Composite diaphragm, preparation method thereof and battery
By using a heat-resistant porous layer composed of inorganic fillers and organic binders with suitable particle size distribution in lithium-ion batteries, the internal resistance and cycle stability problems caused by local defects in the separator are solved, and a higher battery cycle life is achieved. Safety performance.
Patent Information
- Application Number
- CN202411393484.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
AI Technical Summary
Existing lithium-ion battery separators are prone to local defects, resulting in increased battery internal resistance and reduced cycle stability, thereby accelerating battery aging.
The composite separator is adopted, including a porous base film and a heat-resistant porous layer. The heat-resistant porous layer is composed of inorganic fillers and organic binders. The particle size distribution meets 0.5≤H≤1.2, ensuring the heat resistance and bonding properties of the composite separator and improving the Ion conductivity.
It effectively avoids local defects, improves the cycle life and safety of the battery, reduces internal resistance, and enhances the cycle stability and safety performance of the battery.
Smart Images

Figure BDA0005073089210000031 
Figure BDA0005073089210000041 
Figure BDA0005073089210000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a composite diaphragm and a preparation method thereof, and a battery. Background Art
[0002] As the secondary chemical power source with the highest energy density, lithium-ion batteries have been widely used in the field of portable power and energy storage. High-energy-density lithium battery systems are also widely used in energy storage and power supply. In application scenarios, hundreds of single cells are usually connected in series and parallel to form a battery system to meet the voltage or power requirements of the load. For the entire system, once a battery fails, the system maintenance cost is huge and may even lead to systemic risks.
[0003] The most typical example is thermal runaway. As described in the literature Lithium-Ion Battery Pack Robust State of Charge Estimation, Cell Inconsistency, and Balancing: Review, when a battery cell experiences thermal runaway, a large amount of heat will be generated. If this heat cannot be dissipated in time, the temperature inside the battery pack will rapidly increase. The high temperature will trigger thermal runaway of adjacent battery cells, forming a chain reaction, and ultimately leading to thermal runaway of the entire battery pack.
[0004] As a key component in electrochemical cells, the diaphragm is an inactive component, but it has a profound impact on the ion transport, performance, battery life and safety of the battery. As the battery's demand for diaphragm performance increases, the coating film plays an increasingly important role. Because coating can improve the thermal stability of the diaphragm, improve its mechanical strength, improve its puncture resistance, enhance the liquid retention and wettability of the diaphragm, etc. The focus of the existing technology on the coating is mainly on the performance characterization of the material that accounts for more than 90% of the coating composition. For example, the regulation of the particle size in the coating filler often only stipulates Dv90 and above, or at least stipulates the range of Dv50. For Dv10, Dv20, etc., there is often no regulation, and its impact is directly ignored. But just as the failure of a battery cell will affect the voltage and current distribution of the battery pack, causing other battery cells to overcharge or over-discharge, accelerate battery aging or trigger failure. For the diaphragm coating, if the performance of the component with a small content is poor, it will cause local defects, and this defect is often not detected when the diaphragm is tested, such as thermal shrinkage, adhesion test, puncture strength test, etc. The most typical manifestation of this defective diaphragm is that the diaphragm test is fine, but the cycle performance of the assembled battery cell deteriorates, which is related to the presence of micro defects in the diaphragm. For example: the presence of micro defects leads to poor local adhesion of the diaphragm, and the diaphragm adhesion test is to calculate the average value of adhesion over a distance (50mm, according to GB / T 2792-2014), so the diaphragm test meets the standard, but when assembled into a battery cell, the local adhesion of the diaphragm is poor due to the presence of micro defects. Local powder loss does not affect the battery capacity at first, but local powder loss will continue to spread, accelerating the battery aging process, and thus the battery cycle performance deteriorates. In addition, local powder loss will increase the local internal resistance of the battery, and internal resistance failure will cause the battery temperature to rise, and the temperature increase will aggravate the internal resistance failure, forming a vicious cycle and accelerating battery aging.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One object of the present invention is to provide a composite diaphragm to solve the technical problem that the diaphragm in the prior art is prone to local defects, thereby increasing the internal resistance of the battery, accelerating battery aging, and reducing the cycle stability of the battery. The composite diaphragm of the present invention can significantly reduce or avoid local defects, has good heat resistance, coating adhesion and ion conductivity, is conducive to reducing the internal resistance of the battery and improving the cycle stability of the battery.
[0007] Another object of the present invention is to provide a method for preparing the composite membrane, which is simple and easy to implement, environmentally friendly, and the obtained composite membrane has excellent heat resistance, coating adhesion and ionic conductivity.
[0008] Another object of the present invention is to provide a battery.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] A composite diaphragm comprises a porous base film and a heat-resistant porous layer located on at least one side of the porous base film, wherein the heat-resistant porous layer comprises an inorganic filler and an organic binder; and the particle size distribution of the inorganic filler satisfies:
[0011]
[0012] Among them, 0.5≤H≤1.2.
[0013] In some embodiments, the particle size of the inorganic filler is Dv10 of 0.3-0.8 μm, Dv20 of 0.5-0.9 μm, Dv30 of 0.6-1.1 μm, Dv40 of 0.7-1.2 μm, and Dv50 of 0.8-1.3 μm.
[0014] In some embodiments, the inorganic filler includes at least one of metal oxides, metal hydroxides, metal carbonates and metal sulfates, and the metal includes at least one of calcium, chromium, cerium, nickel, barium, aluminum, magnesium and zirconium.
[0015] In some embodiments, the organic binder includes at least one of a polyvinylidene fluoride-based resin and an acrylic polymer.
[0016] In some embodiments, the average particle size of the organic binder is 0.01-1 μm.
[0017] In some implementations, the mass ratio of the inorganic filler to the organic binder is (30-70):(10-30).
[0018] In some embodiments, the total mass of the inorganic filler and the organic binder accounts for more than 90% of the mass of the heat-resistant porous layer.
[0019] In some embodiments, the heat-resistant porous layer further includes an additive, wherein the additive includes at least one of a surfactant, a dispersant, a wetting agent, a tackifier, a leveling agent, a defoaming agent, and a pH regulator.
[0020] In some embodiments, the thickness of the heat-resistant porous layer on one side is 0.5 to 2 μm.
[0021] In some embodiments, the porous base membrane comprises a thermoplastic resin.
[0022] In some embodiments, the thickness of the porous base film is 5 to 10 μm, and the porosity of the base film is 30% to 60%.
[0023] In some embodiments, the ionic conductivity of the composite membrane is greater than or equal to 1.2×10 3 S / cm.
[0024] In some embodiments, the capacity retention rate of a battery prepared by the composite separator after 50 cycles is greater than or equal to 95%.
[0025] In some embodiments, the internal resistance increase rate of the battery prepared by the composite separator after 50 cycles is less than or equal to 6%.
[0026] The method for preparing the composite diaphragm as described above comprises the following steps:
[0027] An inorganic filler, an organic binder and a solvent are mixed, wherein the particle size distribution of the inorganic filler satisfies:
[0028]
[0029] Wherein, 0.5≤H≤1.2, and a coating slurry is obtained;
[0030] The coating slurry is coated on at least one side of the surface of the base film, and a composite diaphragm is obtained after drying.
[0031] In some implementations, the inorganic filler is mainly obtained by grinding an inorganic filler raw material, the grinding speed is 500-700 rpm, and the grinding time is 8-18 hours.
[0032] In some embodiments, the particle size of the inorganic filler is Dv10 of 0.3-0.8 μm, Dv20 of 0.5-0.9 μm, Dv30 of 0.6-1.1 μm, Dv40 of 0.7-1.2 μm, and Dv50 of 0.8-1.3 μm.
[0033] In some embodiments, the mass ratio of the inorganic filler, the organic binder and the solvent is (30-70):(10-30):(40-80).
[0034] In some embodiments, the coating slurry further includes additives, and the additives include at least one of a surfactant, a dispersant, a wetting agent, a tackifier, a leveling agent, a defoaming agent, and a pH regulator.
[0035] A battery comprises the composite diaphragm.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The composite diaphragm of the present invention has a particle size distribution of the inorganic filler in the heat-resistant porous layer that satisfies a specific relationship, and the H value is in the range of 0.5 to 1.2, which can effectively avoid local defects in the composite diaphragm coating. The composite diaphragm has good heat resistance, good bonding performance of the heat-resistant porous layer, and high ionic conductivity, which can improve the battery cycle life and safety of use.
[0038] (2) The preparation method of the composite diaphragm of the present invention is simple and easy. The particulate organic binder and the inorganic filler are dispersed, suspended or emulsified in a solvent in a solid state to obtain a coating slurry. The coating slurry is applied to one or both sides of the base film. After drying, a heat-resistant porous layer is formed to obtain a composite diaphragm.
[0039] (3) The battery prepared by the composite diaphragm of the present invention has excellent cycle performance and safety performance. DETAILED DESCRIPTION
[0040] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0041] According to one aspect of the present invention, the present invention relates to a composite diaphragm, comprising a porous base film and a heat-resistant porous layer located on at least one side of the porous base film, wherein the heat-resistant porous layer comprises an inorganic filler and an organic binder; and the particle size distribution of the inorganic filler satisfies:
[0042]
[0043] Among them, 0.5≤H≤1.2.
[0044] The composite diaphragm of the present invention has a particle size distribution of the inorganic filler in the heat-resistant porous layer that satisfies the above relationship, and the H value is in the range of 0.5 to 1.2, which can effectively avoid local defects in the diaphragm coating. The composite diaphragm has good heat resistance, good bonding performance of the heat-resistant porous layer, and high ionic conductivity, which can improve the battery cycle life and use safety. The ionic conductivity σ of the composite diaphragm is ≥1.2×10 3 S / cm, the capacity retention rate of the battery after 50 cycles is ≥95%, and the internal resistance increase rate of the battery after 50 cycles is ≤6%. When the H value is less than 0.5, it means that there are very small particles mixed in the sample. When the particle size is very small, the H value will change by an order of magnitude. Although the content is not high, the particles with very small particle size will cause the local air permeability of the diaphragm to deteriorate and the internal resistance to increase; when the H value is greater than 1.2, it means that there are a large number of large-size particles mixed in the system, which will reduce the adhesion of the diaphragm.
[0045] In some embodiments, the particle size Dv10 of the inorganic filler is 0.3-0.8 μm, Dv20 is 0.5-0.9 μm, Dv30 is 0.6-1.1 μm, Dv40 is 0.7-1.2 μm, and Dv50 is 0.8-1.3 μm. In some embodiments, the particle size Dv10 of the inorganic filler includes but is not limited to 0.3 μm, 0.35 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm or 0.8 μm, etc., or any range between the two. Dv20 includes but is not limited to 0.5 μm, 0.55 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, etc., or any range between the two. Dv30 includes but is not limited to 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, etc., or any range between them. Dv40 includes but is not limited to 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm or 1.2μm, etc., or any range between them. Dv40 includes but is not limited to 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, etc., or any range between them.
[0046] In some embodiments, the organic binder particles and the inorganic filler are interconnected to form a porous structure.
[0047] In some embodiments, the inorganic filler includes at least one of metal oxides, metal hydroxides, metal carbonates and metal sulfates, and the metal includes at least one of calcium, chromium, cerium, nickel, barium, aluminum, magnesium and zirconium. In some embodiments, the inorganic filler includes aluminum oxide, zirconium oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, magnesium carbonate, zirconium carbonate, aluminum sulfate, magnesium sulfate, etc. In some embodiments, the inorganic filler can be any one or a combination of the above, such as a combination of aluminum oxide and magnesium oxide, a combination of aluminum sulfate and zirconium oxide, etc.
[0048] In some embodiments, the organic binder includes at least one of a polyvinylidene fluoride resin and an acrylic polymer. The polyvinylidene fluoride resin includes polyvinylidene fluoride. The acrylic polymer includes methyl acrylate. The organic binder of the present invention is stable to the electrolyte, electrochemically stable, and has the function of connecting inorganic fillers. In some embodiments, the average particle size of the organic binder is 0.01 to 1 μm, including but not limited to 0.01 μm, 0.02 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.5 μm, 0.8 μm or 1 μm, etc., or any range value between the two.
[0049] In some embodiments, the mass ratio of the inorganic filler to the organic binder is (30-70):(10-30), for example, 30:10, 40:14, 50:23, 60:25, 70:30, etc.
[0050] In some embodiments, the heat-resistant porous layer also includes additives, and the additives include at least one of a surfactant, a dispersant, a wetting agent, a tackifier, a leveling agent, a defoamer, and a pH regulator. Within the scope of not hindering the effect of the present invention, additives can be further added to the heat-resistant porous layer of the present invention as needed. In some embodiments, the dispersant includes at least one of acrylic acid water-soluble polymers, styrene-acrylic acid (ester) copolymers, and maleic acid (ester)-acrylic acid (ester) copolymers. In some embodiments, the surfactant includes anionic surfactants, cationic surfactants, or amphoteric surfactants. Defoamers include at least one of ethylene glycol distearate and polyoxypropylene polyoxyethylene glycerol ether. Leveling agents include polyether silicones. Tackifiers include at least one of polyvinyl alcohol, cellulose, modified cellulose polymers, starch, and various modified starches. Wetting agents include sodium lauryl sulfate. pH regulators include at least one of sodium bicarbonate and disodium bicarbonate.
[0051] In some embodiments, the total mass of the inorganic filler and the organic binder accounts for more than 90% of the mass of the heat-resistant porous layer, such as 91%, 92%, 93%, 94%, 95%, 95%, 97%, etc., or any range between the two. The remainder is the content of the additive.
[0052] In some embodiments, the thickness of the heat-resistant porous layer on one side is 0.5 to 2 μm, including but not limited to 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, etc., or any range between the two. The heat-resistant porous layer of appropriate thickness is combined with the base film to ensure the heat resistance, peel strength and ionic conductivity of the composite separator.
[0053] In some embodiments, the porous base film includes a thermoplastic resin, and the interior of the porous base film has a suitable pore structure. The porous base film includes a porous sheet formed by a fibrous object such as a microporous film, a non-woven fabric, and a paper-like sheet, forming a film with a large number of micropores inside and a structure in which these micropores are connected, and a gas or liquid can pass from one side to the other side. In some embodiments, the porous base film includes a laminate of at least one or more of a PE film, a PP film, a PI film, a PET film, and a non-woven fabric separator, such as a PP / PE / PP film, a PP / PI film, etc. In some embodiments, the thickness of the base film is 5 to 10 μm, including but not limited to 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc., or any range value between the two. The porosity of the base film is 30% to 60%, for example, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc., or any range value between the two.
[0054] According to another aspect of the present invention, the present invention also relates to a method for preparing the composite diaphragm as described above, comprising the following steps:
[0055] An inorganic filler, an organic binder and a solvent are mixed, wherein the particle size distribution of the inorganic filler satisfies:
[0056]
[0057] Wherein, 0.5≤H≤1.2, and a coating slurry is obtained;
[0058] The coating slurry is coated on at least one side of the surface of the base film, and a composite diaphragm is obtained after drying.
[0059] The preparation method of the composite diaphragm of the present invention is simple and easy. The particulate organic binder and inorganic filler are dispersed, suspended or emulsified in a solvent in a solid state to obtain a coating slurry; the coating slurry is applied to one or both sides of the base film, and a heat-resistant porous layer is formed after drying to obtain a composite diaphragm.
[0060] In some embodiments, the inorganic filler is mainly obtained by grinding an inorganic filler raw material, the grinding speed is 500-700rpm, for example, 500rpm, 550rpm, 600rpm, 650rpm, 700rpm, etc., and the grinding time is 8-18h, for example, 8h, 10h, 12h, 15h, 18h, etc.
[0061] In some embodiments, in some embodiments, the particle size Dv10 of the inorganic filler is 0.3-0.8 μm, including but not limited to 0.3 μm, 0.35 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm or 0.8 μm, or any range between the two. Dv20 is 0.5-0.9 μm, including but not limited to 0.5 μm, 0.55 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, or any range between the two. Dv30 is 0.6-1.1 μm, including but not limited to 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, or any range between the two. Dv40 is 0.7-1.2 μm, including but not limited to 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm or 1.2 μm, or any range between them. Dv50 is 0.8-1.3 μm. Dv40 includes but is not limited to 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, or any range between them.
[0062] In some embodiments, the mass ratio of the inorganic filler, the organic binder and the solvent is (30-70):(10-30):(40-80), for example, 30:10:60, 50:20:70, 70:30:80, etc. The solvent includes water.
[0063] In some embodiments, the coating slurry further includes additives, and the additives include at least one of a surfactant, a dispersant, a wetting agent, a tackifier, a leveling agent, a defoaming agent, and a pH regulator.
[0064] In some embodiments, the drying temperature is 50-80° C., such as 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., etc., or any range therebetween. A suitable drying temperature is used to remove the solvent and form a heat-resistant porous layer in which the organic binder particles and the inorganic filler are interconnected.
[0065] According to another aspect of the present invention, the present invention also relates to a battery, comprising the composite separator.
[0066] The battery prepared by the composite diaphragm of the present invention has excellent cycle performance and good safety performance.
[0067] The battery of the present invention comprises a positive electrode sheet, a negative electrode sheet, the above-mentioned composite separator and an electrolyte. The positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer located on the surface of the positive electrode current collector, and the positive electrode active layer comprises a positive electrode active material, a binder and a conductive agent. The negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer located on the surface of the negative electrode current collector, and the negative electrode active layer comprises a negative electrode active material, a binder and a conductive agent. The electrolyte is a solution formed by dissolving a lithium salt in a non-aqueous solvent. The positive electrode sheet, the negative electrode sheet and the composite separator are assembled into a stack to form a battery cell. The battery cell is placed in an outer packaging material (such as an aluminum laminated film packaging), the electrolyte is injected, the battery cell is pressurized, and the performance test is performed after formation.
[0068] The following is further explained in conjunction with specific embodiments and comparative examples.
[0069] Example 1
[0070] A method for preparing a composite diaphragm comprises the following steps:
[0071] An aqueous emulsion (containing PMMA resin particles with a solid content of 36%), ceramic particles, carboxymethyl cellulose (CMC), and 2-propanol are uniformly dispersed in deionized water. The mass ratio of the aqueous emulsion, ceramic particles, carboxymethyl cellulose and 2-propanol is 35%:60%:3%:2% to obtain a coating slurry.
[0072] Among them, the particle size distribution of the ceramic particles is: Dv10 is 0.324μm, Dv20 is 0.517μm, Dv30 is 0.623μm, Dv40 is 0.715μm, and Dv50 is 0.809μm.
[0073]
[0074] H=0.680.
[0075] The ceramic particles are obtained by grinding a ceramic particle raw material in a ball mill at 600 rpm for 15 hours. The particle sizes of the ceramic particle raw material are: Dv10 is 0.576 μm, Dv20 is 0.694 μm, Dv30 is 0.838 μm, Dv40 is 0.989 μm, and Dv50 is 1.124 μm.
[0076] The coating slurry was applied to both sides of a polyethylene microporous membrane (membrane thickness: 7 μm, porosity: 37%, Gurley value: 155 sec / 100 cc) using a coating machine. The coating thickness was set to 1.5 μm and dried at 60°C to form a heat-resistant porous layer integrally formed on both sides of the polyethylene microporous membrane to obtain a composite diaphragm.
[0077] Example 2
[0078] A method for preparing a composite diaphragm, which differs from Example 1 in that:
[0079] The grinding time was 10 h, and the particle size distribution of the obtained ceramic particles was: Dv10 was 0.605 μm, Dv20 was 0.714 μm, Dv30 was 0.808 μm, Dv40 was 0.901 μm, Dv50 was 0.999 μm, and H=0.909.
[0080] Example 3
[0081] A method for preparing a composite diaphragm, which differs from Example 1 in that:
[0082] The grinding time was 8 h, and the particle size distribution of the obtained ceramic particles was: Dv10 was 0.799 μm, Dv20 was 0.891 μm, Dv30 was 0.989 μm, Dv40 was 1.096 μm, Dv50 was 1.222 μm, and H=1.121.
[0083] Example 4
[0084] A method for preparing a composite diaphragm, which differs from Example 1 in that:
[0085] The mass ratio of the water-based emulsion, the ceramic particles, the carboxymethyl cellulose and the 2-propanol is 40%:55%:3%:2%; and the coating thickness is 1 μm.
[0086] Example 5
[0087] A method for preparing a composite diaphragm comprises the following steps:
[0088] The aqueous emulsion (containing PMMA resin particles), zirconium oxide particles, carboxymethyl cellulose, and 2-propanol are uniformly dispersed in deionized water. The mass ratio of the aqueous emulsion, zirconium oxide particles, carboxymethyl cellulose, and 2-propanol is 30%:65%:3%:2% to obtain a coating slurry.
[0089] The particle size distribution of the zirconium oxide particles is as follows: Dv10 is 0.324 μm, Dv20 is 0.517 μm, Dv30 is 0.623 μm, Dv40 is 0.715 μm, and Dv50 is 0.809 μm.
[0090]
[0091] H=0.680.
[0092] The ceramic particles are obtained by grinding the ceramic particle raw material in a ball mill at 600 rpm for 15 hours. The particle sizes of the ceramic particle raw material are: Dv10 is 0.576 μm, Dv20 is 0.694 μm, Dv30 is 0.838 μm, Dv40 is 0.989 μm, and Dv50 is 1.124 μm.
[0093] The coating slurry was applied to both sides of a polyethylene microporous membrane (membrane thickness: 7 μm, porosity: 37%, Gurley value: 155 sec / 100 cc) using a coating machine. The coating thickness was 1.8 μm. The membrane was dried at 70°C to form a heat-resistant porous layer integrally formed on both sides of the polyethylene microporous membrane to obtain a composite diaphragm.
[0094] Comparative Example 1
[0095] A method for preparing a composite diaphragm, which differs from Example 1 in that:
[0096] The ceramic particle raw material is obtained by mixing component A and component B. The particle size of component A is: Dv10 is 0.576μm, Dv20 is 0.694μm, Dv30 is 0.838μm, Dv40 is 0.989μm, and Dv50 is 1.124μm; the particle size of component B is: Dv10 is 0.048μm, Dv20 is 0.053μm, Dv30 is 0.081μm, Dv40 is 0.092μm, and Dv50 is 0.098μm; the mass ratio of component A to component B is 95:5, and the grinding time is 10h. The particle size distribution of the obtained ceramic particles is: Dv10 is 0.051 μm, Dv20 is 0.566 μm, Dv30 is 0.683 μm, Dv40 is 0.781 μm, Dv50 is 0.873 μm, and H=0.417.
[0097] Comparative Example 2
[0098] A method for preparing a composite diaphragm, which differs from Example 1 in that:
[0099] The ceramic particle raw material is obtained by mixing component A and component C. The particle size of component A is: Dv10 is 0.576μm, Dv20 is 0.694μm, Dv30 is 0.838μm, Dv40 is 0.989μm, and Dv50 is 1.124μm; the particle size of component C is: Dv10 is 1.628μm, Dv20 is 1.912μm, Dv30 is 2.535μm, Dv40 is 2.898μm, and Dv50 is 3.237μm; the mass ratio of component A to component C is 95:5, and the grinding time is 10h. The particle size distribution of the obtained ceramic particles is: Dv10 is 0.773 μm, Dv20 is 0.971 μm, Dv30 is 1.295 μm, Dv40 is 1.462 μm, Dv50 is 1.681 μm, and H=1.406.
[0100] Experimental example
[0101] 1. The performance of the composite diaphragms in each embodiment and comparative example was tested as follows:
[0102] 1. Particle size test: Particle size test is carried out according to GB / T 19077-2016 "Particle size distribution laser diffraction method".
[0103] 2. Heat resistance test: Heat resistance test is carried out according to GB / T 12027-2004 "Test method for dimensional change rate of plastic film and sheeting upon heating".
[0104] 3. Adhesion test: Adhesion test is carried out according to GB / T 2792-2014 "Test method for peel strength of adhesive tape".
[0105] 4. Difference test: Cut the diaphragm into small pieces of 2.5 cm × 2.5 cm, and take 75 pieces in total; use a spiral micrometer (Mitutoyo, Japan) to measure the thickness.
[0106] 5. Ionic conductivity test: Punch the cut diaphragm with a punching machine with a diameter of 19μm. Prepare 5 diaphragm layers of 1, 2, 3, and 4 layers respectively to make button batteries (there are only diaphragms and electrolytes between the positive and negative shells). Use the AC impedance method to measure the EIS of the battery at an amplitude of 10mV and a frequency of 100kHz, and then calculate the ionic conductivity. Diaphragm ionic conductivity σ = L / (Rb*A); σ is ionic conductivity (S / cm); L is the thickness of the diaphragm (cm); Rb is the intrinsic resistance of the diaphragm (Ω); A is the effective area (cm 2 ).
[0107] The performance test results of the composite membrane are shown in Table 1.
[0108] Table 1 Performance test results of composite diaphragm
[0109]
[0110] As shown in Table 1, the composite membrane obtained by the method of the present invention has excellent heat resistance and coating adhesiveness, high uniformity and high ionic conductivity. Heat resistance (TD): less than or equal to 1.18%, heat resistance (MD): less than or equal to 1.92%; peel strength is 68-71N / m; thickness error is within ±0.4; ionic conductivity is 1.25×10 3 S / cm and above.
[0111] The composite diaphragms obtained in Comparative Examples 1 and 2 have a large thickness error, poor uniformity of the coating, and low ion conductivity.
[0112] 2. Battery performance test
[0113] The batteries prepared from the composite diaphragms of the embodiments and comparative examples specifically include:
[0114] Preparation of positive electrode sheet: 200g polyvinylidene fluoride, 200g conductive carbon black, 80g conductive graphite and 5kg nickel-cobalt-manganese ternary material were placed in a stirring tank, the speed was adjusted to 600rpm, and after stirring for 1h, 4.5kg N-methylpyrrolidone was added and continued to stir for 30min. After confirming that all powders were completely infiltrated, the vacuum was evacuated to -90kPa, the speed was adjusted to 1300rpm, and stirred for 4h. The positive electrode slurry was obtained, and the material was filtered out using a 150-mesh steel screen. The positive electrode slurry was applied to the surfaces of both sides of the positive current collector, dried, and then rolled to obtain the positive electrode sheet.
[0115] Preparation of negative electrode sheet: 80g sodium carboxymethyl cellulose, 160g conductive carbon black and 3.6kg artificial graphite are placed in a stirring tank, the speed is adjusted to 600rpm, and after stirring for 1h, 6.1kg of deionized water is added, and stirring is continued for 30min. After confirming that each powder is completely infiltrated, vacuum is evacuated to -90kPa, the speed is adjusted to 1300rpm, and stirring is continued for 4h. Then 200g of styrene-butadiene rubber latex is added, the speed is adjusted to 600rpm, stirring for 1h, and then 150g of N-methylpyrrolidone is added, and stirring is continued for 30min. The negative electrode slurry is obtained. The material is filtered out using a 150-mesh steel screen, and the negative electrode slurry is applied to the surfaces of both sides of the negative electrode current collector, and the negative electrode sheet is obtained after drying and rolling. The positive electrode sheet, negative electrode sheet, composite separator and electrolyte were assembled into a battery. The electrolyte composition was as follows: the electrolyte was 1M LiPF6, the solvent was ethylene carbonate (EC), diethyl carbonate (DEC) and propylene carbonate (PC), and the volume ratio of EC, DEC and PC was 60:30:10. The performance of each battery was tested.
[0116] Battery capacity test: Test the battery capacity according to GB / T 31486-2015 "Electrical performance requirements and test methods for power batteries for electric vehicles". ① Charge at 1C constant current to the upper voltage limit of 3.65V, then charge at 3.65V constant voltage until the charging current drops to 0.05C; ② Stand for 30 minutes; ③ Discharge at 1C constant current to the lower voltage limit of 2.5V; ④ Stand for 30 minutes. ①-④ are cycled 50 times in total.
[0117] Cyclic test: Cyclic test is carried out according to GB / T 4937.34-2024 "Mechanical and climatic test methods for semiconductor devices Part 34: Power cycling".
[0118] The performance test results of the batteries prepared by the composite diaphragms of the embodiments and comparative examples are shown in Table 2.
[0119] Table 2 Battery performance test results
[0120]
[0121] As can be seen from Table 2, the capacity retention rate of the battery prepared by the composite diaphragm obtained by the method of the present invention is high, and the capacity retention rate of the battery after 50 cycles is above 95%. The internal resistance change rate after 50 cycles of the battery is small, less than 6%.
[0122] The capacity retention rates of the batteries prepared by the composite diaphragms obtained by the methods of Comparative Examples 1 and 2 were relatively low, being 70.10% and 76.00% respectively, and the internal resistance change rates were relatively high, being 25.56% and 22.72% respectively.
[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite diaphragm, characterized in that: It comprises a porous base film and a heat-resistant porous layer located on at least one side of the porous base film, wherein the heat-resistant porous layer comprises an inorganic filler and an organic binder; The particle size distribution of the inorganic filler satisfies: Among them, 0.5≤H≤1.
2.
2. The composite diaphragm according to claim 1, characterized in that: The particle size Dv10 of the inorganic filler is 0.3-0.8 μm, Dv20 is 0.5-0.9 μm, Dv30 is 0.6-1.1 μm, Dv40 is 0.7-1.2 μm, and Dv50 is 0.8-1.3 μm.
3. The composite diaphragm according to claim 1, characterized in that: The inorganic filler includes at least one of metal oxides, metal hydroxides, metal carbonates and metal sulfates, and the metal includes at least one of calcium, chromium, cerium, nickel, barium, aluminum, magnesium and zirconium.
4. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (2): (1) The organic binder comprises at least one of a polyvinylidene fluoride resin and an acrylic polymer; (2) The average particle size of the organic binder is 0.01 to 1 μm.
5. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The mass ratio of the inorganic filler to the organic binder is (30-70):(10-30); (2) The total mass of the inorganic filler and the organic binder accounts for more than 90% of the mass of the heat-resistant porous layer; (3) The heat-resistant porous layer further includes additives, wherein the additives include at least one of a surfactant, a dispersant, a wetting agent, a thickener, a leveling agent, a defoaming agent and a pH regulator.
6. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The thickness of the heat-resistant porous layer on one side is 0.5 to 2 μm; (2) The porous base film comprises a thermoplastic resin; (3) The thickness of the porous base film is 5 to 10 μm, and the porosity of the porous base film is 30% to 60%.
7. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (3): (1) The ionic conductivity of the composite membrane is greater than or equal to 1.2×10 3 S / cm; (2) The capacity retention rate of the battery prepared by the composite diaphragm after 50 cycles is greater than or equal to 95%; (3) The internal resistance increase rate of the battery prepared by the composite diaphragm after 50 cycles is less than or equal to 6%.
8. The method for preparing a composite diaphragm according to any one of claims 1 to 7, characterized in that: The following steps are involved: An inorganic filler, an organic binder and a solvent are mixed, wherein the particle size distribution of the inorganic filler satisfies: Wherein, 0.5≤H≤1.2, and a coating slurry is obtained; The coating slurry is coated on at least one side of the surface of the base film, and a composite diaphragm is obtained after drying.
9. The method for preparing a composite diaphragm according to claim 8, characterized in that: The method comprises at least one of the following features (1) to (4): (1) The inorganic filler is mainly obtained by grinding the inorganic filler raw material, the grinding speed is 500-700 rpm, and the grinding time is 8-18 hours; (2) The particle size of the inorganic filler is Dv10 of 0.3-0.8 μm, Dv20 of 0.5-0.9 μm, Dv30 of 0.6-1.1 μm, Dv40 of 0.7-1.2 μm, and Dv50 of 0.8-1.3 μm; (3) The mass ratio of the inorganic filler, the organic binder and the solvent is (30-70):(10-30):(40-80). (4) The coating slurry further includes additives, wherein the additives include at least one of a surfactant, a dispersant, a wetting agent, a tackifier, a leveling agent, a defoaming agent and a pH regulator.
10. A battery, characterized in that: A composite diaphragm comprising any one of claims 1 to 7.