage of the base solvent changes accordingly, and the mass percentage of the lithium salt remains unchanged.

[0097] Examples 4-5 to 4-6 are the same as Examples 1-4 except that the cyclic sulfur-oxygen double bond compound and the compound of formula II are added in the preparation of the electrolyte as shown in Table 4. The mass percentage of the base solvent changes accordingly, and the mass percentage of the lithium salt remains unchanged.

[0098] Examples 4-7 to 4-8 are the same as Examples 1-4 except that a cyclic sulfur-oxygen double bond compound and a fluorocarbonate are added to the preparation of the electrolyte as shown in Table 4. The mass percentage of the base solvent changes accordingly, while the mass percentage of the lithium salt remains unchanged.

[0099] Examples 4-9 to 4-10 are the same as Examples 1-4 except that a cyclic sulfur-oxygen double bond compound, a fluorocarbonate and a compound of formula II are added to the preparation of the electrolyte as shown in Table 4. The mass percentage of the base solvent changes accordingly, and the mass percentage of the lithium salt remains unchanged.

[0100] The preparation parameters and performance parameters of Examples 1-1 to 1-17 and Comparative Examples 1-1 to 1-6 are shown in Table 1.

[0101] Table 1

[0102]

[0103] Note: “ / ” in Table 1 means there is no corresponding parameter.

[0104] According to Examples 1-1 to 1-17 and Comparative Examples 1-1 and 1-6 in Table 1, it can be seen that the electrolyte includes the compound of formula I and lithium tetrafluoroborate, which can effectively improve the low-temperature impedance of the electrochemical device, and the compound of formula I and lithium tetrafluoroborate can form a purification layer rich in elements such as B, P, and S at the positive electrode interface, which reduces the interface impedance while improving the low-temperature discharge performance of the electrochemical device.

[0105] It can be seen from Examples 1-1 to 1-6, Comparative Examples 1-3 and 1-4 that the mass percentage A of lithium tetrafluoroborate satisfies 0.1%≤A≤2%, which can effectively improve the low-temperature impedance performance of the electrochemical device. When A is lower than the lower limit of 0.3%, it is difficult to improve the interface stability. When A is higher than the upper limit of 10%, lithium tetrafluoroborate cannot be completely ionized, reducing the conductivity of the electrolyte. In serious cases, it will also deteriorate the impedance of the lithium-ion battery.

[0106] According to Examples 1-7 to 1-17, Comparative Examples 1-5 and Comparative Examples 1-6, it can be seen that the mass percentage content B of the compound of Formula I satisfies 0.01%≤B≤20%, which can effectively improve the low-temperature interface impedance performance of the electrochemical device. When B is lower than the lower limit of 1%, it is also difficult to play a role in interface modification. When B exceeds the upper limit of 30%, the thickness of the formed purification layer will increase and become fluffy, which will reduce the ionic conductivity, thereby worsening the impedance of the lithium-ion battery.

[0107] It can be seen from Examples 1-1 to 1-17 that A and B satisfy 15≤B / A≤70, and the purification layer formed by the compound of Formula I and lithium tetrafluoroborate can improve the conductivity of lithium ions, thereby effectively improving the low-temperature discharge performance of lithium ion batteries.

[0108] The preparation parameters and performance parameters of Examples 1-4 and 2-1 to 2-7 are shown in Table 2.

[0109] Table 2

[0110]

[0111] Note: “ / ” in Table 2 means there is no corresponding parameter.

[0112] It can be seen from Examples 1-4 and 2-1 to 2-7 in Table 2 that by introducing the compound of Formula II into the electrolyte, the content C of the compound of Formula II satisfies 0.1%≤C≤20%, which can reduce the viscosity of the electrolyte and help improve the dissociation of the lithium salt, thereby further effectively improving the low-temperature impedance performance of the electrochemical device.

[0113] The preparation parameters and performance parameters of Examples 1-4 and 3-1 to 3-8 are shown in Table 2.

[0114] Table 3

[0115]

[0116] Note: “ / ” in Table 3 means there is no corresponding parameter.

[0117] According to Examples 1-4, 3-1 to 3-8 in Table 3, it can be seen that by introducing fluorocarbonate into the electrolyte, the content F of fluorocarbonate satisfies 0.01%≤F≤5%, 0.005≤F / (A+B)≤0.5, which can effectively improve the low temperature impedance and low temperature discharge performance of lithium ion batteries. This is because fluorocarbonate can improve the dissociation ability of lithium salts and improve the ionic conductivity of the electrolyte. However, the dissociation ability of fluorocarbonate with too low a content is limited, and the viscosity of the electrolyte will be increased if the content of fluorocarbonate with too high a content is too high. When the contents of the compound of formula I, lithium tetrafluoroborate and fluorocarbonate are within the above range, the conductivity of the electrolyte can be improved, and the passivation layer components can be further optimized to generate a low impedance passivation layer, thereby achieving the effect of optimizing low temperature impedance and low temperature discharge performance at the same time.

[0118] The preparation parameters and performance parameters of Examples 1-4 and 4-1 to 4-10 are shown in Table 4.

[0119] Table 4

[0120]

[0121]

[0122] Note: “ / ” in Table 4 means there is no corresponding parameter.

[0123] According to Examples 1-4 and 4-1 to 4-4 in Table 4, it can be seen that the content S of the cyclic sulfur-oxygen double bond compound satisfies 0.01%≤S≤5.0%, 0.003≤S / (A+B)≤0.5, and the cyclic sulfur-oxygen double bond compound can further enrich the positive and negative electrode interface components and improve the density of the passivation layer, thereby effectively improving the low-temperature impedance performance and low-temperature discharge performance of the electrochemical device. When S is lower than the above range, the effect of improving the low-temperature impedance and low-temperature discharge performance of the electrochemical device is not obvious. When S is higher than the above range, the conductivity of the electrolyte will decrease, and the effect of improving the low-temperature impedance performance of the electrochemical device is poor.

[0124] It can be seen from Examples 4-5 to 4-6 and 4-9 to 4-10 in Table 4 that by adding a cyclic sulfur-oxygen double bond compound to the electrolyte, the cyclic sulfur-oxygen double bond compound can be combined with the compound of Formula I and the compound of Formula II to form a solvation structure to promote the transmission of lithium ions, thereby further improving the low-temperature discharge performance of the electrochemical device.

[0125] Both the compound of formula II and the fluorinated carbonate can improve the dissociation ability of lithium salts. According to Examples 4-5 to 4-10, it can be seen that the compound of formula II and the fluorinated carbonate can further improve the low-temperature impedance performance of the electrochemical device by combining with the cyclic sulfur-oxygen double bond compound.

[0126] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0127] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0128] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. An electrolyte, characterized in that: Comprising lithium tetrafluoroborate and a compound of formula I; Wherein, in the compound of formula I, R is selected from C2-C6 alkyl which is unsubstituted or substituted by Ra, C2-C6 alkenyl which is unsubstituted or substituted by Ra, C2-C6 alkynyl which is unsubstituted or substituted by Ra, C2-C6 nitrogen-containing heteroaryl which is unsubstituted or substituted by Ra, C6-C 12 Aryl, the substituents Ra of each group are independently selected from fluorine or C1-C6 fluoroalkyl; Based on the total mass of the electrolyte, the mass percentage of the lithium tetrafluoroborate is A, and the mass percentage of the compound of formula I is B, wherein 0.1%≤A≤2%, and 0.01%≤B≤20%.

2. The electrolyte according to claim 1, characterized in that The electrolyte satisfies at least one of the following conditions: (1)0.2%≤A≤1.5%; (2)2.0%≤B≤10%。 3. The electrolyte according to claim 1 or 2, characterized in that 15≤B / A≤70.

4. The electrolyte according to claim 1, characterized in that The compounds of formula I include at least one of the following compounds:

5. The electrolyte according to claim 1, characterized in that The electrolyte further comprises a compound of formula II, wherein the compound of formula II comprises at least one of the following compounds:

6. The electrolyte according to claim 5, characterized in that Based on the total mass of the electrolyte, the mass percentage of the compound of formula II is C, wherein 0.1%≤C≤20%.

7. The electrolyte according to claim 1, characterized in that The electrolyte further includes a fluorocarbonate, wherein the fluorocarbonate includes at least one of fluoroethylene carbonate, difluoroethylene carbonate or 3,3,3-trifluoropropylene carbonate; Based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate is F, wherein 0.01%≤F≤5%, 0.005≤F / (A+B)≤0.

5.

8. The electrolyte according to claim 1, characterized in that The electrolyte further comprises a cyclic sulfur-oxygen double bond compound, wherein the cyclic sulfur-oxygen double bond compound comprises at least one of 1,3-propane sultone, ethylene sulfate or methylene methane disulfonate; Based on the total mass of the electrolyte, the mass percentage of the cyclic sulfur-oxygen double bond compound is S, wherein 0.01%≤S≤5.0%, and 0.003≤S / (A+B)≤0.

5.

9. An electrochemical device, characterized in that: The invention comprises the electrolyte according to any one of claims 1 to 8.

10. An electronic device, characterized in that: An electrochemical device comprising the electrochemical device of claim 9.