Artificial retina and manufacturing method thereof

By forming a porous structure of microfibers on the film and fixing organic pigment compounds, the problem of insufficient biocompatibility of artificial retinal in the prior art is solved, high-sensitivity photostimulation receptor potential and liquid permeability are achieved, and retinal tissue is enhanced stability of bonding.

CN119072289APending Publication Date: 2024-12-03UNIV OKAYAMA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380035596.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-03-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the artificial retina cannot pass through fluids such as body fluids or blood, resulting in insufficient biocompatibility and ineffective in alleviating visual impairments related to the optic nerve.

Method used

By fixing the organic pigment compound on the film sheet, a porous structure of fine fibers with an average fiber diameter of 2 to 1000 nm is formed, and the organic pigment compound is fixed on the fine fibers by covalent bonds to form an artificial retina with liquid permeability.

Benefits of technology

High-sensitivity photostimulation receptor potential induction is achieved, biocompatibility is improved, body fluids or blood can pass through, binding stability with retinal tissue, and effectively inhibit the deterioration of retinal tissue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072289A_ABST
    Figure CN119072289A_ABST
Patent Text Reader

Abstract

The present invention provides an artificial retina in which an organic dye compound is fixed to a film sheet, the artificial retina being characterized in that the organic dye compound induces a receptor potential corresponding to photostimulation, and the film sheet is obtained by connecting fine fibers having an average fiber diameter of 2-1000 nm and forming a porous structure. The porous structure has liquid permeability. As a result, provided is an artificial retina which is capable of inducing a receptor potential corresponding to photostimulation with high sensitivity, and which is capable of improving biocompatibility due to liquid permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an artificial retina in which an organic pigment compound that induces a receptor potential corresponding to light stimulation is fixed in the optic nerve, and a method for producing the same. Background Art

[0002] Among organic pigment compounds, some are known to induce a receptor potential corresponding to light stimulation in the optic nerve, particularly in the retinal nerve cells constituting the optic nerve. Research on retinal substitute materials using such organic pigment compounds is also underway.

[0003] Patent document 1 records a receptor potential inducer containing an organic pigment compound that induces a receptor potential corresponding to light stimulation in the optic nerve. Accordingly, the receptor potential inducer is very useful as a material to replace vision-related substances in retinal replacement materials represented by the following artificial retina. The above-mentioned artificial retina is used to alleviate or eliminate visual disorders such as narrow visual field, low vision, night blindness, drug poisoning, neural disorders of the visual center, retinal diseases, and color vision abnormalities caused by specific pituitary insufficiency due to retinal disorders associated with injuries.

[0004] In addition, a method for manufacturing an artificial retina is described in patent document 2, which is used to manufacture an artificial retina in which an organic pigment compound that induces a receptor potential corresponding to light stimulation is fixed on a substrate composed of a polymer sheet, and the manufacturing method includes: a bonding process of immersing a substrate in a solution containing an organic pigment compound to chemically bond the organic pigment compound to the substrate; a first cleaning process of washing the substrate chemically bonded with the organic pigment compound with water; and a second cleaning process of washing the substrate chemically bonded with the organic pigment compound with an organic solvent after the first cleaning process. Accordingly, an artificial retina having excellent mechanical properties such as elongation at break, good bioaffinity, and capable of inducing a receptor potential corresponding to light stimulation with high sensitivity can be obtained.

[0005] However, the artificial retinas described in these patent documents are formed by fixing an organic pigment compound on a polyethylene film or the like, and liquids such as body fluids and blood cannot pass through them.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2004-121292

[0009] Patent Document 2: WO2015 / 152233 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The present invention is made to solve the above-mentioned technical problems, and its purpose is to provide an artificial retina that can induce receptor potentials corresponding to light stimulation with high sensitivity and improve biocompatibility by having liquid permeability.

[0012] Technical solutions to solve problems

[0013] The above technical problem is solved by providing the following artificial retina, which is characterized in that it is made of an organic pigment compound fixed on a thin film, the organic pigment compound induces a receptor potential corresponding to light stimulation, and the thin film is obtained by connecting fine fibers with an average fiber diameter of 2 to 1000 nm to form a porous structure, and has liquid permeability through the porous structure.

[0014] In this case, the organic pigment compound is preferably fixed to the fine fibers in the film sheet by covalent bonds, and the fine fibers are preferably biocompatible.

[0015] In addition, the above technical problem is solved by providing the following method for manufacturing an artificial retina, which is used to manufacture the above artificial retina, characterized in that the above-mentioned microfibers having carboxyl groups are modified with diamines, and the above-mentioned organic pigment compound is reacted with the above-mentioned microfibers modified with diamines to fix them on the above-mentioned microfibers modified with diamines, and then a thin film sheet is prepared in a manner that the above-mentioned microfibers are connected to each other to form a porous structure.

[0016] Furthermore, the above technical problem is solved by providing the following method for manufacturing an artificial retina, which is used to manufacture the above artificial retina, characterized in that after a thin film sheet is prepared in a manner in which the above-mentioned microfibers are connected to each other to form a porous structure, the above-mentioned microfibers having carboxyl groups constituting the above-mentioned thin film sheet are subjected to diamine modification, and the above-mentioned organic pigment compound is reacted with the above-mentioned diamine-modified microfibers constituting the above-mentioned thin film sheet, thereby fixing the organic pigment compound on the above-mentioned diamine-modified microfibers constituting the above-mentioned thin film sheet.

[0017] Effects of the Invention

[0018] The present invention can provide an artificial retina that can induce a receptor potential corresponding to light stimulation with high sensitivity and has improved biocompatibility by having liquid permeability. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a photograph of the TOCN porous body of Example 1.

[0020] Figure 2 This is a photograph of the pigment-fixing film sheet of Example 1.

[0021] Figure 3 This is the EDX spectrum of the pigment-fixing film sheet of Example 1.

[0022] Figure 4 This is a graph showing the amount of change in the surface potential of the dye-fixing film sheet of Example 1.

[0023] Figure 5 IR spectra of the TOCN film and TOCN-COOH film of Example 2.

[0024] Figure 6 This is a photograph of the dye-fixed TOCN-COOH film sheet of Example 2.

[0025] Figure 7 This is the EDX spectrum of the dye-fixed TOCN-COOH thin film of Example 2.

[0026] Figure 8 This is a graph showing the amount of change in the surface potential of the dye-fixed TOCN-COOH thin film of Example 2.

[0027] Fig. 9 These are the UV-visible absorbance measurement results of the dye-fixed TOCN-COOH film of Example 2 and the existing dye-fixed film. DETAILED DESCRIPTION

[0028] The artificial retina of the present invention is characterized in that the artificial retina is formed by fixing an organic pigment compound on a thin film, the organic pigment compound induces a receptor potential corresponding to light stimulation, and the thin film is obtained by connecting fine fibers with an average fiber diameter of 2 to 1000 nm to form a porous structure, and has liquid permeability through the porous structure. Since the porous structure is formed by connecting fine fibers with an average fiber diameter of 2 to 1000 nm, it has liquid permeability and has the advantage of improving biocompatibility. In the present invention, liquid permeability refers to the liquid that penetrates from the surface of the artificial retina passing through to the back.

[0029] As the organic pigment compound used in the present invention, as long as it is the compound that induces the receptor potential corresponding to the light stimulus, it is not particularly limited, for example, acridine system, azacyclopentene system, azo system, anthraquinone system, indigo system, indanthrene system, oxazine system, xanthene system, coumarin system, dioxazine system, thiazine system, thioindigo system, tetrazoporphine (tetraporphyrazine) system, triphenylmethane system, triphenothiazine system, naphthoquinone system, phthalocyanine system, benzoquinone system, benzopyran system, benzofuranone system, polymethine system, porphyrin system, rhodamine system compound can be listed. Wherein, the organic pigment compound of polymethine system is suitable for use. As specific examples of the polymethine-based organic dye compound, compounds exemplified by Chemical Formulas 1 to 17 in Japanese Patent No. 5090431 and compounds exemplified by Chemical Formula 2 (NK-10714) in Japanese Unexamined Patent Application Publication No. 2020-146296 can be preferably used.

[0030] The thin film sheet in the artificial retina of the present invention is obtained by connecting fine fibers with an average fiber diameter of 2 to 1000 nm to form a porous structure. In the present invention, the porous structure refers to the space formed by the connection of fine fibers to each other. As a porous structure, there is no particular limitation as long as it can form holes through which the liquid that permeates from the surface of the thin film sheet passes to the back. As for the porosity of the above-mentioned porous structure, there is no particular limitation, but it is preferably 5 to 99.9%. As for the porosity, it is more preferably 10% or more, further preferably 20% or more, and particularly preferably 50% or more. On the other hand, the porosity is more preferably 99% or less. The porosity can be calculated using the method described in the embodiments described later.

[0031] As the fine fiber used in the present invention, there is no particular limitation, and it can be natural fibers such as cellulose, chitin, chitosan, etc., or it can be synthetic fibers such as polyolefin fibers such as polyethylene, polypropylene, polyester fibers such as polyethylene terephthalate, polybutylene terephthalate, polyamide fibers such as nylon, and polyvinyl alcohol fibers such as vinylon. Among them, cellulose nanofiber (CNF), which is a representative of natural fibers, has the advantages of improved biocompatibility to cells, etc., and excellent chemical and physical stability in the organism due to good flexibility. It is an important feature that the material used in the artificial retina of the present invention has biocompatibility, so as the above-mentioned fine fiber, it is preferably a compound with biocompatibility. Among them, biocompatibility refers to being able to use it without deteriorating cells, etc. From such a viewpoint, as the above-mentioned fine fiber, it is preferably composed of natural fibers, and more preferably composed of at least one selected from cellulose, chitin and chitosan.

[0032] The average fiber diameter of the microfibers is 2 to 1000 nm. When the average fiber diameter is less than 2 nm, the strength of the film sheet may be insufficient when the microfibers are connected to each other to form a porous structure. The average fiber diameter is preferably 3 nm or more, and more preferably 4 nm or more. On the other hand, when the average fiber diameter exceeds 1000 nm, it may be difficult to form a porous structure with liquid permeability. The average fiber diameter is preferably 800 nm or less, more preferably 600 nm or less, further preferably 500 nm or less, and particularly preferably 400 nm or less.

[0033] The artificial retina of the present invention is formed by fixing an organic pigment compound that induces a receptor potential corresponding to light stimulation. In the present invention, fixing the above-mentioned organic pigment compound means chemically fixing the above-mentioned organic pigment compound on the above-mentioned fine fibers in the above-mentioned film. A preferred embodiment is to fix the above-mentioned organic pigment compound on the above-mentioned fine fibers through a covalent bond. The above-mentioned covalent bond is not particularly limited and can be an amide bond, an ester bond, an ether bond, an urethane bond, etc., among which an amide bond is preferred. Since the artificial retina of the present invention has a porous structure formed by connecting the above-mentioned fine fibers, it is possible to make the fixed amount of the above-mentioned organic pigment compound more than the prior art, and it is expected to improve the effect of resolution when used as an artificial retina.

[0034] The artificial retina of the present invention preferably has a contact angle of 50 to 90° relative to the water on the surface of the artificial retina. By having the contact angle of water in such a range, there is an advantage of improving biocompatibility. As the contact angle of water, it is more preferably 60° or more, more preferably 70° or more, and particularly preferably 75° or more. On the other hand, the contact angle of water is more preferably 85° or less, and more preferably 80° or less.

[0035] The thickness of the artificial retina of the present invention is preferably 5 to 100 μm. When the thickness is less than 5 μm, the strength may decrease, and it is more preferably 10 μm or more. On the other hand, when the thickness exceeds 100 μm, it may be difficult to insert into the eyeball, and it is more preferably 80 μm or less, and further preferably 60 μm or less.

[0036] The method for manufacturing the artificial retina of the present invention is not particularly limited. The above-mentioned fine fibers having carboxyl groups are modified with diamines, and the above-mentioned organic pigment compound is reacted with the above-mentioned fine fibers after diamine modification, so that it is fixed on the above-mentioned fine fibers after diamine modification, and a thin film sheet is prepared in a manner that the above-mentioned fine fibers are connected to each other and form a porous structure. Such a method for manufacturing an artificial retina (hereinafter preferably referred to as the "first manufacturing method") is a preferred embodiment. In addition, after a thin film sheet is prepared in a manner that the above-mentioned fine fibers are connected to each other and form a porous structure, the above-mentioned fine fibers having carboxyl groups constituting the above-mentioned thin film sheet are modified with diamines, and the above-mentioned organic pigment compound is reacted with the above-mentioned fine fibers after diamine modification constituting the above-mentioned thin film sheet, so that it is fixed on the above-mentioned fine fibers after diamine modification constituting the above-mentioned thin film sheet. Such a method for manufacturing an artificial retina (hereinafter sometimes referred to as the "second manufacturing method") is also a preferred embodiment.

[0037] The first manufacturing method is described below. In the first manufacturing method, the above-mentioned fine fibers having carboxyl groups are preferably modified with diamines. As a result, the reaction between the above-mentioned fine fibers modified with diamines and the above-mentioned organic pigment compound can be easily performed. There is no particular limitation on the method for performing diamine modification. For example, for the above-mentioned fine fibers having carboxyl groups, a method of using ethylenediamine and DCC (N,N-dicyclohexylcarbodiimide) to react them is suitable. As a result, the carboxyl group and the amine are dehydrated and condensed to form an amide bond, and the obtained diamine-modified fine fibers have an amino group.

[0038] In addition, it is also a preferred embodiment to subject the above-mentioned fine fibers having carboxyl groups to an acid treatment before diamine modification. In the case where the carboxyl groups of the fine fibers are salts such as COONa type, the dehydration condensation reaction with amines may not proceed sufficiently, so it is a preferred embodiment to convert the carboxyl groups of the fine fibers into COOH type in advance by acid treatment. As the acid treatment, a method of immersing the above-mentioned fine fibers having carboxyl groups in an acid such as hydrochloric acid, sulfuric acid, nitric acid, etc. is suitable.

[0039] Next, the organic pigment compound is preferably reacted with the diamine-modified microfibers to fix them on the diamine-modified microfibers. There is no particular limitation on the method for reacting the organic pigment compound. For example, when the organic pigment compound has a carboxyl group, a method of using DCC to react in the same manner as the diamine-modified method is suitable. Thus, the organic pigment compound can be fixed on the diamine-modified microfibers by dehydration condensation of the amino group of the diamine-modified microfibers and the carboxyl group of the organic pigment compound.

[0040] The solvent used in the above reaction is not particularly limited, and examples thereof include: halogenated hydrocarbon solvents such as chlorobenzene, dichlorobenzene, trichlorobenzene, dichloroethane, trichloroethane, dichloromethane, chloroform, and carbon tetrachloride; saturated aliphatic hydrocarbon solvents such as pentane, hexane, heptane, octane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; ether solvents such as dimethyl ether, ethyl methyl ether, diethyl ether, tetrahydrofuran, and 1,4-dioxane; nitrile solvents such as acetonitrile, propionitrile, and benzonitrile; aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone, etc. Among them, it is preferred to use at least one organic solvent selected from the group consisting of halogenated hydrocarbon solvents, saturated aliphatic hydrocarbon solvents, and aromatic hydrocarbon solvents, and it is more preferred to use halogenated hydrocarbon solvents.

[0041] In addition, for the microfibers fixed with organic pigment compounds, the film is made in a mode that the above-mentioned microfibers are connected to each other and form a porous structure, thereby the artificial retina of the present invention can be obtained. As the method for making the above-mentioned film, it is not particularly limited, and it is suitable to adopt the method of drying after the dispersion liquid containing the above-mentioned microfibers is made into a sheet. As the method for making a sheet, it can be a method of pouring the dispersion liquid containing the above-mentioned microfibers into a container and making a sheet, or it can be a method of applying the dispersion liquid containing the above-mentioned microfibers on a substrate and making a sheet. After being made into a sheet, dry it, remove the dispersion medium, and thus make the film. As the method for drying, it is not particularly limited, and natural drying, heat drying, freeze drying, etc. can be appropriately adopted. As a dispersion medium, it is suitable to use water, and it is also possible to contain an organic solvent to the extent that the organic pigment compound after fixing is not dissolved. As an organic solvent, a solvent identical with the solvent used in the above-mentioned reaction can be used.

[0042] In the dispersion containing the above-mentioned fine fibers, the concentration of the fine fibers is not particularly limited, but is preferably 0.01 to 5% by weight. When the concentration of the fine fibers is less than 0.01% by weight, it may not be possible to form a film, and it is more preferably 0.05% by weight or more, and more preferably 0.1% by weight or more. On the other hand, when the concentration of the fine fibers exceeds 5% by weight, density non-uniformity may occur, and liquid permeability may be insufficient, and it is more preferably 3% by weight or less, more preferably 1% by weight or less, and particularly preferably 0.8% by weight or less.

[0043] The dispersion containing the microfibers may contain an adhesive polymer from the viewpoint that the microfibers are easily connected to each other. Examples of the adhesive polymer include polyvinyl alcohol, polyvinyl acetate, polyethylene glycol, polyacrylamide, starch, carboxymethyl cellulose, etc., preferably a biocompatible compound. The concentration of the adhesive polymer in the dispersion containing the microfibers is not particularly limited, but is preferably 0.01 to 2% by weight, more preferably 0.05 to 1% by weight, and further preferably 0.1 to 0.8% by weight.

[0044] The second manufacturing method is described below. In the second manufacturing method, it is also preferred to perform diamine modification on the fine fibers having carboxyl groups in the same manner as in the first manufacturing method, but it is preferred to perform diamine modification after preparing a thin film sheet in a manner that the fine fibers are connected to each other and form a porous structure. Thus, the fine fibers of the thin film sheet have amino groups. As a method for preparing the thin film sheet and a method for performing the diamine modification, the same method as in the first manufacturing method is preferably used.

[0045] In addition, from the viewpoint of smoothly carrying out the dehydration condensation reaction of diamine modification, it is also a preferred embodiment to subject the film sheet to an acid treatment before carrying out the diamine modification. As the acid treatment method, the same method as the first production method can be suitably adopted.

[0046] Next, the organic pigment compound is reacted with the diamine-modified microfibers to be fixed on the diamine-modified microfibers, thereby obtaining the artificial retina of the present invention. As a method for reacting the organic pigment compound, the same method as the first manufacturing method is preferably used.

[0047] Artificial retina of the present invention is formed by fixing the organic pigment compound that induces the receptor potential corresponding to light stimulation. As shown in Japanese Patent No. 5090431, Matsuo, one of the inventors of the present invention, etc. confirmed that, using the organic pigment compound that induces the receptor potential corresponding to light stimulation, in the optic nerve, particularly the retinal nerve cells that constitute the optic nerve, as a significant receptor potential is observed as intracellular potential. Therefore, it can be known that the film formed by fixing the organic pigment compound that induces the receptor potential corresponding to light stimulation is useful as artificial retina. Especially the artificial retina of the present invention is characterized in that: because of the porous structure formed by the connection of the above-mentioned fine fibers, it has liquid permeability, and compared with the existing artificial retina that does not have liquid permeability, body fluid or blood can be passed through, and biocompatibility is improved. Thus, when the artificial retina of the present invention is made to fit with retinal tissue, the deterioration of the retinal tissue can be suppressed. Therefore, it is a preferred embodiment to use it in close contact with retinal tissue, no matter in clinical trials, or in non-clinical trials, it can be used as a very useful artificial retina.

[0048] Example

[0049] The present invention will be described in more detail below using examples. In the examples, the organic dye compound used was a polymethine-based organic dye compound represented by the following formula, which was reported and produced by Hayashibara Co., Ltd. as "NK-5962".

[0050]

[0051] Example 1

[0052] [Production of TOCN porous body]

[0053] Distilled water was added to RHEOCRYSTA (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., solid content 2.0 wt%, average fiber diameter 4 nm), which is a cellulose nanofiber having a carboxyl group (TOCN: TEMPO oxidized CNF), so that the TOCN concentration becomes 1.0 wt%, and ultrasonic irradiation was performed for 1 hour using a desktop ultrasonic cleaner (manufactured by BRANSON, 2510J-MT) to prepare a TOCN aqueous dispersion. After degassing for 30 minutes using a rotation / revolution mixer (manufactured by THINKY, AR-100), the dispersion was transferred to a stainless steel culture dish and allowed to stand in a freezer overnight. Freeze drying was performed using a freeze dryer (manufactured by EYELA, FDU-1200) to prepare a TOCN porous body. A photograph of the obtained TOCN porous body is shown in Figure 1 The porosity calculated by the following formula was 99%, which was confirmed to have a high specific surface area.

[0054]

[0055] [Diamine modification]

[0056] 0.1 g of TOCN porous body disassembled into about 5 mm pieces with tweezers and 2.6 μL of ethylenediamine (4.0×10 -5 mol), 75 mL of chlorobenzene as solvent, 8.25 × 10 -3 g(4.0×10 -5 mol). The mixture was placed in a 35°C constant temperature oscillating water tank (NTS-4000AM manufactured by EYELA) and stirred at 50 rpm for 48 hours. The TOCN porous body to which ethylenediamine was bonded (hereinafter referred to as "diamine-modified porous body") was taken out and washed by filtration using chlorobenzene. The diamine-modified porous body was not dried, and the dye was fixed as the next step.

[0057] [Pigment fixation]

[0058] 2.0 × 10 photoelectric conversion dye (NK-5962 manufactured by Hayashibara Co., Ltd.) was added to a 200 mL stoppered Erlenmeyer flask. -2 g(4.0×10 -5 mol), 75 mL of chlorobenzene as solvent, 8.25 × 10 -3 g(4.0×10 -5 mol). Ultrasonic irradiation was performed for 30 minutes using a tabletop ultrasonic cleaner to disperse the pigment. Next, a diamine-modified porous body was added and stirred at 50 rpm in a constant temperature oscillating water tank at 35°C for 48 hours. The TOCN porous body combined with the photoelectric conversion pigment (hereinafter referred to as the "pigment-fixed porous body") was taken out, filtered, washed with chlorobenzene, and dried naturally.

[0059] [Preparation of Pigment-Fixed Film Sheet]

[0060] Measure 0.1 g of PVA powder (manufactured by Sigma-Aldrich, with a saponification degree of 99% or more and an average molecular weight of 89,000 to 98,000) into a 100 mL eggplant-shaped flask, add distilled water to make the PVA concentration 0.5 wt%, and completely dissolve it in a 95°C oil bath under reflux, then cool it to room temperature to prepare a PVA aqueous solution. Add 0.1 g of the pigment-fixed porous body and a PVA aqueous solution (concentration 0.5 wt%) to a 100 mL beaker, and add distilled water to make the total 50 mL. Use a desktop ultrasonic cleaner to perform ultrasonic irradiation for 1 hour to prepare an aqueous dispersion with a weight ratio of TOCN:PVA=1:1. Transfer the dispersion to a PFA culture dish, dry it at 40°C, wash it with methanol and dry it naturally to prepare a pigment-fixed film sheet. The thickness of the obtained pigment-fixed film sheet is about 30 μm. A photograph of the obtained pigment-fixed film sheet is shown in Figure 2 .

[0061] [Elemental analysis using energy dispersive X-ray analysis (EDX)]

[0062] In order to confirm that the pigment is chemically fixed in the pigment-fixed film sheet produced, a scanning electron microscope (manufactured by Japan Electronics Co., Ltd., JSM-IT100) with an energy dispersive X-ray spectrometer (EDX) device was used to perform elemental analysis of the pigment-fixed film sheet. The accelerating voltage was 5 keV and the irradiation current was 60 probe current (PC). In addition, before SEM observation, an ion plating machine (manufactured by EICOH, IB-3) was used to perform Au vapor deposition on the sample surface. The EDX spectrum is shown in Figure 3 On the surface of the dye-fixed film sheet, a large peak of Na derived from COONa-type carboxyl groups, a peak derived from Br of the dye, and a small peak derived from N of the dye and amide bond were observed. Therefore, it was confirmed that the dye was chemically fixed in the dye-fixed film sheet.

[0063] [Evaluation of liquid permeability]

[0064] In order to evaluate whether there is liquid permeability, the pigment-fixed film sheet is clamped with filter paper, and phosphate buffered saline (PBS, pH 7.2) is dripped from one side to measure the weight of the filter paper on the opposite side. As a result, the weight of the filter paper before dripping is 0.0140g, and the weight of the filter paper after dripping is 0.0252g. Since the weight of the filter paper on the opposite side has increased, it can be confirmed that the liquid is penetrated. Therefore, it can be known that the pigment-fixed film sheet has liquid permeability.

[0065] [Photoinduced surface potential measurement]

[0066] In order to confirm that the produced pigment-fixed film sheet generates a potential when exposed to light, a scanning Kelvin probe (SKP5050 manufactured by KPTechnology) was used to perform light-induced surface potential measurement. The device was set in an atmospheric pressure replacement dryer. The light intensity was controlled using a surface photovoltage spectroscopy (SPS) module (SPS040 manufactured by KPTechnology) to perform the measurement in the SPV (Surface Photo Voltage) mode by changing the intensity of the irradiated light. Within the range of light intensity of 0-5000 arbitrary units (arb.Units), the light was irradiated in increments of 100 arb.Units each time, and the change in surface potential was measured. The obtained measurement results are shown in Figure 4 .

[0067] Example 2

[0068] [Preparation of TOCN-COOH thin film]

[0069] Distilled water was added to RHEOCRYSTA (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., solid content 2.0 wt%, average fiber diameter 4 nm), which is a cellulose nanofiber with a carboxyl group (TOCN: TEMPO oxidized CNF), to make a TOCN concentration of 0.2 wt%, and irradiated with a homogenizer for 1 hour. Next, ultrasonic irradiation was performed for 1 hour using a desktop ultrasonic cleaner to prepare a TOCN aqueous dispersion. The TOCN dispersion was transferred to a PFA culture dish and dried at 50°C to prepare a TOCN film sheet. The TOCN film sheet was cut into 1.5 cm × 1.5 cm pieces, and in order to convert the carboxyl group from COONa type to COOH type, the TOCN film sheet was allowed to stand in 0.01 M hydrochloric acid for 30 minutes. It was washed with distilled water until neutral, and dried naturally to prepare a TOCN-COOH film sheet. In order to confirm that the carboxyl groups of the prepared TOCN-COOH thin film were converted into COOH type, infrared spectroscopy (IR) measurement of the TOCN thin film and the TOCN-COOH thin film was performed using a Fourier transform infrared spectrophotometer (IRAffinity-1S manufactured by SHIMADZU). The obtained IR spectrum is shown in Figure 5 .

[0070] [Diamine modification]

[0071] TOCN-COOH film and 2.6 μL (4.0 × 10 -5mol), 75 mL of chlorobenzene as solvent, 8.25 × 10 -3 g(4.0×10 - 5 mol). It was placed in a 35°C constant temperature oscillating water tank (NTS-4000AM manufactured by EYELA) and stirred at 50 rpm for 48 hours. The film sheet bonded with ethylenediamine (hereinafter referred to as "diamine-modified TOCN-COOH film sheet") was taken out and washed with chlorobenzene. The diamine-modified TOCN-COOH film sheet was not dried, but was fixed as the pigment in the next step.

[0072] [Pigment fixation]

[0073] 2.0 × 10 photoelectric conversion dye (NK-5962 manufactured by Hayashibara Co., Ltd.) was added to a 200 mL stoppered Erlenmeyer flask. -2 g(4.0×10 -5 mol), 75 mL of chlorobenzene as solvent, 8.25 × 10 -3 g(4.0×10 -5 mol). Use a desktop ultrasonic cleaner to irradiate with ultrasound for 30 minutes to disperse the pigment. Next, add a diamine-modified TOCN-COOH film and react it in a constant temperature oscillating water tank at 35°C for 48 hours while stirring at 50 rpm. Take out the film sheet to which the photoelectric conversion pigment is bonded (hereinafter referred to as the "pigment-fixed TOCN-COOH film sheet"), wash it with chlorobenzene, and then dry it naturally. Wash with chlorobenzene and check the color of chlorobenzene every hour. In the case of chlorobenzene coloring, wash it again for 1 hour. In the case of no coloring, wash it and dry it naturally. The thickness of the obtained pigment-fixed TOCN-COOH film sheet is about 30μm. A photograph of the obtained pigment-fixed TOCN-COOH film sheet is shown in Figure 6 .

[0074] [Elemental analysis using energy dispersive X-ray analysis (EDX)]

[0075] The elemental analysis of the dye-fixed TOCN-COOH film was performed in the same manner as in Example 1. The EDX spectrum is shown in Figure 7. On the surface of the pigment-fixed TOCN-COOH film, no peak of Na from the COONa-type carboxyl group was observed, but the peak of Br from the pigment and the peak of N from the pigment and amide bond were observed to be larger. Therefore, it can be confirmed that the pigment is chemically fixed in the pigment-fixed TOCN-COOH film. In addition, compared with the elemental analysis results of the pigment-fixed film of Example 1, larger peaks of Br and N were observed, which is considered to be due to the chemical fixation of more pigments.

[0076] [Evaluation of liquid permeability]

[0077] The evaluation of liquid permeability was performed using the same method as in Example 1. As a result, the weight of the filter paper before the dropwise addition was 0.0135 g, and the weight of the filter paper after the dropwise addition was 0.0288 g. Since the weight of the filter paper on the opposite side increased, it was possible to confirm that the liquid was penetrated. Therefore, it can be seen that the pigment-fixed TOCN-COOH film sheet has liquid permeability. After the pigment-fixed TOCN-COOH film sheet contains physiological saline, it is not dispersed and maintained in a film shape, and can be used even in vivo without being damaged.

[0078] [Photoinduced surface potential measurement]

[0079] The light-induced surface potential of the dye-fixed TOCN-COOH thin film was measured in the same manner as in Example 1. The obtained measurement results are shown in Figure 8 .

[0080] [UV-visible absorbance measurement]

[0081] The absorbance of the dye-immobilized TOCN-COOH thin film sheet prepared in Example 2 was measured using an ultraviolet-visible spectrophotometer (V-750 manufactured by JASCO Corporation) equipped with an integrating sphere unit (PIV-75 manufactured by JASCO Corporation). The obtained ultraviolet-visible absorbance measurement results are shown in Fig. 9 The absorbance at the peak top of the dye-fixed TOCN-COOH film was 1.104. On the other hand, the absorbance of the film in which the dye was fixed on the polyethylene film measured for comparison was about 0.1, indicating that the amount of dye fixed was increased.

Claims

1. An artificial retina, characterized in that: The artificial retina is made by fixing organic pigment compounds on a thin film. The organic pigment compound induces a receptor potential corresponding to light stimulation, The film sheet is obtained by connecting fine fibers with an average fiber diameter of 2 to 1000 nm to form a porous structure. The porous structure provides liquid permeability.

2. The artificial retina according to claim 1, characterized in that: The organic pigment compound is fixed to the fine fibers in the film sheet through covalent bonds.

3. The artificial retina according to claim 1 or 2, characterized in that: The microfibers are biocompatible.

4. A method for manufacturing an artificial retina, which is used to manufacture the artificial retina according to any one of claims 1 to 3, wherein the method is characterized in that: The microfibers having carboxyl groups are modified with diamine, After reacting the organic pigment compound with the diamine-modified microfibers to fix the organic pigment compound on the diamine-modified microfibers, The film sheet is manufactured in such a manner that the fine fibers are connected to each other and form a porous structure.

5. A method for manufacturing an artificial retina, which is used to manufacture the artificial retina according to any one of claims 1 to 3, wherein the method is characterized in that: After manufacturing a thin film sheet in such a manner that the microfibers are connected to each other and form a porous structure, The fine fibers having carboxyl groups constituting the film sheet are modified with diamine, The organic pigment compound is reacted with the diamine-modified fine fibers constituting the film sheet, thereby being fixed to the diamine-modified fine fibers constituting the film sheet.

Citation Information

Patent Citations

  • Receptor potential inducer

    JP2004121292A

  • Artificial retina and method for producing the same

    JP2020146296A

  • Method for producing artificial retina

    WO2015152233A1