Battery diaphragm, preparation method thereof and battery

By using porphyrin compounds to graft silicon particles, inorganic oxides and polymers in the lithium battery separator, a separator that efficiently adsorbs transition metal ions is solved, and the battery stability and Performance improvement.

CN119069946AActive Publication Date: 2024-12-03GAC AION NEW ENERGY AUTOMOBILE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411495002.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03
Estimated Expiration
2044-10-24

AI Technical Summary

Technical Problem

During the cycle of lithium batteries, transition metal ions are dissolved into the electrolyte, passing through the separator to the negative electrode, destroying the SEI film on the surface of the negative electrode, resulting in a degradation of the battery's circulation performance. The complexing agent added in the prior art cannot be effectively improved during long cycles. Battery performance reduces stability.

Method used

A battery separator with a combination of porphyrin-based compounds grafted with silicon particles, inorganic oxides and polymers was prepared by ultraviolet grafting reaction to form a separator with efficient adsorption of transition metal ions to ensure lithium ions passing through and structural stability.

Benefits of technology

It significantly improves the cycling performance and stability of the battery, effectively adsorbs transition metal ions in the positive electrode material, reduces the internal resistance of the battery, and improves the passing of lithium ions and the long-term cycling performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069946A_ABST
    Figure CN119069946A_ABST
Patent Text Reader

Abstract

The invention provides a battery diaphragm, a preparation method thereof and a battery, and belongs to the technical field of battery preparation. The battery diaphragm comprises porphyrin compound grafted silicon particles, an inorganic oxide and a polymer, the battery diaphragm is provided with a plurality of pores, and the pore diameter of the pores is 0.1 nm-100 nm. The porphyrin compound grafted silicon particles are introduced into the battery diaphragm, so that the battery diaphragm has relatively high porosity, and can efficiently adsorb transition metal ions and improve the cycle performance of the battery while ensuring the safety of the battery and the trafficability of lithium ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery preparation, and in particular to a battery separator and a preparation method thereof, and a battery. Background Art

[0002] In lithium batteries, the battery separator is usually placed between the positive and negative electrodes, which can prevent the positive and negative electrodes of the battery from directly contacting each other while conducting lithium ions to ensure the normal operation of the battery. During the cycle of lithium batteries, transition metal ions (such as ions corresponding to Fe, Co, Ni and Mn) in the positive electrode material will slowly dissolve into the electrolyte, migrate through the battery separator to the negative electrode, and destroy the solid electrolyte interface (SEI) film on the surface of the negative electrode, thereby increasing the interface resistance of the negative electrode and reducing the cycle performance of the battery.

[0003] The patent application with application number CN201911144312.9 and titled “A diaphragm slurry, diaphragm and its application for efficient capture of metal ions” discloses a diaphragm slurry for efficient capture of metal ions, which adsorbs transition metal ions by adding multidentate chelating agents, macrocyclic chelating agents or polymer chelating agents to the diaphragm. However, these chelating agents cannot effectively improve the cycle performance of the battery during long-term use, and may even reduce the cycle stability of the battery. Summary of the invention

[0004] To solve the above problems, the purpose of the embodiments of the present application includes providing a diaphragm slurry and a preparation method thereof, a battery diaphragm and a battery, which can efficiently adsorb transition metal ions and improve the cycle performance of the battery while ensuring safety and lithium ion permeability.

[0005] In a first aspect, the present application provides a battery separator, comprising porphyrin compound grafted silicon particles, inorganic oxides and polymers, the battery separator having a plurality of pores, and the pore diameter of the pores is 0.1 nm to 100 nm.

[0006] In the above technical solution, by introducing porphyrin compounds grafted with silicon particles into the battery separator, such materials have good durability, good wettability with electrolyte, high material utilization rate, and can efficiently adsorb transition metal ions dissolved in the positive electrode, thereby effectively improving the battery's cycle performance. In addition, the battery separator formed by porphyrin compounds grafted with silicon particles, inorganic oxides and polymers has good safety and structural stability, and has sufficient pore structure and ideal pore size, which has little effect on the permeability of lithium ions, thereby further ensuring the cycle stability of the battery during long-term cycles.

[0007] In some embodiments of the present application, the thickness of the battery separator is 1 nm to 100 μm.

[0008] In the above technical solution, the thickness range of the battery separator is wide and can be adjusted according to actual conditions to ensure the safety and ion permeability of the battery separator, and is suitable for a wider range of battery systems.

[0009] In some embodiments of the present application, the inorganic oxide includes at least one of boehmite, alumina, silica, titanium dioxide, ferric oxide or ferrosoferric oxide.

[0010] The polymer includes at least one of polyvinylidene fluoride, poly(vinylidene fluoride hexafluoropropylene), polytetrafluoroethylene, polyhexafluoropropylene, polyacrylate, polymethacrylate, polyacrylamide, polymethacrylamide, epoxy resin, polyvinyl pyrrolidone, carboxymethyl cellulose, sodium carboxymethyl cellulose, cellulose or chitosan.

[0011] In the above technical solution, inorganic oxides can enhance the mechanical properties and thermal stability of battery separators, polymers can improve the processability of separator slurry, and the selection range of inorganic oxides and polymers is wide, which can provide a variety of feasible implementation plans.

[0012] In some embodiments of the present application, the mass ratio of the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer is (1-99):(0-99):(0-99).

[0013] In the above technical solution, the mass ratio of the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer has a wide range and can be adjusted according to the actual application needs.

[0014] In some embodiments of the present application, the battery separator includes a functional layer and a polymer base film, the functional layer includes porphyrin compound grafted silicon particles, inorganic oxides and polymers, and the functional layer is located on at least one side of the polymer base film.

[0015] In the above technical solution, adding a polymer base film to the battery separator can improve structural stability and mechanical strength and reduce production costs.

[0016] In some embodiments of the present application, the thickness of the polymer base film is 1 nm to 100 μm.

[0017] Optionally, the material of the polymer base film includes at least one of polyethylene terephthalate, polyvinyl chloride, polyethylene, polyacrylonitrile, polypropylene, polyamide, polyetherimide, and polyvinylidene fluoride.

[0018] In the above technical solution, the thickness of the functional layer and the polymer base film as well as the material of the polymer base film can be adjusted according to actual application requirements.

[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned battery separator, comprising the following steps:

[0020] Dissolving a porphyrin compound having an alkenyl group in a first solvent and mixing the mixture with mercapto-functionalized silicon particles, and performing a grafting reaction under ultraviolet light to prepare porphyrin compound grafted silicon particles;

[0021] The porphyrin compound grafted silicon particles, inorganic oxides and polymers are dispersed in a second solvent and mixed to form a slurry, and the battery separator is obtained by solidifying the slurry.

[0022] In the above technical scheme, porphyrin compounds with alkenyl groups and mercapto-functionalized silicon particles are selected as raw materials. The alkenyl groups and mercapto groups can directly react under ultraviolet light to complete the grafting. The preparation method is simple, the grafting rate is high, and there are few by-products. The prepared porphyrin compound grafted silicon particles are not easy to react chemically in the battery system, the chemical bonds are not easy to break, and have excellent stability. The porphyrin compound grafted silicon particles, inorganic oxides and polymers are mixed and dispersed, and conventional spinning or coating curing is used to prepare the battery separator. The preparation method is simple.

[0023] In some embodiments of the present application, the mercapto-functionalized silicon particles are 3-mercaptopropyl grafted silicon particles, and the porphyrin compound having an alkenyl group includes at least one of protoporphyrin, protoporphyrin monomethyl ester, protoporphyrin dimethyl ester, protoporphyrin monosodium salt, protoporphyrin disodium salt, protoporphyrin monolithium salt or protoporphyrin dilithium salt.

[0024] In the above technical solution, specific mercapto-functionalized silicon particles and porphyrin compounds are selected, and the raw materials are simple and easy to obtain, which can improve the reaction efficiency and production cost.

[0025] In some embodiments of the present application, the grafting reaction temperature is 40 to 80° C., and the time is 6 to 24 hours.

[0026] In the above technical solution, by controlling the conditions of the grafting reaction, the grafting stability and grafting rate can be enhanced and the purity of the product can be ensured.

[0027] In some embodiments of the present application, the method for forming a battery separator after curing the slurry includes:

[0028] The separator slurry is spun to form a battery separator; or, the separator slurry is spun or coated on at least one side of a polymer base film to form a battery separator.

[0029] In the above technical scheme, the separator slurry can be directly spun into a non-woven membrane, or it can be formed on a polymer base membrane by spinning or coating. The preparation method is simple, and the thickness and pore size are controllable, so that the battery separator can be widely used in various battery systems.

[0030] In a third aspect, an embodiment of the present application provides a battery, comprising a positive electrode sheet, a negative electrode sheet, an electrolyte and the above-mentioned battery separator, wherein the battery separator is located between the positive electrode sheet and the negative electrode sheet, and the electrolyte infiltrates the positive electrode sheet, the negative electrode sheet and the battery separator. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 A schematic cross-sectional view of a battery separator provided in an embodiment of the present application;

[0033] Figure 2 A schematic cross-sectional view of another battery separator provided in an embodiment of the present application;

[0034] Figure 3 A schematic cross-sectional view of another battery separator provided in an embodiment of the present application.

[0035] Description of reference numerals:

[0036] 100-battery separator; 10-functional layer; 20-polymer base film. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0038] During the charge and discharge process of lithium-ion batteries, the continuous deintercalation of lithium ions causes structural distortion, and the transition metal ions in the positive electrode active material will slowly dissolve into the electrolyte and deposit on the negative electrode surface, thereby causing the negative electrode SEI film to be damaged and the battery cycle performance to decrease. In response to this problem, although there are studies on adding metal complexing agents such as porphine, porphyrin and their derivatives to the diaphragm, the applicant has found through research that these complexing agents cannot effectively improve the battery cycle performance in a long cycle system, and may even reduce the battery cycle stability.

[0039] Based on this, the researchers of this application discovered through creative research that porphyrin compound-grafted silicon particles obtained by grafting functionalized silicon particles with porphyrin compounds and adding them to battery separators not only have good safety and structural stability in long-cycle systems, but can also efficiently adsorb transition metal ions (such as corresponding ions of Fe, Co, Ni and Mn) released by the positive electrode material during the charge and discharge cycle, thereby effectively improving the cycle performance of the battery.

[0040] The following is a detailed description of a battery separator and a preparation method thereof and a battery according to an embodiment of the present application.

[0041] First, an embodiment of the present application provides a battery separator and a preparation method thereof. The battery separator includes porphyrin compound grafted silicon particles, inorganic oxides and polymers. The preparation method may include the following steps:

[0042] S1: dissolving a porphyrin compound having an alkenyl group in a first solvent and mixing the mixture with mercapto-functionalized silicon particles, and performing a grafting reaction under ultraviolet light to prepare porphyrin compound grafted silicon particles.

[0043] It should be noted that the porphyrin compound grafted silicon particles can be easily understood as a substance obtained by grafting and modifying silicon particles with a porphyrin compound. The porphyrin compound can be porphyrin, protoporphyrin, or a porphyrin derivative.

[0044] The general structural formula of the porphyrin compound grafted silicon particles is shown in formula (I):

[0045]

[0046] Among them, R3, R5, R7, R8, R 10 , R 12 , R 13 , R 15 , R 17 , R 18 , R 20 are each independently phenyl, vinyl, allyl, C n H 2n+1 , C n H 2n OH, C n H 2n CHO, C n H 2n COOH, C n H 2n COONa、C n H 2n COOLi, C n H 2n COOC n H 2n, C n H 2n SH, n is an integer between 0 and 20; i and j are each independently an integer between 0 and 10.

[0047] As an example, the mercapto-functionalized silicon particles may be 3-mercaptopropyl grafted silicon particles, and the porphyrin compound having an alkenyl group may include at least one of protoporphyrin, protoporphyrin monomethyl ester, protoporphyrin dimethyl ester, protoporphyrin monosodium salt, protoporphyrin disodium salt, protoporphyrin monolithium salt or protoporphyrin dilithium salt.

[0048] The temperature of the grafting reaction is 40 to 80° C., the time is 6 to 24 hours, and the first solvent can be methanol.

[0049] After the grafting reaction, the following steps may be performed: filtering and washing with methanol, and vacuum drying at 60-100°C.

[0050] As an example, when the porphyrin compound is protoporphyrin IX and the mercapto-functionalized silicon particles are 3-mercaptopropyl-functionalized silica gel, the preparation method of the porphyrin compound grafted silicon particles can be represented by the following structural formula:

[0051]

[0052] S2: dispersing the porphyrin compound grafted silicon particles, inorganic oxides and polymers in a second solvent and mixing them to form a diaphragm slurry, and curing the diaphragm slurry to form a battery diaphragm.

[0053] The mass ratio of the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer may be (1-99):(0-99):(0-99). As an example, the mass ratio of the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer is 10:10:80.

[0054] The inorganic oxide includes at least one of boehmite, alumina, silica, titania, ferric oxide or ferrous oxide.

[0055] The polymer includes at least one of polyvinylidene fluoride, poly(vinylidene fluoride hexafluoropropylene), polytetrafluoroethylene, polyhexafluoropropylene, polyacrylate, polymethacrylate, polyacrylamide, polymethacrylamide, epoxy resin, polyvinyl pyrrolidone, carboxymethyl cellulose, sodium carboxymethyl cellulose, cellulose or chitosan. The weight average molecular weight of the polymer is 0.1 to 3 million, for example but not limited to any one of 0.1, 0.5, 0.1, 0.1, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.10, 0.3 ...

[0056] The second solvent may be at least one of water, acetone, N-methylpyrrolidone (NMP) or N,N-dimethylformamide (DMF).

[0057] As an example, the method of curing the separator slurry to form a battery separator may include the steps of: directly spinning the separator slurry into a film, and drying it to obtain the battery separator. At this time, the structure of the corresponding battery separator 100 can be seen in Figure 1 .

[0058] The spinning may be electrostatic spinning, and the drying temperature may be 100° C. for 2 hours. In some embodiments, after drying, the method may further include: hot pressing to a predetermined thickness.

[0059] As an example, a method for curing a separator slurry to form a battery separator may include the steps of:

[0060] The separator slurry is spun or coated on at least one side of the polymer base film to form a functional layer to obtain a battery separator. At this time, the corresponding battery separator structure can be seen in Figure 2 and Figure 3 The battery separator 100 includes a polymer base film 20 and a functional layer 10 disposed on at least one side of the polymer base film 20 .

[0061] The thickness of the polymer base film is 1 nm to 100 μm. The material of the polymer base film may include at least one of polyethylene terephthalate, polyvinyl chloride, polyethylene, polyacrylonitrile, polypropylene, polyamide, polyetherimide, and polyvinylidene fluoride.

[0062] The specific coating method may be roller coating, spray coating, electrospray coating, ultrasonic spray coating, etc. The specific spinning method may be melt spinning or electrostatic spinning, etc.

[0063] It should be noted that since spinning and coating are both common and well-known preparation methods in the art, they can be set according to the conventional selection in the art during specific implementation, and will not be elaborated in detail here.

[0064] In addition, the present application also provides a battery separator prepared by the above preparation method, the thickness of the battery separator can be 1nm~100μm, and the battery separator has multiple pores, its porosity can be 30%~80%, and the pore size can be 0.1nm~100nm.

[0065] In addition, an embodiment of the present application also provides a battery, including a positive electrode sheet, a negative electrode sheet, an electrolyte and the above-mentioned battery separator, the battery separator is located between the positive electrode sheet and the negative electrode sheet, and the electrolyte infiltrates the positive electrode sheet, the negative electrode sheet and the battery separator.

[0066] It should be noted that the battery in the present application can be a lithium-ion battery, a lithium-sulfur battery, a sodium-ion battery, etc., and is not limited to this.

[0067] The features and performance of the present application are further described in detail below in conjunction with specific embodiments.

[0068] Example 1

[0069] The present application embodiment provides a battery C1, and the preparation method thereof comprises the following steps:

[0070] (1) Preparation of porphyrin-grafted silicon particles

[0071] Take 100g silicon particles (particle diameter is 100nm) and slowly add them to 1L of Piranha solution under magnetic stirring, then stir at 90℃ for 1h. After completion, filter and wash with a large amount of pure water and vacuum dry the silicon particles at 60℃. Then take the above activated silicon particles, then add 600mL of toluene solution of 3-mercaptopropyltrimethoxysilane with a concentration of 60mmol / L, and stir the reaction for 12h. Finally, filter and wash the above silicon particles with acetone and pure water, vacuum dry at 120℃ for use, and obtain 3-mercaptopropyl grafted silicon particles. Among them, the thiol loading is 0.3mmol / g.

[0072] 134.9 g of protoporphyrin IX (Aladdin, CAS: 553-12-8) was dissolved in 1214.1 g of anhydrous methanol, and then 100 g of 3-mercaptopropyl grafted silicon particles were added, stirred and dispersed at 60°C, and irradiated with ultraviolet light for 12 hours. After that, it was filtered and washed with 12000 g of anhydrous methanol, and then vacuum dried at 80°C to obtain protoporphyrin IX grafted silicon particles (Pr-Si for short).

[0073] (2) Preparation of battery separator

[0074] Take 80g of polyacrylonitrile (PAN for short, with a weight average molecular weight of 100,000), dissolve it in 900g of NMP, then add 10g of alumina and 10g of protoporphyrin IX grafted silicon particles, and disperse at high speed for 5h to obtain a diaphragm slurry. The obtained diaphragm slurry is made into a membrane by electrostatic spinning, then dried at 100℃ for 2h, and then hot pressed at 150℃ for 12h to obtain a battery diaphragm S1 with a thickness of 14μm. The porosity of the battery diaphragm S1 is 50% and the average pore size is 80nm.

[0075] (3) Preparation of positive electrode

[0076] Take 96g of lithium nickel manganese oxide (LNMO, chemical formula LiNi 0.5 Mn 1.5 O4), 1.8g polyvinylidene fluoride, and 2.2g conductive carbon were dispersed at high speed for 8 hours and then coated on both sides of an aluminum foil with a thickness of 12μm, then dried at 100℃ and cut into positive electrode sheets for use.

[0077] (4) Preparation of negative electrode

[0078] Take 95.6g of artificial graphite, 1.5g of carboxymethyl cellulose, 1.1g of conductive carbon, and 4.5g of styrene-butadiene rubber latex (solid content 40wt%), disperse them at high speed for 8h, then coat them on both sides of a copper foil with a thickness of 8μm, then dry them at 100℃, and cut them into negative electrode sheets for use.

[0079] (5) Preparation of batteries

[0080] The positive electrode sheet, negative electrode sheet and battery separator are taken as above to form a small soft-pack battery through a lamination process, and then the battery C1 is obtained by normal liquid injection, formation and capacity separation.

[0081] Example 2

[0082] The present embodiment provides a battery C2, which differs from the embodiment 1 only in that:

[0083] In step (2), the battery separator also includes a polymer base film, and the specific steps include: taking 80g of polyacrylonitrile (PAN for short, with a weight average molecular weight of 100,000), dissolving it in 900g of NMP, then adding 10g of aluminum oxide and 10g of protoporphyrin IX grafted silicon particles, and dispersing at high speed for 5h to obtain a separator slurry. The obtained separator slurry is deposited on one side of a polyethylene separator with a thickness of 12μm by electrospinning, then dried at 100℃ for 0.5h, and then hot pressed at 110℃ for 12h, and finally a battery separator S2 with a thickness of 13μm is obtained. The porosity of the battery separator S2 is 40% and the average pore size is 50nm.

[0084] Example 3

[0085] The present embodiment provides a battery C3, which differs from the embodiment 2 only in that:

[0086] In step (2), the separator slurry is deposited on two opposite surfaces of the polyethylene separator. The porosity of the battery separator S3 is 41% and the average pore size is 52 nm.

[0087] Example 4

[0088] The present embodiment provides a battery C4, which differs from the embodiment 2 only in that:

[0089] In step (2), the membrane slurry is coated on one side of the polyethylene membrane by a coating process. The porosity of the battery membrane S4 is 40% and the average pore size is 40 nm.

[0090] Example 5

[0091] The present embodiment provides a battery C5, which differs from the embodiment 4 only in that:

[0092] In step (2), the membrane slurry is coated on two opposite surfaces of the polyethylene membrane by a coating process. The porosity of the battery membrane S5 is 41% and the average pore size is 42 nm.

[0093] Example 6

[0094] The present embodiment provides a battery C6, which differs from the embodiment 1 only in that:

[0095] The positive electrode active material in step (3) is lithium nickel cobalt manganese oxide (referred to as NCM811, chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2).

[0096] Example 7

[0097] The present embodiment provides a battery C7, which differs from the embodiment 2 only in that:

[0098] The positive electrode active material in step (3) is lithium nickel cobalt manganese oxide (referred to as NCM811, chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2).

[0099] Example 8

[0100] The present embodiment provides a battery C8, which differs from the embodiment 3 only in that:

[0101] The positive electrode active material in step (3) is lithium nickel cobalt manganese oxide (referred to as NCM811, chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2).

[0102] Example 9

[0103] The present embodiment provides a battery C9, which differs from the embodiment 4 only in that:

[0104] The positive electrode active material in step (3) is lithium nickel cobalt manganese oxide (referred to as NCM811, chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2).

[0105] Example 10

[0106] The present embodiment provides a battery C10, which differs from the embodiment 5 only in that:

[0107] The positive electrode active material in step (3) is lithium nickel cobalt manganese oxide (referred to as NCM811, chemical formula LiNi 0.8 Co 0.1Mn 0.1 O2).

[0108] Embodiment 11

[0109] The present embodiment provides a battery C11, which differs from the embodiment 1 only in that:

[0110] In step (3), the positive electrode active material is lithium iron phosphate (LFP for short, chemical formula LiFePO4).

[0111] Example 12

[0112] The present embodiment provides a battery C12, which differs from the embodiment 2 only in that:

[0113] In step (3), the positive electrode active material is lithium iron phosphate (LFP for short, chemical formula LiFePO4).

[0114] Example 13

[0115] The present embodiment provides a battery C13, which differs from the embodiment 3 only in that:

[0116] In step (3), the positive electrode active material is lithium iron phosphate (LFP for short, chemical formula LiFePO4).

[0117] Embodiment 14

[0118] The present embodiment provides a battery C14, which differs from the embodiment 4 only in that:

[0119] In step (3), the positive electrode active material is lithium iron phosphate (LFP for short, chemical formula LiFePO4).

[0120] Embodiment 15

[0121] The present embodiment provides a battery C15, which differs from the embodiment 5 only in that:

[0122] In step (3), the positive electrode active material is lithium iron phosphate (LFP for short, chemical formula LiFePO4).

[0123] Comparative Example 1

[0124] The comparative example of the present application provides a battery R1, which is different from the embodiment 1 in that:

[0125] Excluding steps (1) and (2), the battery separator in step (5) is a conventional polyethylene separator with a thickness of 12 μm.

[0126] Comparative Example 2

[0127] The comparative example of the present application provides a battery R2, which differs from Example 6 in that:

[0128] Excluding steps (1) and (2), the battery separator in step (5) is a conventional polyethylene separator with a thickness of 12 μm.

[0129] Comparative Example 3

[0130] The comparative example of the present application provides a battery R3, which differs from Example 11 in that:

[0131] Excluding steps (1) and (2), the battery separator in step (5) is a conventional polyethylene separator with a thickness of 12 μm.

[0132] Comparative Example 4

[0133] The comparative example of the present application provides a battery R4, which is different from Example 1 in that:

[0134] In step (2), protoporphyrin IX is used to replace the protoporphyrin IX grafted silicon particles to prepare a battery separator RS-1 with a porosity of 50% and an average pore size of 70 nm.

[0135] For ease of review, some important preparation conditions of the batteries in Examples 1 to 15 and Comparative Examples 1 to 4 are listed in Table 1 below.

[0136] Table 1 Partial preparation conditions of batteries in Examples 1 to 15 and Comparative Examples 1 to 4

[0137]

[0138]

[0139] Test example

[0140] The performance of the diaphragms prepared in the above examples and comparative examples was tested, and the prepared batteries were cycled 1000 times at room temperature and 1C to test the cycle performance, and the content of transition metal ions in the electrolyte after 1000 cycles was measured. The specific test method is as follows:

[0141] 1. Battery separator performance test

[0142] The porosity and puncture strength of the battery separator were tested according to the GB / T 36363-2018 test standard, and the thermal shrinkage of the battery separator was tested according to the GB / T12027-2004 test standard, and compared with conventional polyethylene separators. The test results are shown in Table 2.

[0143] 2. Battery cycle performance test

[0144] The batteries of Examples 1 to 15 and the batteries prepared in Comparative Examples 1 to 4 were tested according to the following steps:

[0145] (1) Leave for 1 minute;

[0146] (2) Discharge from the open circuit voltage to the lower limit voltage at a constant current of 1C;

[0147] (3) Leave for 1 min;

[0148] (4) Charge at a constant current of 1C to the upper voltage limit, and then charge at a constant voltage of 0.05C;

[0149] (5) Leave for 1 min;

[0150] (6) Discharge at a constant current of 1C to the lower limit voltage;

[0151] (7) Leave for 1 min;

[0152] (8) Repeat steps (4) to (7) for 1000 times.

[0153] Among them, the voltage upper limit of Examples 1 to 5 and Comparative Examples 1 and 4 is 4.8V, and the voltage lower limit is 3.5V; the voltage upper limit of Examples 6 to 10 and Comparative Example 2 is 4.3V, and the voltage lower limit is 2.8V; the voltage upper limit of Examples 11 to 15 and Comparative Example 3 is 3.85V, and the voltage lower limit is 2.5V. The test results are shown in Table 3.

[0154] 3. Transition metal ion content test

[0155] The aluminum shell battery after 1000 cycles at room temperature was disassembled, and 0.5 g of free electrolyte was extracted, and then diluted to 10 g with dimethyl carbonate. The diluted sample was taken and the contents of Fe, Co, Ni, and Mn in the sample were determined by ICP external standard method. The measurement results are shown in Table 4.

[0156] Table 2 Battery separator performance test results of Examples 1 to 5 and Comparative Example 4

[0157]

[0158] As can be seen from Table 2, the battery separator prepared in the examples of the present application has comparable porosity and puncture strength to conventional polyethylene separators, but significantly reduced thermal shrinkage, indicating better safety and reliability.

[0159] Table 3 Cyclic performance test results of Examples 1 to 15 and Comparative Examples 1 to 4

[0160]

[0161]

[0162] Table 4 Transition metal ion content in Examples 1 to 15 and Comparative Examples 1 to 4

[0163]

[0164]

[0165] It can be seen from Table 3 and Table 4 that the batteries prepared in Examples 1 to 15 have a low content of transition metal ions in the electrolyte after 1000 cycles at room temperature 1C. Correspondingly, the batteries prepared in Examples 1 to 15 have a capacity retention rate of not less than 85% after 1000 cycles at room temperature 1C, and the capacity retention rate in Example 11 can be as high as 97%.

[0166] Comparing the performance test results of Example 1 and Comparative Example 1, it can be seen that the capacity retention rate of battery C1 is 92%, while in battery R1 of Comparative Example 1, the content of nickel and manganese ions in the electrolyte increases significantly, and the capacity retention rate decreases significantly to 65%. Comparing the performance test results of Example 6 and Comparative Example 2, it can be seen that the capacity retention rate of battery C6 is 95%, while in battery R2 of Comparative Example 2, the content of nickel ions, cobalt ions and manganese ions increases significantly, and the corresponding capacity retention rate decreases to 88%. Comparing the performance test results of Example 11 and Comparative Example 3, it can be seen that the capacity retention rate of battery C11 is 97%, while in battery R3 of Comparative Example 3, the content of iron ions increases, and the corresponding capacity retention rate decreases to 93%. It shows that the porphyrin compound grafted silicon particles in the battery separator can effectively adsorb the transition metal ions dissolved by the positive electrode material during the cycle process, enhance the cycle stability of the battery, and especially effectively improve the cycle performance of nickel manganese oxide lithium batteries.

[0167] By comparing the performance test results of Example 1 and Comparative Example 4, it can be seen that although pure porphyrin can also adsorb a certain amount of transition metal ions, the cycle performance is significantly worse than that of Example 1 during long-term cycling. This may be due to the poor stability of pure porphyrin and its slow electrochemical oxidation, which reduces the lithium ion permeability of the battery separator and increases the internal resistance of the battery.

[0168] The above-mentioned embodiments 1-5 and comparative examples 1 and 4 are batteries of a nickel manganese oxide lithium system, the above-mentioned embodiments 6-10 and comparative example 2 are batteries of a nickel cobalt manganese oxide lithium system, and the above-mentioned embodiments 11-15 and comparative example 3 are batteries of a lithium iron phosphate system. It can be seen from the contents of Tables 2 and 3 that for batteries of different positive electrode active material systems, the technical solution provided in the present application can efficiently adsorb transition metal ions dissolved from the positive electrode active material during the cycle by providing a battery separator including porphyrin compound grafted silicon particles, and effectively improve the cycle performance during a long cycle, especially effectively improve the cycle stability of the nickel manganese oxide lithium battery system.

[0169] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A battery separator, characterized in that: The battery separator comprises porphyrin compound grafted silicon particles, inorganic oxides and polymers. The battery separator has a plurality of pores, and the pore diameters of the pores are 0.1nm to 100nm.

2. The battery separator according to claim 1, characterized in that: The battery separator has a thickness of 1 nm to 100 μm.

3. The battery separator according to claim 1, characterized in that: The inorganic oxide comprises at least one of boehmite, alumina, silica, titanium dioxide, ferric oxide or ferrosinite; The polymer includes at least one of polyvinylidene fluoride, poly(vinylidene fluoride hexafluoropropylene), polytetrafluoroethylene, polyhexafluoropropylene, polyacrylate, polymethacrylate, polyacrylamide, polymethacrylamide, epoxy resin, polyvinyl pyrrolidone, carboxymethyl cellulose, sodium carboxymethyl cellulose, cellulose or chitosan.

4. The battery separator according to claim 1, characterized in that: The mass ratio of the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer is (1-99):(0-99):(0-99).

5. The battery separator according to claim 1, characterized in that: The battery separator comprises a functional layer and a polymer base film, wherein the functional layer comprises the porphyrin compound grafted silicon particles, the inorganic oxide and the polymer, and the functional layer is located on at least one side surface of the polymer base film.

6. The battery separator according to claim 5, characterized in that: The thickness of the polymer base film is 1 nm to 100 μm; Optionally, the material of the polymer base film includes at least one of polyethylene terephthalate, polyvinyl chloride, polyethylene, polyacrylonitrile, polypropylene, polyamide, polyetherimide, and polyvinylidene fluoride.

7. A method for preparing a battery separator according to any one of claims 1 to 6, characterized in that: The following steps are involved: Dissolving a porphyrin compound having an alkenyl group in a first solvent and mixing the mixture with mercapto-functionalized silicon particles, and performing a grafting reaction under ultraviolet light to prepare porphyrin compound grafted silicon particles; The porphyrin compound grafted silicon particles, inorganic oxides and polymers are dispersed in a second solvent and mixed to form a diaphragm slurry, and the diaphragm slurry is solidified to form a battery diaphragm.

8. The preparation method according to claim 7, characterized in that: The mercapto-functionalized silicon particles are 3-mercaptopropyl grafted silicon particles; The porphyrin compound having an alkenyl group includes at least one of protoporphyrin, protoporphyrin monomethyl ester, protoporphyrin dimethyl ester, protoporphyrin monosodium salt, protoporphyrin disodium salt, protoporphyrin monolithium salt or protoporphyrin dilithium salt; Optionally, the grafting reaction is carried out at a temperature of 40 to 80° C. and for a time of 6 to 24 hours.

9. The preparation method according to claim 7, characterized in that: The method for forming a battery separator by curing the slurry comprises: Spinning the separator slurry to form the battery separator; Alternatively, the separator slurry is spun or coated on at least one surface of a polymer base film to form a functional layer to obtain the battery separator.

10. A battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and a battery separator as claimed in any one of claims 1 to 6, wherein the battery separator is located between the positive electrode sheet and the negative electrode sheet, and the electrolyte infiltrates the positive electrode sheet, the negative electrode sheet and the battery separator.

Citation Information

Patent Citations

  • Diaphragm slurry capable of efficiently capturing metal ions, diaphragm and application of diaphragm

    CN111081953A

  • Ionic liquid composition, ion-conductive material, and electrolyte material

    JP2006202646A

  • Lithium ion-based internal hybrid electrochemical energy storage cell

    US20190108948A1

  • Sodium ion-based internal hybrid electrochemical energy storage cell

    US20190109358A1

  • Polymer electrolyte for a solid state battery

    US20240186564A1