Porous carbon-magnetic metal particle composite wave-absorbing material as well as preparation method and application thereof
By loading magnetic metal particles in porous carbon materials, using magnetic metal salts and pore-forming agents to generate porous structures, the problems of impedance mismatch and limited absorption bandwidth of porous carbon materials in electromagnetic wave absorption are solved, and efficient electromagnetic wave absorption performance is achieved , suitable for multiple application fields.
Patent Information
- Application Number
- CN202411200663.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
The existing porous carbon materials have problems of impedance mismatch and limited absorption bandwidth in electromagnetic wave absorption, which is difficult to meet the needs of practical applications.
Porous carbon-magnetic metal particle composite material is used to generate porous structures and load magnetic metal particles through the synergistic effect of magnetic metal salts and pore-forming agents, so as to realize the multiple absorption mechanism of dielectric loss, magnetic loss and interface polarization loss, and adjust the Wave absorption performance.
It significantly improves the absorption performance, adjustable absorption strength and bandwidth, and is simple in preparation process. It is suitable for 5G communication, consumer electronics, wireless charging and other fields.
Smart Images

Figure CN119070032A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a porous carbon-magnetic metal particle composite absorbing material and a preparation method and application thereof. Background Art
[0002] With the rapid development of communication technology (especially the large-scale promotion and application of 5G communication technology), people's communication and entertainment life have become more and more convenient. However, electromagnetic radiation pollution caused by various complex electromagnetic environments will not only affect the normal operation of electronic equipment, but also endanger people's health. Therefore, high-performance electromagnetic wave absorbing materials for electromagnetic protection have attracted more and more attention, and their application fields have been continuously expanded.
[0003] Carbon materials (such as graphene, carbon nanotubes, porous carbon, etc.) have the advantages of low density, good high temperature resistance, and high conductivity, and are often used as dielectric absorbing materials. Porous carbon has the advantages of large specific surface area and adjustable pore shape and size, and has become a research hotspot for absorbing materials. However, the high conductivity of porous carbon easily causes impedance mismatch, and it only has dielectric loss as an absorbing mechanism, which is not conducive to expanding the absorption bandwidth of electromagnetic waves and is difficult to fully meet the requirements of practical applications.
[0004] Therefore, it is of great significance to develop an electromagnetic wave absorbing material with excellent wave absorbing performance, simple preparation process, safe and environmentally friendly raw materials. Summary of the invention
[0005] The purpose of the present invention is to provide a porous carbon-magnetic metal particle composite absorbing material and a preparation method and application thereof.
[0006] The technical solution adopted by the present invention is:
[0007] A porous carbon-magnetic metal particle composite wave absorbing material comprises a porous carbon carrier and loaded magnetic metal particles.
[0008] Preferably, the mass percentage of the magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 30% to 70%.
[0009] Preferably, the magnetic metal particles are at least one of cobalt particles, iron particles and nickel particles.
[0010] Preferably, the particle size of the magnetic metal particles is 30 nm to 300 nm.
[0011] Preferably, the BET specific surface area of the porous carbon-magnetic metal particle composite absorber is 700 m 2 / g~1200m 2 / g, and the average pore diameter is 3nm~10nm.
[0012] A method for preparing the porous carbon-magnetic metal particle composite absorbing material as described above comprises the following steps:
[0013] 1) adding water to dissolve the polysaccharide, then adding hydrochloric acid solution to partially hydrolyze (obtaining low molecular weight polysaccharide), then adding magnetic metal salt and pore-forming agent and mixing evenly to obtain a mixed solution;
[0014] 2) freeze-drying the mixed solution, calcining the obtained solid in an inert atmosphere, washing with water and drying the solid to obtain a porous carbon-magnetic metal particle composite absorbing material.
[0015] Preferably, in step 1), the mass ratio of the polysaccharide, water, hydrochloric acid solution, magnetic metal salt and pore-forming agent is 1:15-40:5-10:0.5-3:4-15.
[0016] Preferably, the polysaccharide in step 1) is at least one of starch, chitosan and chitin.
[0017] Preferably, the concentration of the hydrochloric acid solution in step 1) is 0.5 mol / L to 1.5 mol / L.
[0018] Preferably, the magnetic metal salt in step 1) is at least one of cobalt chloride, cobalt nitrate, cobalt sulfate, ferric chloride, ferric nitrate, nickel chloride, nickel nitrate and nickel sulfate.
[0019] Preferably, the pore-forming agent in step 1) is at least one of sodium chloride, potassium chloride and calcium carbonate.
[0020] Preferably, the mixing method in step 1) is stirring, the stirring rate is 300 rpm to 1000 rpm, and the stirring time is 30 min to 60 min.
[0021] Preferably, the freeze-drying in step 2) is carried out at a cold trap temperature of -40°C to -70°C, and the freeze-drying time is 24h to 48h.
[0022] Preferably, in step 2), the inert atmosphere is a nitrogen atmosphere or an argon atmosphere, and the flow rate of the inert gas is 30 mL / min to 60 mL / min.
[0023] Preferably, the calcination in step 2) comprises the following process: firstly controlling the heating rate to be 2°C / min-5°C / min from room temperature to 700°C-900°C, keeping the temperature for 2h-4h, and then naturally cooling to room temperature.
[0024] Preferably, the drying in step 2) is carried out at a temperature of 50° C. to 80° C., and the drying time is 6 h to 12 h.
[0025] An application of the porous carbon-magnetic metal particle composite absorbing material as described above in the fields of 5G communications, consumer electronics, wireless charging, or national defense and military industry.
[0026] Principle of the present invention: The present invention utilizes the synergistic effect of magnetic metal salt and pore-forming agent to realize the porous structure of polysaccharide after carbonization. The metal oxide generated by the magnetic metal salt during the calcination process can react with part of the carbon atoms, so that the metal ions are reduced and metal elements are generated in situ, and carbon dioxide and carbon monoxide are generated at the same time, so that the carbon material produces micropores. In addition, the pore-forming agent is further used as a salt template. After the salt template is removed by washing with water, a large number of larger pore structures can be formed in the carbon material, which ultimately increases the multiple reflection loss and interface polarization loss of electromagnetic waves inside the absorbing material, and greatly improves the absorbing performance of the absorbing material.
[0027] The beneficial effects of the present invention are: the porous carbon-magnetic metal particle composite absorbing material of the present invention has multiple loss mechanisms such as dielectric loss, magnetic loss, and multiple interface polarization loss, excellent absorbing performance, adjustable absorption intensity and bandwidth, simple preparation process, variable material composition and structure, and is suitable for 5G communications, consumer electronics, wireless charging, national defense and military industries and other fields.
[0028] Specifically:
[0029] 1) The present invention utilizes the contact between magnetic metal salt and carbon material to generate carbon oxides, so that the carbon material generates micropores, and at the same time, the metal ions are reduced into metal element particles loaded on the porous carbon surface through an in-situ reduction reaction to obtain a carbon-magnetic composite material, and finally the absorbing material has a synergistic multiple absorbing mechanism of dielectric loss, magnetic loss, interface polarization loss and multiple reflection loss;
[0030] 2) The present invention can change the composition of magnetic metal particles and carbon in the absorbing material and the microstructure of porous carbon by adjusting the ratio of magnetic metal salt, pore former and polysaccharide, and finally adjust the electromagnetic parameters of the absorbing material to achieve a minimum reflection loss of the absorbing material lower than -50dB, an effective absorption bandwidth greater than 5GHz, and a matching thickness less than 3.00mm;
[0031] 3) The preparation process of the porous carbon-magnetic metal particle composite absorbing material of the present invention is simple, green and environmentally friendly. By changing the calcination temperature and the insulation time, the carbonization degree of the porous carbon and the reduction degree of the metal salt can be controlled, thereby adjusting the electromagnetic parameters of the absorbing material, significantly improving the impedance matching, and enhancing the absorbing performance of the absorbing material. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the preparation process of the porous carbon-magnetic metal particle composite absorbing material of the present invention.
[0033] Figure 2 This is the SEM image of the porous carbon-magnetic metal particle composite absorbing material of Example 1.
[0034] Figure 3 This is the nitrogen adsorption-desorption isotherm curve of the porous carbon-magnetic metal particle composite absorbing material of Example 1.
[0035] Figure 4 The minimum reflection loss of the porous carbon-magnetic metal particle composite absorbing materials of Examples 1 to 5 and the absorbing materials of Comparative Examples 1 to 2 varies with frequency. DETAILED DESCRIPTION
[0036] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0037] Embodiment 1:
[0038] A porous carbon-magnetic metal particle composite absorbing material, the preparation method of which is as follows (the preparation process diagram is as follows Figure 1 shown):
[0039] 1) Add chitosan to deionized water, stir for 5 min at a stirrer speed of 400 rpm, then add a hydrochloric acid solution with a concentration of 1 mol / L, adjust the stirrer speed to 750 rpm and continue stirring for 30 min, then add CoCl2 and NaCl, and continue stirring for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, CoCl2, and NaCl is 1:26:7:2:11, and a mixed solution is obtained;
[0040] 2) The mixed solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is controlled to be 4°C / min from room temperature to 750°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain a porous carbon-magnetic metal particle composite absorbing material (the mass percentage of magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 52.5%).
[0041] Performance Test:
[0042] 1) The scanning electron microscope (SEM) image of the porous carbon-magnetic metal particle composite absorber of this embodiment is as follows: Figure 2 shown.
[0043] Depend on Figure 2It can be seen that the surface of the porous carbon-magnetic metal particle composite absorbing material presents a rich pore structure, and granular magnetic metal particles are attached to the porous carbon surface, and the particle size of the magnetic metal particles is 50nm to 200nm.
[0044] 2) The nitrogen adsorption-desorption isotherm curve of the porous carbon-magnetic metal particle composite absorber of this embodiment is as follows Figure 3 shown.
[0045] Depend on Figure 3 It can be seen that the BET specific surface area of the porous carbon-magnetic metal particle composite absorber is 978m 2 / g, and contains rich pore structure inside, with the average pore diameter of 3nm to 10nm. Such a porous structure is conducive to enhancing the multiple losses of electromagnetic waves.
[0046] Embodiment 2:
[0047] A porous carbon-magnetic metal particle composite absorbing material, the preparation method of which is as follows (the preparation process diagram is as follows Figure 1 shown):
[0048] 1) adding chitosan to deionized water, stirring for 5 min at a stirrer speed of 400 rpm, then adding a hydrochloric acid solution with a concentration of 1 mol / L, adjusting the stirrer speed to 750 rpm and continuing to stir for 30 min, then adding FeCl3 and NaCl, and continuing to stir for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, FeCl3, and NaCl is 1:26:7:2:11, and obtaining a mixed solution;
[0049] 2) The mixed solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is controlled to be 4°C / min from room temperature to 750°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain a porous carbon-magnetic metal particle composite absorbing material (the mass percentage of magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 52.5%).
[0050] Performance Test:
[0051] 1) The results of scanning electron microscopy test show that the surface of the porous carbon-magnetic metal particle composite absorbing material of this embodiment also presents a rich pore structure, and granular magnetic metal particles are attached to the porous carbon surface, and the particle size of the magnetic metal particles is 100nm to 180nm;
[0052] 2) The nitrogen adsorption-desorption test results show that the porous carbon-magnetic metal particle composite absorbing material of this embodiment and the porous carbon-magnetic metal particle composite absorbing material of Example 1 have highly similar pore structures.
[0053] Embodiment 3:
[0054] A porous carbon-magnetic metal particle composite absorbing material, the preparation method of which is as follows (the preparation process diagram is as follows Figure 1 shown):
[0055] 1) Add chitosan to deionized water, stir for 5 min at a stirrer speed of 400 rpm, then add a hydrochloric acid solution with a concentration of 1 mol / L, adjust the stirrer speed to 750 rpm and continue stirring for 30 min, then add CoCl2 and NaCl, and continue stirring for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, CoCl2, and NaCl is 1:26:7:2:11, and a mixed solution is obtained;
[0056] 2) The mixed solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is controlled to be 4°C / min from room temperature to 700°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain a porous carbon-magnetic metal particle composite absorbing material (the mass percentage of magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 52.5%).
[0057] After testing (the testing method is the same as that of Example 1), the microstructure of the porous carbon-magnetic metal particle composite absorbing material of this example is highly similar to that of the porous carbon-magnetic metal particle composite absorbing material of Example 1.
[0058] Embodiment 4:
[0059] A porous carbon-magnetic metal particle composite absorbing material, the preparation method of which is as follows (the preparation process diagram is as follows Figure 1 shown):
[0060] 1) Add chitosan to deionized water, stir for 5 min at a stirrer speed of 400 rpm, then add a hydrochloric acid solution with a concentration of 1 mol / L, adjust the stirrer speed to 750 rpm and continue stirring for 30 min, then add CoCl2 and NaCl, and continue stirring for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, CoCl2, and NaCl is 1:26:7:3:11, and a mixed solution is obtained;
[0061] 2) The mixed solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is controlled to be 4°C / min from room temperature to 750°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain a porous carbon-magnetic metal particle composite absorbing material (the mass percentage of magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 62.4%).
[0062] After testing (the testing method is the same as that of Example 1), the microstructure of the porous carbon-magnetic metal particle composite absorbing material of this example is highly similar to that of the porous carbon-magnetic metal particle composite absorbing material of Example 1.
[0063] Embodiment 5:
[0064] A porous carbon-magnetic metal particle composite absorbing material, the preparation method of which is as follows (the preparation process diagram is as follows Figure 1 shown):
[0065] 1) Add chitosan to deionized water, stir for 5 min at a stirrer speed of 400 rpm, then add a hydrochloric acid solution with a concentration of 1 mol / L, adjust the stirrer speed to 750 rpm and continue stirring for 30 min, then add CoCl2, NaCl and KCl, and continue stirring for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, CoCl2, NaCl, and KCl is 1:26:7:2:3:8, and a mixed solution is obtained;
[0066] 2) The mixed solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is controlled to be 4°C / min from room temperature to 750°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain a porous carbon-magnetic metal particle composite absorbing material (the mass percentage of magnetic metal particles in the porous carbon-magnetic metal particle composite absorbing material is 52.5%).
[0067] After testing (the testing method is the same as that of Example 1), the microstructure of the porous carbon-magnetic metal particle composite absorbing material of this example is highly similar to that of the porous carbon-magnetic metal particle composite absorbing material of Example 1.
[0068] Comparative Example 1:
[0069] A wave absorbing material, the preparation method of which is as follows:
[0070] 1) adding chitosan to deionized water, stirring for 5 min at a stirrer speed of 400 rpm, then adding a hydrochloric acid solution with a concentration of 1 mol / L, adjusting the stirrer speed to 750 rpm and continuing to stir for 30 min, then adding NaCl, and continuing to stir for 60 min, the mass ratio of chitosan, deionized water, hydrochloric acid solution, and NaCl is 1:26:7:11, to obtain a mixed solution;
[0071] 2) The mixed solution was placed in a cylindrical container for freeze drying, the cold trap temperature was -60 ° C, the freeze drying time was 36 hours, and the obtained solid was placed in a tubular furnace, nitrogen was introduced at a flow rate of 50 mL / min, and the heating rate was controlled to be 4 ° C / min from room temperature to 750 ° C, and the temperature was kept for 2 hours. After naturally cooling to room temperature, the calcined product was washed with deionized water for 5 times, and then vacuum dried at 80 ° C for 8 hours to obtain the absorbing material.
[0072] Comparative Example 2:
[0073] A wave absorbing material, the preparation method of which is as follows:
[0074] 1) adding chitosan to deionized water, stirring for 5 min at a stirrer speed of 400 rpm, then adding a hydrochloric acid solution with a concentration of 1 mol / L, adjusting the stirrer speed to 750 rpm and continuing stirring for 30 min to obtain a low molecular weight chitosan solution;
[0075] 2) The low molecular weight chitosan solution is placed in a cylindrical container for freeze drying, the cold trap temperature is -60°C, the freeze drying time is 36 hours, and then the obtained solid is placed in a tubular furnace, nitrogen is introduced at a flow rate of 50 mL / min, and the heating rate is first controlled to be 4°C / min from room temperature to 750°C, and the temperature is kept for 2 hours. After naturally cooling to room temperature, the calcined product is washed with deionized water 5 times, and then vacuum dried at 80°C for 8 hours to obtain the absorbing material.
[0076] Performance Test:
[0077] 1) The porous carbon-magnetic metal particle composite absorbing materials of Examples 1 to 5 and the absorbing materials of Comparative Examples 1 to 2 were respectively mixed with paraffin wax at a mass ratio of 3:7, and then pressed into coaxial rings with an outer diameter of 7.00 mm and an inner diameter of 3.04 mm. The absorbing performance was tested by the coaxial method. The absorbing performance test results are shown in the following table:
[0078] Table 1 Wave absorbing performance test results
[0079]
[0080] Note:
[0081] Absorption performance: The complex dielectric constant and complex magnetic permeability of the absorbing material sample are tested by a vector network analyzer through the coaxial method. The test frequency range is 2GHz to 18GHz. According to the transmission line theory, the complex dielectric constant and complex magnetic permeability of the absorber at a given frequency and the thickness of the absorbing material are used to calculate the reflection loss (RL):
[0082] The reflection loss of a single-layer absorber is calculated by formula (1):
[0083] Formula (1): Where Z0 is the free space impedance, which is approximately 377, and Z in is the standardized input impedance, calculated as shown in formula (2):
[0084] Formula (2): Z in =(μ r / ε r ) 1 / 2 tanh[j(2πfd / c)(μ r ε r ) 1 / 2 ], where μ r is the free space permeability and the relative permeability of the material, ε r are the free space dielectric constant and the relative dielectric constant of the material, j represents the imaginary part, f is the frequency, d is the sample thickness, and c is the speed of light.
[0085] It can be seen from Table 1 that the porous carbon-magnetic metal particle composite absorbing material prepared by adding a pore-forming agent and a magnetic metal salt in Examples 1 to 5 has a significantly reduced minimum reflection loss and a significantly increased maximum effective absorption bandwidth (reflection loss RL<-10dB) compared with the absorbing material prepared by direct calcination and the absorbing material prepared by adding only a pore-forming agent in Comparative Examples 1 to 2; in Examples 1 to 5, by adjusting the process parameters (for example, calcination temperature and holding time) and adjusting the mass ratio of the pore-forming agent, the magnetic metal salt and the polysaccharide, the maximum effective absorption bandwidth of the prepared porous carbon-magnetic metal particle composite absorbing material is greater than 5GHz, up to 6.7GHz, and the reflection loss is generally less than -35dB, and the lowest is -63.5dB, indicating that by adding a magnetic metal salt to assist in pore formation and in-situ reduction to produce a magnetic metal element during the calcination process, not only the dielectric loss capacity of the absorbing material is greatly improved, but also additional magnetic loss and polarization loss mechanisms are brought about. In addition, the impedance mismatch problem of the porous carbon material is improved, and excellent absorbing performance is obtained.
[0086] 2) Minimum reflection loss (RL) of the porous carbon-magnetic metal particle composite absorbing materials of Examples 1 to 5 and the absorbing materials of Comparative Examples 1 to 2 min ) changes with frequency as shown in the curve Figure 4 shown.
[0087] Depend on Figure 4 It can be seen that compared with the absorbing materials of Comparative Examples 1 to 2, the minimum reflection loss of the porous carbon-magnetic metal particle composite absorbing materials of Examples 1 to 5 is significantly reduced, and the effective absorption bandwidth (reflection loss RL<-10dB) is significantly increased, indicating that its absorbing performance is greatly improved.
[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A porous carbon-magnetic metal particle composite absorbing material, characterized in that: The composition includes a porous carbon support and supported magnetic metal particles.
2. The porous carbon-magnetic metal particle composite absorbing material according to claim 1, characterized in that: The mass percentage of the magnetic metal particles in the porous carbon-magnetic metal particle composite wave absorbing material is 30% to 70%.
3. The porous carbon-magnetic metal particle composite absorbing material according to claim 1 or 2, characterized in that: The magnetic metal particles are at least one of cobalt particles, iron particles and nickel particles.
4. The porous carbon-magnetic metal particle composite absorbing material according to claim 1 or 2, characterized in that: The particle size of the magnetic metal particles is 30nm to 300nm.
5. The porous carbon-magnetic metal particle composite absorbing material according to claim 1 or 2, characterized in that: The BET specific surface area of the porous carbon-magnetic metal particle composite absorber is 700 m 2 / g~1200m 2 / g, and the average pore diameter is 3nm~10nm.
6. A method for preparing the porous carbon-magnetic metal particle composite absorbing material according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) dissolving the polysaccharide in water, then adding hydrochloric acid solution to partially hydrolyze it, then adding magnetic metal salt and pore-forming agent and mixing them evenly to obtain a mixed solution; 2) freeze-drying the mixed solution, calcining the obtained solid in an inert atmosphere, washing with water and drying the solid to obtain a porous carbon-magnetic metal particle composite absorbing material.
7. The preparation method according to claim 6, characterized in that: The mass ratio of the polysaccharide, water, hydrochloric acid solution, magnetic metal salt and pore-forming agent in step 1) is 1:15-40:5-10:0.5-3:4-15; the concentration of the hydrochloric acid solution in step 1) is 0.5 mol / L-1.5 mol / L.
8. The preparation method according to claim 6 or 7, characterized in that: The polysaccharide in step 1) is at least one of starch, chitosan, and chitosan; the magnetic metal salt in step 1) is at least one of cobalt chloride, cobalt nitrate, cobalt sulfate, ferric chloride, ferric nitrate, nickel chloride, nickel nitrate, and nickel sulfate; the pore-forming agent in step 1) is at least one of sodium chloride, potassium chloride, and calcium carbonate.
9. The preparation method according to claim 6 or 7, characterized in that: The freeze drying in step 2) is carried out under the condition of a cold trap temperature of -40°C to -70°C, and the freeze drying time is 24h to 48h; the calcination in step 2) includes the following process: firstly control the heating rate to be 2°C / min to 5°C / min from room temperature to 700°C to 900°C, keep warm for 2h to 4h, and then cool naturally to room temperature.
10. An application of the porous carbon-magnetic metal particle composite absorbing material as described in any one of claims 1 to 5 in the field of 5G communications, consumer electronics, wireless charging or national defense and military industry.
Citation Information
Cited By
Confined range assembly method of superstructure magnetic material and product
CN119730218A