Alumina-based thermally conductive disc-shaped particles, method for producing same, thermally conductive composition, article, liquid composition, thermally conductive film, and member for electronic device
Alumina-based disc-shaped particles are prepared by mixing aluminum raw materials and glass powder, which solves the problems of difficulty in mixing alumina in the resin and poor filling properties, and realizes a resin composition with excellent thermal conductivity and resistance, which is suitable for electronic components etc.
Patent Information
- Application Number
- CN202380036042.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-03-03
- Publication Date
- 2024-12-03
AI Technical Summary
The high Mohs hardness of alumina makes it difficult to mix in resin, and the plate-shaped alumina has poor filling properties, making it difficult to meet the application needs of thermally conductive materials. The existing manufacturing methods have equipment restrictions and health for diluent use and hydrothermal methods. Problems such as hazardous substance residues.
By mixing aluminum raw materials with glass powder, alumina-based thermally conductive disc-shaped particles were prepared, and their aspect ratio and surface state were adjusted. A disc-shaped shape with no sharp angles was adopted to improve the mixing and thermal conductivity in the resin and the like. , combining specific oxide feedstocks to improve dispersion and thermal conductivity.
Alumina-based thermal conductivity disc-shaped particles with excellent thermal conductivity, chemical resistance, water resistance and electrical insulation are achieved, which improves the filling and moldability in the resin, and is suitable for applications such as electronic components.
Smart Images

Figure CN119072460A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to alumina-based thermally conductive disc-shaped particles having excellent filling properties and a method for producing the same. Background Art
[0002] Currently, various raw materials are being studied as thermally conductive materials. With the improvement of the integration of semiconductor elements, the demand for heat dissipation is increasing, and it is necessary to develop materials with higher thermal conductivity and insulation than the existing ones. As a material that meets this requirement, a composite material (resin composition) obtained by mixing a thermally conductive filler into a resin is known.
[0003] As a filler for composite materials, alumina has excellent water resistance, acid resistance and insulation, good thermal conductivity, and is inexpensive, so it is used in many cases. It is also known that alumina also has various shapes of alumina, including spherical, circular, amorphous and plate-like. Among them, plate-like alumina has many uses such as thermal conductive fillers, bright pigments, abrasives, sliding materials, lubricants and barrier materials. When it is used as a thermal conductive filler, it is strongly required that the alumina has excellent mixing properties (filling properties) in the resin and high thermal conductivity.
[0004] As a method for preparing plate-like alumina, many methods have been known. As a related prior art, there is a method of adding a metal fluoride such as cryolite as a mineralizer to a large amount of diluent materials such as sodium chloride and potassium sulfate, and heat-treating the aluminum raw material (Patent Document 1). In addition, there is a method of making a mixed solution of an aqueous solution of aluminum sulfate and an aqueous solution of sodium hydroxide undergo a hydrothermal reaction in an autoclave (Patent Document 2). In addition, there is a method of advocating that by adding an aluminum raw material, a shape-controlling material, and molybdenum oxide during roasting, the Zeta potential can be made into highly dispersible plate-like particles and a method for making the same (Patent Document 3). Furthermore, there is a method for making alumina-based thermally conductive particles using an aluminum raw material, and powder (frit) and / or a metal oxide (Patent Document 4).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2006-515557
[0008] Patent Document 2: Japanese Patent Application Publication No. 2008-195569
[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-123664
[0010] Patent Document 4: Japanese Patent Application Publication No. 2018-145025 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] Alumina has a high Mohs hardness and applies a load to blades and extruder shafts, so it is difficult to mix it into resin compositions, etc., and it may mix into worn parts, causing contamination. In addition, plate-shaped alumina is expected to be used in a variety of applications such as bright materials, lubricants, and sliding materials due to its shape, but from the perspective of application in thermal conductive materials, there is a tendency that its filling property in resin is inferior to that of other aluminas due to its shape.
[0013] In the method using diluent and mineralizer in Patent Document 1 and the synthesis based on hydrothermal method in Patent Document 2, particles with small particle size and high aspect ratio are generated. However, in Patent Document 1, the raw aluminum hydroxide must be crushed in advance. In addition, after heat treatment, a large amount of diluent material needs to be washed to remove. The diluent material is also a component that easily corrodes the steel plate, so there is a problem of increasing the load on the manufacturing equipment. In addition, the hydrothermal method in Patent Document 2 requires special manufacturing equipment and is a reaction under high temperature and high pressure. Therefore, there is a limitation in the size of the device, and there is also a restriction that the amount that can be manufactured at one time is small.
[0014] In the method of adding aluminum raw material, shape control material, and molybdenum oxide during roasting proposed in Patent Document 3, although the amount of molybdenum added is several tens of% relative to the aluminum raw material and gasification and diffusion occur during roasting, the residual molybdenum content is reduced to a certain extent by cleaning the surface of the particles. However, in this patent, it is pointed out that molybdenum, which is harmful to health, exists in the particles, so it is necessary to pay attention to the handling of products containing the particles. In addition, the aluminum raw material is not specifically mentioned, and there is no record of what kind of influence is caused by the difference in the aluminum raw material used. Furthermore, in this patent, although it is claimed that the dispersion can be high by measuring the Zeta potential, there is actually no example of application in polymer materials, etc. In addition, there is no experimental data on thermal conductivity. Therefore, it is not clear how much can be added to the polymer composition and how the thermal conductivity changes when added.
[0015] In the alumina-based thermally conductive particles using glass powder and / or metal oxide proposed in Patent Document 4, although the materials used are similar, the particle size is considered to be spherical in the patent. However, although there is a description that it can be controlled to other shapes in the patent, particles other than spherical are not actually produced, and no detailed method for changing the shape is described. Furthermore, the filling amount and filling properties of the resin composition and the like are not shown.
[0016] The present invention is completed in view of the problems existing in the prior art, and its subject is to provide: alumina-based thermally conductive disc-shaped particles that are not only excellent in thermal conductivity, but also excellent in chemical resistance, water resistance and electrical insulation, and have good mixing (filling) properties in resins, and can produce materials and articles such as resin compositions with excellent moldability, and a method for producing the same. In the present invention, it is found that by using glass powder and oxide raw materials according to the situation, the crystallinity is excellent, and the aspect ratio and the surface state of the particles can be adjusted. In particular, it is easy to obtain a disc-shaped particle with a thickness compared to the existing plate-shaped alumina, and it is a method that can easily obtain a disc-shaped particle with a not too large aspect ratio because it is a disc-shaped particle. In addition, it is also characterized in that, as the properties of the particles, by adopting a particle shape without sharp corners and with a rounded shape as a whole, the mixing (filling) properties in the resin are improved. The subject of the present invention is to provide: a thermally conductive composition and an article using the above-mentioned alumina-based thermally conductive disc-shaped particles.
[0017] Solutions for solving problems
[0018] That is, according to the present invention, there are provided the following alumina-based thermally conductive disc-shaped particles and a method for producing the same.
[0019] [1] Alumina-based thermally conductive disc-shaped particles, which are particles of alumina-based thermally conductive oxide obtained by calcining a raw material mixture containing an aluminum raw material and glass powder (excluding a mixture containing a boric acid compound),
[0020] The aluminum raw material is at least one selected from the group consisting of boehmite and aluminum hydroxide,
[0021] The deformation point of the glass powder is 300°C or higher and 800°C or lower.
[0022] The content of the glass powder in the raw material mixture is 0.5 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the aluminum raw material.
[0023] The primary particles of the alumina-based thermally conductive oxide have an average particle size of 1 μm to 50 μm, an average thickness of 0.1 μm to 5 μm, an aspect ratio of more than 1 to 50, and a disc shape.
[0024] [2] The alumina-based thermally conductive disc-shaped particles according to [1], wherein the raw material mixture further contains an oxide raw material other than the glass powder, and the oxide raw material comprises at least one selected from the group consisting of titanium compounds, phosphorus compounds, tungsten compounds and bismuth compounds.
[0025] [3] The alumina-based thermally conductive disc-shaped particles according to [1] or [2], wherein the alumina-based thermally conductive oxide contains at least one element selected from the group consisting of iron, cobalt, copper, manganese, and nickel, and is colored.
[0026] [4] The alumina-based thermally conductive disc-shaped particles according to any one of [1] to [3], wherein the glass powder does not contain lead.
[0027] [5] A method for producing alumina-based thermally conductive disc-shaped particles, which is the method for producing alumina-based thermally conductive disc-shaped particles according to any one of [1] to [4], the method comprising the following steps:
[0028] A step of mixing at least one aluminum raw material selected from the group consisting of boehmite and aluminum hydroxide with glass powder to obtain a raw material mixture; and,
[0029] The obtained raw material mixture is calcined.
[0030] The content of the glass powder in the raw material mixture is 0.5 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the aluminum raw material.
[0031] In the step of calcining the raw material mixture, the raw material mixture is calcined in air at 1000° C. or higher and 1400° C. or lower.
[0032] Furthermore, according to the present invention, there are provided the thermally conductive composition and article shown below.
[0033] [6] A thermally conductive composition comprising: a thermally conductive filler and the alumina-based thermally conductive disc-shaped particles according to any one of [1] to [4].
[0034] [7] An article comprising the alumina-based thermally conductive disk-shaped particles according to any one of [1] to [4].
[0035] [8] The article according to [7], further comprising a thermally conductive filler.
[0036] [9] The article according to [7] or [8], wherein the article is any one of a gravure ink, a coating liquid, a resin composition, and an adhesive composition.
[0037] Furthermore, according to the present invention, there are provided the following liquid composition, thermally conductive film, and electronic device member.
[0038]
[10] A liquid composition for forming a thermally conductive thin film,
[0039] The liquid composition contains:
[0040] A film-forming resin, a liquid medium, and a thermally conductive component comprising the alumina-based thermally conductive disc-shaped particles according to any one of [1] to [4].
[0041]
[11] The liquid composition according to
[10] , wherein the thermally conductive component further contains a thermally conductive filler.
[0042] The thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc and boron nitride.
[0043]
[12] The liquid composition according to
[10] or
[11] , wherein the content of the thermally conductive component is 50 parts by mass or more and 600 parts by mass or less relative to 100 parts by mass of the film-forming resin.
[0044]
[13] The liquid composition according to any one of
[10] to
[12] , wherein the film-forming resin is at least one solvent-soluble resin selected from the group consisting of acrylic resins, urethane resins, urea resins, epoxy resins, rubber resins, fluorine resins, polyamide resins, polyimide resins, silicone resins, cellulose resins and thermoplastic elastomers.
[0045]
[14] A thermally conductive film formed by coating the liquid composition according to any one of
[10] to
[13] .
[0046]
[15] An electronic device component comprising: a metal component; and the thermally conductive film according to
[14] disposed on a surface of the metal component.
[0047] According to the present invention, it is possible to provide alumina-based thermally conductive disc-shaped particles which have excellent thermal conductivity, chemical resistance, water resistance, and electrical insulation, and which have good mixing properties (filling properties) in resins and can produce materials and articles such as resin compositions with excellent moldability, and a method for producing the same. In addition, it is possible to provide a thermally conductive composition and an article using the alumina-based thermally conductive disc-shaped particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is an electron microscope photograph showing the alumina-based thermally conductive disc-shaped particles obtained in Example 2.
[0049] Figure 2 This is an electron microscope photograph showing the alumina-based thermally conductive disc-shaped particles obtained in Example 19.
[0050] Figure 3 This is an electron microscope photograph showing the alumina-based thermally conductive disc-shaped particles obtained in Example 26.
[0051] Figure 4 This is an electron microscope photograph showing the alumina-based thermally conductive particles obtained in Comparative Example 2. DETAILED DESCRIPTION
[0052] <Alumina-based thermally conductive disc-shaped particles>
[0053] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. The alumina-based thermally conductive disc-shaped particles (hereinafter, sometimes also referred to as "disc-shaped particles") in the present embodiment are obtained by roasting a raw material mixture containing an aluminum raw material. In addition, the aluminum raw material is at least one selected from the group consisting of boehmite and aluminum hydroxide. The raw material mixture also contains glass powder, and according to circumstances, contains at least one oxide raw material other than glass powder selected from the group consisting of boron compounds, titanium compounds, phosphorus compounds, tungsten compounds and bismuth compounds. Moreover, the content of the glass powder in the raw material mixture is greater than 0.5 parts by mass and less than 5 parts by mass relative to 100 parts by mass of the aluminum raw material. Hereinafter, the details of the disc-shaped particles of the present embodiment will be described.
[0054] Resins usually have low thermal conductivity. Therefore, in order to improve the thermal conductivity of resin articles, a method of adding a large amount of thermally conductive fillers such as aluminum oxide to the resin is usually adopted. By mixing a thermally conductive filler into the resin, the thermally conductive filler is dispersed in the resin in a manner that the thermally conductive fillers have contact points with each other, so that the thermal conductivity unique to the thermally conductive filler can be exerted. Among them, in order to exert higher thermal conductivity, aluminum oxide with a larger particle size or spherical aluminum oxide is used, and it is designed to be easy to disperse a large amount of aluminum oxide into the resin. However, when aluminum oxide designed in this way is mixed into the resin, there are many cases where the contact points between aluminum oxides decrease and the thermal conductivity is not improved. On the other hand, when aluminum oxide with a smaller particle size is added to the resin, the mixing property (filling property) in the resin is reduced, and it is difficult to disperse a large amount of aluminum oxide in the resin, and it is difficult to improve the thermal conductivity.
[0055] On the other hand, plate-like alumina has shape anisotropy, so the chances of surface contact increase, which can improve the thermal conductivity in the surface direction. However, due to its plate shape, it is often less filling in resin than spherical or crushed alumina, and currently there are many restrictions on compounding for achieving high thermal conductivity.
[0056] The disc-shaped particles of the present embodiment are obtained by roasting a raw material mixture containing aluminum raw materials such as aluminum hydroxide, glass powder, and oxide raw materials other than glass powder according to circumstances in a specified ratio. Glass powder is also referred to as frit or multi-component glass, and is therefore mainly used for coating in the ceramic industry, but the inventors have found that it is suitable for bringing shape anisotropy to aluminum oxide. The glass powder is preferably melted below the roasting temperature. It is speculated that the crystal orientation of aluminum oxide is limited when the aluminum oxide crystal grows by melting, thereby obtaining the disc-shaped particles of the present embodiment. In addition, the glass powder also functions as a mineralizer while melting, and has the advantage of obtaining α-alumina at a lower temperature than usual. By adding a small amount, it is easy to obtain disc-shaped α-alumina, which synergizes with the effect of being a mineralizer and has the effect of making the surface smooth, so that disc-shaped particles with high wettability to resin can be obtained, thereby improving thermal conductivity and manufacturing materials and articles such as resin compositions with excellent moldability. Furthermore, by combining with other thermally conductive fillers having shapes other than disk shapes, such as spherical or polygonal shapes, more contact points between the fillers can be formed, which is one of the preferred uses.
[0057] Glass powder is composed of several metals uniformly fused together. Even if the oxides of the metals constituting the glass powder are added separately as respective metal oxides, the melting points of the respective metal oxides are different, and the effect of the present embodiment will not be achieved. The inventors of the present invention have confirmed the necessity of using a substance that is a multi-component glass called glass powder.
[0058] Among them, since it is a glass component, when added in excess, the molten glass powder will cause the particles to fuse together, forming large particles or aggregates, which will become particles with poor dispersibility. Therefore, the inventors of the present invention have limited the amount of glass powder used to a certain specific range.
[0059] In addition to the glass powder, oxide raw materials other than the glass powder can also be mixed. These components are used to assist the glass powder component. Oxide raw materials are added to solve the problems of easy aggregation, difficult alpha formation, and the need to adjust the aspect ratio.
[0060] The primary particles of the disc-shaped particles of the present embodiment must satisfy the following conditions.
[0061] The average particle size must be 1 μm or more and 50 μm or less. When the average particle size is less than 1 μm, the mixing property (filling property) in the resin will be reduced. On the other hand, if the average particle size exceeds 50 μm, the improvement effect of thermal conductivity will be insufficient. From this point of view, the average particle size is preferably 1.1 μm or more and 30 μm or less, and more preferably 1.2 μm or more and 20 μm or less.
[0062] The average thickness must be 0.1 μm or more and 5 μm or less. If the average thickness is less than 0.1 μm, the mixing property in the resin will be reduced. On the other hand, if the average thickness exceeds 5 μm, it becomes difficult to obtain particles with a high aspect ratio. From this point of view, the average thickness is preferably 0.2 μm or more and 3 μm or less, and more preferably 0.3 μm or more and 1.5 μm or less.
[0063] The aspect ratio must be greater than 1 and less than 50. The aspect ratio is calculated by dividing the value of the average particle size by the value of the average thickness (average particle size / average thickness). When the aspect ratio is 1, there is no shape anisotropy, and therefore, in particular, the effect of thermal conductivity in a shape such as a film cannot be fully exerted. On the other hand, when the aspect ratio exceeds 50, the filling property into the resin deteriorates, and it becomes difficult to use the thermal conductive material under high filling required. From this point of view, the aspect ratio is preferably greater than 2 and less than 45, more preferably greater than 3 and less than 40, and particularly preferably greater than 3.5 and less than 36.
[0064] The particle shape must be disc-shaped. The particle shape can be confirmed by observation under an electron microscope.
[0065] In this specification, average particle size can be measured using a laser diffraction particle size distribution measuring device. Specifically, it can be measured by the method described in the embodiments described later. In addition, average particle size can also be measured by the observation result under an electron microscope. In this method, the measured value becomes the same value as the measured value based on the laser diffraction particle size distribution measuring device.
[0066] The average thickness can also be measured from the average particle size by observation under an electron microscope. Specifically, it can be measured by the method described in the Examples described below.
[0067] About the mixing property (filling property) of the disc-shaped particles in the resin of the present embodiment, it is good for various resins, but in the present embodiment, as an example, it is judged by evaluating the filling amount of the epoxy resin commonly used in electronic components. As an evaluation method, relative to 100 mass parts of epoxy resin, it is preferably possible to fill more than 250 mass parts, and more preferably more than 300 mass parts. If it is less than 250 mass parts, the affinity to the resin is low, and it becomes poorly dispersed, and the amount of thermally conductive particles relative to the resin is small, therefore, it is impossible to exert sufficient thermal conductivity. In addition, the filling amount is preferably less than 1000 mass parts. This is because, if it exceeds 1000 mass parts, the disc-shaped particles are too many, and the moldability, processability, and strength of the resin will be poor.
[0068] Regarding the thermal conductivity of the disc-shaped particles of this embodiment, the value when 70 parts by mass are added relative to 30 parts by mass of epoxy resin is used as an index. At this time, the thermal conductivity of the epoxy resin composition is preferably 0.9 W / m·K or more. Thus, when used in electronic components, the thermal conductivity becomes high and the target heat dissipation performance can be achieved.
[0069] The disc-shaped particles of this embodiment have excellent thermal conductivity, chemical resistance, water resistance and electrical insulation. In addition, they have high wettability to resins and good mixing (filling) properties in resins, so that materials such as resin compositions, coatings, adhesive compositions and other articles with excellent formability can be manufactured.
[0070] (Aluminum raw materials)
[0071] The disc-shaped particles of this embodiment are obtained by calcining a raw material mixture containing an aluminum raw material, glass powder, and, if necessary, an oxide raw material other than the glass powder, and preferably contain α-alumina as a main component. The aluminum raw material is at least one selected from the group consisting of aluminum hydroxide and boehmite.
[0072] As the aluminum raw material, boehmite and aluminum hydroxide can be used. The shape and particle size of the aluminum raw material are not particularly limited. If the dispersibility of the disc-shaped particles is considered, particles with an average particle size of 1 μm or more and 50 μm or less are preferably used. As more specific shapes of the aluminum raw material, spherical and amorphous shapes can be cited. When aluminum oxide is used as the aluminum raw material, it is difficult to produce the so-called disc-shaped particles in this embodiment, and it is not suitable for use.
[0073] (Raw material mixture)
[0074] The raw material mixture used together with the aluminum raw material may further contain an oxide raw material other than the glass powder in addition to the glass powder. The oxide raw material is at least one selected from the group consisting of a boron compound, a titanium compound, a phosphorus compound, a tungsten compound, and a bismuth compound. These have the effects of improving the dispersibility of the disc-shaped particles, promoting the alpha formation of aluminum oxide, or adjusting the aspect ratio.
[0075] (Glass powder)
[0076] Glass powder is composed of a variety of elements. As an amorphous (non-crystalline) material, there is no melting point, but instead there is a softening point and a sag temperature. In this embodiment, the focus is on the sag temperature. The sag temperature of the glass powder must be above 300°C and below 800°C. If the sag temperature is below 300°C, the proportion of particle fusion increases, resulting in particles with poor dispersibility. If the sag temperature is above 800°C, it becomes difficult to form the disc-shaped particles of this embodiment, which is not preferred. From this point of view, the sag temperature of the glass powder is preferably above 350°C and below 600°C, and more preferably above 380°C and below 550°C. As a glass powder, it is preferred to contain silicon and boron, and also contain at least one element selected from the group consisting of lithium, sodium, potassium, magnesium, calcium, aluminum, zinc, fluorine, titanium and phosphorus. By using glass powder of such a composition, disc-shaped particles are generated, the wettability to the resin is improved, and the mixing property (filling property) in the resin can be further improved. Furthermore, from the viewpoint of environmental protection, it is preferred that the glass frit does not contain lead.
[0077] (Oxide raw materials)
[0078] As examples of oxide raw materials other than glass powder, as boron compounds, boric acid, sodium borate, ammonium borate, magnesium borate and lithium borate can be cited. As titanium compounds, rutile or anatase titanium oxide can be cited. As phosphorus compounds, orthophosphoric acid, metaphosphoric acid, sodium orthophosphate and sodium metaphosphate can be cited. As tungsten compounds, tungsten oxide, ammonium tungstate and sodium tungstate can be cited. As bismuth compounds, bismuth oxide, basic bismuth carbonate and sodium bismuthate can be cited. Among them, if boric acid, sodium tungstate, bismuth oxide or basic bismuth carbonate is used, disc-shaped particles with a high filling rate are formed, so it is preferred. Furthermore, by containing at least one element selected from the group consisting of iron, cobalt, copper, manganese and nickel, colored thermally conductive disc-shaped particles can be formed.
[0079] The above-mentioned oxide raw material can be used as long as it generates oxides through thermal decomposition or phase change. In addition to oxides, hydroxides, oxoacid salts, carbonates, bicarbonates, ammonium salts, etc. can also be used. By using a component that generates oxides through thermal decomposition or phase change as an oxide raw material, the particle size can be controlled, the reaction can be uniformed, and the particle surface can be smooth.
[0080] The content of glass powder in the raw material mixture must be 0.5 mass parts or more and 5 mass parts or less relative to 100 mass parts of aluminum raw material. If the amount of glass powder relative to 100 mass parts of aluminum raw material is less than 0.5 mass parts, the disc-shaped shape is weak, and the effect as disc-shaped particles cannot be expected. In addition, if the amount of glass powder added relative to 100 mass parts of aluminum raw material exceeds 5 mass parts, the particles accompanying the melting of the glass powder will be welded to each other, and the particles will become disc-shaped particles with poor dispersibility. From such a viewpoint, the content of glass powder in the raw material mixture is preferably more than 0.5 mass parts and less than 3 mass parts, more preferably more than 0.8 mass parts and less than 3 mass parts, and particularly preferably more than 1 mass part and less than 2 mass parts relative to 100 mass parts of aluminum raw material.
[0081] The content of the oxide raw material other than the glass powder in the raw material mixture is preferably 0.1 mass parts or more and 6 mass parts or less relative to 100 mass parts of the aluminum raw material. On the other hand, if the amount of the oxide raw material other than the glass powder relative to 100 mass parts of the aluminum raw material exceeds 6 mass parts, it sometimes causes an adverse effect on the disc-shaped effect of the glass powder, and there is a tendency that the thermal conductivity is reduced. If the amount of the oxide raw material other than the glass powder relative to 100 mass parts of the aluminum raw material is less than 0.1 mass part, there is a tendency that the target disc-shaped particles cannot be obtained. From such a viewpoint, the content of the oxide raw material other than the glass powder in the raw material mixture is more preferably 0.2 mass parts or more and 3 mass parts or less, and particularly preferably 0.3 mass parts or more and 2 mass parts or less relative to 100 mass parts of the aluminum raw material.
[0082] By making the amount of glass powder relative to 100 parts by mass of aluminum raw material and the amount of oxide raw materials other than glass powder within the above range, the disc-shaped particles of this embodiment can be formed into disc-shaped particles that can maintain various resistances, and have excellent thermal conductivity, chemical resistance, water resistance and electrical insulation, and have good mixing (filling) properties in resin, and can manufacture materials and articles such as resin compositions with excellent moldability.
[0083] The disc-shaped particles of this embodiment can be designed to have a small amount of glass powder or oxide raw materials other than glass powder added relative to the aluminum raw material, so the influence of aluminum oxide on thermal conductivity is small. In addition, the ability to manufacture by a simple process of calcining a mixture of powders is also an advantage in terms of cost. Furthermore, since the filling property in the resin is good, when considering the application in thermal conductive fillers, the problem of difficulty in designing at a high amount of filler addition, which is easy to become a problem in existing plate-shaped particles, can also be solved.
[0084] The disc-shaped particles of this embodiment can be suitably used as thermally conductive fillers, but can also be fully used for uses that meet the use conditions, such as disc-shaped alumina, abrasives, reflective materials, sliding materials, gas barrier materials, lubricants, hardness enhancement materials, or mechanical strength enhancement materials.
[0085] (Surface treatment)
[0086] The disc-shaped particles of the present embodiment can be surface treated. The affinity and dispersibility of the surface-treated disc-shaped particles to the resin are improved, and therefore, articles such as resin compositions with excellent thermal conductivity can be manufactured. As compounds (treatment agents) used in the surface treatment, fatty acids, fatty acid esters, fatty acid metal salts, phosphates, phosphate metal salts, silane coupling agents, surfactants, polymer aggregating agents, titanates and silicones can be cited. These treatment agents can be used alone or in combination of two or more. The amount of the compound used in the surface treatment is preferably set to 0.01 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the disc-shaped particles. As a treatment method, for example, there are: a method of treating by adding a treatment agent to a powder of disc-shaped particles and mixing it; a method of treating by adding a powder of disc-shaped particles to water and dispersing it, and then further adding a treatment agent, filtering and drying it; etc.
[0087] (Use of disc-shaped particles)
[0088] Among the preferred uses of the disc-shaped particles of the present embodiment, it is effective to add the particles to various plastics such as thermoplastic resins and thermosetting resins for the purpose of imparting thermal conductivity. As the thermoplastic resin, polyethylene resin, polypropylene resin, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, acrylonitrile-ethylene-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, acrylonitrile-styrene copolymer, polyvinyl chloride resin, polystyrene resin, polyacrylonitrile resin, polyamide resin, thermoplastic polyimide resin, thermoplastic urethane resin, polyaminobismaleimide resin, polyamideimide resin, polyetherimide resin, polymethyl methacrylate resin, polyvinyl acetate resin, polycarbonate resin, polyacetal resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyphenylene ether resin, polyphenylene sulfide resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, polyallyl sulfone resin, bismaleimide triazine resin, polymethylpentene resin, fluorinated resin, liquid crystal polymer, olefin-vinyl alcohol copolymer, ionomer resin and polyarylate resin can be used. These thermoplastic resins can be used alone or in combination of two or more. As thermosetting resins, phenolic resins, urea-formaldehyde resins, epoxy resins, melamine resins, silicone resins, polyurethane resins, unsaturated polyester resins, alkyd resins, polyimide resins, acrylic resins, and (modified) polyphenylene ethers can be used. These thermosetting resins can be used alone or in combination of two or more.
[0089] <Method for producing alumina-based disc-shaped particles>
[0090] Next, the method for producing the disc-shaped particles of the present embodiment is described. The method for producing the disc-shaped particles of the present embodiment comprises the following steps: a step of mixing aluminum raw material, glass powder, and oxide raw materials other than glass powder as appropriate to obtain a raw material mixture (step (1)); and a step of calcining the obtained raw material mixture (step (2)).
[0091] According to this manufacturing method, a disk-shaped alumina having a thickness compared to the conventional plate-shaped alumina can be easily obtained, and a disk-shaped alumina having a relatively small aspect ratio can be easily obtained because of the disk-shaped alumina. The reason for this is not necessarily clear, but the inventors speculate as follows. That is, the inventors speculate that the glass powder melts below the firing temperature, and the crystal orientation of the alumina is limited when the alumina crystal grows, so that the disk-shaped particles of the present embodiment can be obtained.
[0092] In step (1), an aluminum raw material, glass powder, and an oxide raw material other than the glass powder, if necessary, are mixed. As an apparatus for mixing the aluminum raw material and the oxide raw material, a pot mill, a Henschel mixer, a gas mixer, a cone mixer, a planetary ball mill, a vibration mill, a ribbon mixer, a vertical mixer, etc. are used to mix the components and then calcine. When mixing the components, the components only need to be uniformly mixed, and the particles of the components do not need to be crushed.
[0093] The amounts of the components in the raw material mixture are as described above.
[0094] In step (2), the raw material mixture obtained in step (1) is calcined at a temperature of not less than 1000°C and not more than 1400°C. In addition, it is preferably calcined at a temperature of not less than 1100°C and not more than 1300°C. By calcining, α-alumina of the aluminum raw material can be formed. If the calcination temperature is lower than 1000°C, it becomes difficult to form an α-alumina structure. The thermal conductivity of transition alumina is lower than that of α-alumina, so it is preferred to form α-alumina by calcination. On the other hand, even if the calcination temperature exceeds 1400°C, the properties of the obtained disc-shaped particles will not change significantly, and energy consumption is wasted. After calcination, the calcined product is crushed as needed, thereby obtaining the alumina-based thermally conductive disc-shaped particles of this embodiment. Regarding crushing, a known method can be used, and various equipment that has been used so far, such as a hammer mill, a roller mill, a ball mill, a jet mill, a bead mill, or a vibration mill, can be used.
[0095] <Thermal conductive composition>
[0096] In the thermally conductive composition, it is also a preferred embodiment to use the disc-shaped particles of the present embodiment in combination with other thermally conductive fillers such as aluminum oxide, boron nitride, graphite, zinc oxide, barium sulfate, talc, and magnesium oxide.
[0097] Common fillers are added to materials such as resins, rubbers, and coatings for the purpose of improving strength, functionality, etc. When the compounding amount of a thermal conductivity filler is increased, the melt fluidity and mechanical strength of materials such as resins are usually reduced. In addition, carbon-based fillers have conductivity, so there is a problem that the original characteristics of the resin, namely insulation, are easily damaged when compounded into the resin. Furthermore, although ceramic-based fillers have insulation properties, they have problems such as low thermal conductivity. Thermal conductivity fillers include, for example, metal-based fillers such as silver, copper, aluminum, and iron; inorganic-based fillers such as alumina, magnesia, silica, boron nitride, aluminum nitride, silicon carbide, boron carbide, and titanium carbide; and carbon-based fillers such as diamond, graphite (Japanese: 黒鉛), and graphite (Japanese: グラファイト). In electronic devices that require high electrical insulation, etc., fillers such as alumina, magnesia, zinc oxide, silica, boron nitride, aluminum nitride, and diamond are preferred. However, these fillers have many problems in terms of water resistance, chemical resistance, hardness, and electrical insulation.
[0098] In contrast, the disk-shaped particles of the present embodiment improve the weaknesses of the above various fillers and have excellent characteristics, so they can be suitably used as modified fillers. Furthermore, in order to make up for the weaknesses of the existing thermal conductivity fillers, it is also preferable to use them together with the above various thermal conductivity fillers. That is, in a thermal conductivity composition containing the above various thermal conductivity fillers, the application of the disk-shaped particles of the present embodiment is a preferred method prepared according to the target characteristics. In addition, for the disk-shaped particles of the present embodiment, even without adding pigments or dyes, coloring can be achieved by containing at least one element selected from the group consisting of iron, cobalt, copper, manganese, and nickel.
[0099] <Article>
[0100] The article of the present embodiment is an article (thermal conductivity article, thermal conductivity material) such as gravure ink, coating liquid, resin composition, and adhesive composition containing the aforementioned disk-shaped particles. It should be noted that it is also preferable to further contain the above various thermal conductivity fillers in the article of the present embodiment as needed.
[0101] (Gravure ink)
[0102] The disk-shaped particles of the present embodiment can be added to and used in gravure ink used as a topcoat agent for battery packaging materials, etc. The content of the disk-shaped particles in the gravure ink is preferably 5% by mass or more and 80% by mass or less, more preferably 10% by mass or more and 50% by mass or less, relative to the whole gravure ink. If such gravure ink (topcoat agent for battery packaging materials) is used, a battery packaging material with excellent chemical resistance such as acid resistance, high thermal conductivity, and high heat radiation rate can be produced.
[0103] (Coating liquid)
[0104] The disc-shaped particles of the present embodiment can be added to coating liquids such as coatings and used. For coating liquid, it is also possible to make disc-shaped particles and resins such as colorants, coatings or moldings formed and dispersed in carriers together with organic solvents etc. to mix and obtain the coloring preparation. The content of the disc-shaped particles in the coating liquid is preferably more than 5 mass % and below 80 mass %, more preferably more than 10 mass % and below 70 mass % relative to the coating liquid as a whole. The coating film formed using the coating liquid prepared in this way, the water resistance, chemical resistance and insulation of the coating molding are excellent, and strength is maintained and thermal conductivity is also excellent.
[0105] Specific examples of the resin that can be contained in the coating liquid include: polyolefin-based, polyester-based, polystyrene-based, acrylic-based, fluorine-based, polyamide-based, cellulose-based, polycarbonate-based, or polylactic acid-based thermoplastic resins; and urethane-based, phenol-based, or silicone-based thermosetting resins, etc. These resins may also be in the form of emulsions.
[0106] Specific examples of the liquid medium that can be contained in the coating liquid include water, methanol, ethanol, butanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, butyl acetate, cyclohexane, etc. These liquid media may be used in combination of two or more.
[0107] The coating liquid may also contain "other components" as appropriate according to the application and within the scope that does not impair the purpose of the present invention. Specific examples of "other components" include: antioxidants, ultraviolet absorbers, light stabilizers, dispersants, antistatic agents, lubricants, and bactericides.
[0108] As a method for applying the coating liquid, a conventionally known method can be used. Specifically, a method using spraying, brushing, electrostatic coating, curtain coating or roller coating, or a method based on dipping, etc. can be cited. In addition, as a drying method for forming the applied coating liquid into a film, a conventionally known method can also be used. Specifically, a method such as natural drying or baking can be appropriately selected according to the properties of the coating liquid.
[0109] If coating liquid is used, coating film and coating molding obtained by coating on substrate can be made. As substrate, metal, glass, natural resin, synthetic resin, ceramic, wood, paper, fiber, nonwoven fabric, woven fabric and leather etc. can be selected according to the purpose. It should be noted that the coating film endowed with functionality in this way can also be used in various industries such as industry, agriculture, mining or fishery except for household use. In addition, the coating shape is also not limited, and sheet or film can be selected according to the purpose.
[0110] (Resin composition)
[0111] By the disc-shaped particles of the present embodiment being compounded in resins such as polyamide resins and polyolefin resins, resin compositions can be made. More specifically, with respect to resin, according to known methods, disc-shaped particles are compounded and mixed with other additives as required, resin compositions can be obtained. And then, if the resin composition obtained is supplied to an extrusion molding machine and molded, a specified resin molding can be manufactured. The content of the disc-shaped particles in the resin composition is preferably more than 5% by mass and less than 95% by mass relative to the entire resin composition. By setting the content of the disc-shaped particles to the above-mentioned range, a resin composition with better water resistance, chemical resistance and insulation, and better strength and better moldability can be made. When the content of the disc-shaped particles exceeds 95% by mass, sometimes strength and moldability are reduced. On the other hand, when the content of the disc-shaped particles is less than 5% by mass, sometimes thermal conductivity is insufficient.
[0112] There is no particular limitation on the method of adding the disc-shaped particles to the resin, and existing known methods can be used. For example, in addition to the method of directly mixing the disc-shaped particles in the resin, mixing and molding, there is also a method of using a composition (masterbatch) in which the disc-shaped particles are dispersed in a resin, a lubricant, etc. at a high concentration in advance. As other additives, antioxidants, ultraviolet absorbers, antistatic agents, antibacterial agents, stabilizers, cross-linking agents, plasticizers, lubricants, release agents, flame retardants, and inorganic fillers such as talc, alumina, clay and silica can be listed. In addition, as a dispersing aid for the disc-shaped particles, metal soaps and polyethylene waxes can also be used. As metal soaps, for example, lithium stearate, magnesium stearate, zinc stearate, calcium stearate, magnesium palmitate, calcium oleate and cobalt oleate can be listed. As polyethylene wax, for example, various polyethylene waxes such as general polymerization type, degradation type or modified type can be used.
[0113] It should be noted that various organic pigments and inorganic pigments can also be mixed into the above-mentioned coating liquid and resin composition as colorants. As colorants, for example, organic pigments such as phthalocyanine pigments, azo pigments, azomethine pigments, isoindolinone pigments, quinacridone pigments, anthraquinone pigments, dioxazine pigments and perinone / perylene pigments can be listed; composite oxide pigments other than black; titanium oxide white pigments, titanium oxide yellow pigments and titanium oxide black pigments; and inorganic pigments such as carbon black, ultramarine and red iron. It should be noted that as phthalocyanine pigments, brominated phthalocyanine blue pigments, phthalocyanine green pigments, etc. can be listed. In addition, as azo pigments, polycondensed azo pigments, azomethine azo pigments, etc. can be listed.
[0114] Furthermore, a resin composition can also be obtained by melt-kneading a masterbatch mixture obtained by mixing disc-shaped particles, various pigments and additives with a resin for a mixture using an extruder or the like. More specifically, a resin composition can be obtained by the following methods, etc.: (i) a method of mixing disc-shaped particles and a dispersing aid with a resin for a mixture, adding other additives as needed, and mixing using a mixer such as a Henschel mixer; (ii) a method of mixing a masterbatch mixture using a kneader or a heated double-roll mill, cooling it, and then crushing it using a pulverizer to form a coarse powder; or (iii) a method of supplying the masterbatch mixture to an extruder for extrusion molding and molding it into a bead-like, column-like shape, etc. The molding method is not particularly limited, and for example, injection molding, extrusion molding, heating compression molding, blow molding, inflation molding, or vacuum molding can be used.
[0115] (Adhesive composition)
[0116] The disc-shaped particles of the present embodiment can be added to the adhesive and used as an adhesive composition. The type of resin contained in the adhesive is not limited, as long as it is a resin with adhesiveness such as urethane, epoxy, vinyl acetate or acrylic. In addition, the bonding mechanism is not limited, and it can be any one of a chemical reaction type, a solvent volatilization type, a hot melt type or a hot pressing type. The content of the disc-shaped particles in the adhesive composition is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 50% by mass or less relative to the adhesive composition as a whole. By setting the content of the disc-shaped particles to the above range, it is possible to make an adhesive composition with better thermal conductivity, adhesion, water resistance, chemical resistance and insulation. When the content of the disc-shaped particles exceeds 80% by mass, sometimes the bonding strength is insufficient. On the other hand, when the content of the disc-shaped particles is less than 5% by mass, sometimes the thermal conductivity is insufficient.
[0117] The disc-shaped particles of the present embodiment are made into thermally conductive articles and thermally conductive materials such as the above-mentioned gravure ink, coating liquid, resin composition and adhesive composition and utilized, so that they can also be used as electronic devices with heat dissipation (thermal conductivity) and excellent chemical resistance, water resistance and insulation. More specifically, it can be used for metal circuit substrates, circuit substrates, metal laminates, metal laminates with inner layer circuits, battery packaging materials, sealing materials or protective sheets, etc. Furthermore, it can be used as adhesive sheets, heat sinks, heat dissipation coating agents, semiconductor sealants, adhesives, heat dissipation spacers, greases, etc.
[0118] <Liquid composition>
[0119] The liquid composition of this embodiment is a liquid composition for forming a thermally conductive thin film, and contains: a thermally conductive component containing the above-mentioned disc-shaped particles, a film-forming resin, and a liquid medium. It should be noted that the thermally conductive component preferably further contains at least one selected from the group consisting of barium sulfate, talc, and boron nitride.
[0120] The content of the disc-shaped particles in the liquid composition is preferably 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 70% by mass or less relative to the entire liquid composition. In addition, the content of the thermally conductive component relative to 100 parts by mass of the film-forming resin is preferably 50 parts by mass or more and 600 parts by mass or less. The thermally conductive film formed using the liquid composition prepared in this way has excellent water resistance, chemical resistance and insulation, while maintaining strength and excellent thermal conductivity.
[0121] The film-forming resin is at least one solvent-soluble resin selected from the group consisting of acrylic resins, urethane resins, urea resins, epoxy resins, rubber resins, fluorine resins, polyamide resins, polyimide resins, silicone resins, cellulose resins, and thermoplastic elastomers. In addition, the liquid medium is the same as the liquid medium used in the above-mentioned coating liquid.
[0122] <Thermal conductive film and electronic device member>
[0123] The thermally conductive film of this embodiment is a film formed by applying the liquid composition. The thickness of the thermally conductive film is preferably 20 μm or more and 1000 μm or less, and more preferably 50 μm or more and 200 μm or less.
[0124] Furthermore, the electronic device member of the present embodiment is a member including a metal member and the thermally conductive thin film disposed on the surface of the metal member.
[0125] Examples of the metal member include a metal circuit board, a circuit board, a metal laminate, and a metal-clad laminate with an inner layer circuit.
[0126] Example
[0127] The present invention will be specifically described below based on Examples, but the present invention is not limited to these Examples. It should be noted that "parts" and "%" in Examples and Comparative Examples are based on mass unless otherwise specified.
[0128] <Aluminum Raw Materials>
[0129] The following aluminum raw materials were used.
[0130] Boehmite: spherical, average particle size 3μm
[0131] Aluminum hydroxide A: spherical, average particle size 6μm
[0132] Aluminum hydroxide B: spherical, average particle size 10 μm
[0133] Aluminum hydroxide C: spherical, average particle size 1μm
[0134] <Glass powder>
[0135] As the glass frit, the following metal-containing glass frit was used.
[0136] Glass powder A: sag temperature 390℃, contains silicon, boron and fluorine, etc.
[0137] Glass powder B: sag temperature 460℃, contains silicon, boron and fluorine, etc.
[0138] Glass powder C: sag temperature 540℃, contains silicon, boron and fluorine, etc.
[0139] <Production of Thermally Conductive Disc-Shaped Particles> (Example 1)
[0140] 100 parts of aluminum hydroxide A and 1 part of glass powder A were added to a small stirrer and stirred to obtain a raw material mixture. The obtained raw material mixture was calcined at 1200° C. in air for 3 hours and then crushed to obtain powdery thermally conductive disc-shaped particles.
[0141] (Examples 2 to 28)
[0142] Except for using the aluminum raw material, glass powder, and oxide raw material of the types and amounts shown in Table 1, the same procedure as in Example 1 was carried out to obtain powdery thermally conductive disc-shaped particles.
[0143] (Comparative Example 1)
[0144] A sample of Comparative Example 1 was prepared by calcining 100 parts of aluminum hydroxide A at 1200° C. for 2 hours in air to obtain a powder.
[0145] (Comparative Example 2)
[0146] A raw material mixture was obtained by mixing 100 parts of aluminum hydroxide A and 7 parts of glass powder A in the same manner as in Example 1. The obtained raw material mixture was calcined in air at 1200° C. for 2 hours to obtain a powder as a sample of Comparative Example 2.
[0147] (Comparative Example 3)
[0148] A sample of Comparative Example 3 was prepared by calcining 100 parts of boehmite at 1200° C. for 2 hours in air to obtain a powder.
[0149] (Comparative Examples 4 to 9)
[0150] The substances shown in Table 1 were used as samples of Comparative Examples 4 to 9, respectively.
[0151] [Table 1]
[0152]
[0153] <Evaluation (1)>(Filling property)
[0154] The maximum filling amount of the powder obtained in Examples 1 to 28 and Comparative Examples 1 to 9 in epoxy resin was evaluated. As an evaluation method, the aforementioned powder was kneaded in the epoxy resin with a spatula and slowly added gradually, and the addition amount when it became a powder state and could not maintain a block state was taken as the maximum filling amount. Based on the maximum filling amount at this time, the filling property was evaluated using the following evaluation criteria. The results are shown in Table 2.
[0155] AA: Filling volume more than 80%
[0156] A: Filling volume is more than 75% and less than 80%
[0157] B: Filling volume is more than 70% and less than 75%
[0158] F: Filling less than 70%
[0159] (Abrasion Formability)
[0160] A resin composition obtained by mixing 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 minutes) and 70 parts of a thermally conductive oxide was placed in a Plastomill and melt-kneaded at a set temperature of 200°C. Next, a mold pressure molding was performed at 175°C using a mold of 20 mm in length × 20 mm in width × 6 mm in height to produce a test piece. The mechanical wear properties during production and the surface state of the produced molded body were observed, and the wear moldability was evaluated according to the evaluation criteria shown below. The results are shown in Table 2.
[0161] A: There are no particular issues with abrasion and surface condition.
[0162] B: There is a problem with either abrasion or surface condition
[0163] F: There are problems with both abrasion and surface condition
[0164] (average particle size, average thickness and aspect ratio)
[0165] The average particle size of the powders obtained in Examples 1 to 28 and Comparative Examples 1 to 9 was measured using a Mastersizer 3000 (manufactured by Malvern Panalytical Ltd.). Specifically, the powders were added to a 0.2% sodium metaphosphate aqueous solution and subjected to a deflocculation treatment for 2 minutes using an ultrasonic cleaner (manufactured by AS ONE Corporation, ASU-6D), followed by measurement. The results are shown in Table 2.
[0166] The powders obtained in Examples 1 to 28 and Comparative Examples 1 to 9 were observed using an electron microscope, and the average thickness of 10 particles was calculated. It should be noted that particles with known particle thickness were selected as the particles to be observed. The results are shown in Table 2. It should be noted that electron microscope photographs of the powders obtained in Examples 2, 19 and 26, and Comparative Example 2 are shown in Table 2. Figure 1 to Figure 4 In addition, in Comparative Examples 1 to 4, 8 and 9, Figure 4 As shown, the particles have disordered shapes and the average thickness cannot be determined.
[0167] Furthermore, the powder obtained in Example 1 was observed with an electron microscope, and the average particle size of 10 particles was calculated. As a result, it was confirmed that the measured value was substantially consistent with the measured value using Mastersizer 3000.
[0168] The aspect ratio (average particle diameter / average thickness) was calculated from the average particle diameter and average thickness values for the powders obtained in Examples 1 to 28 and Comparative Examples 1 to 4, 8, and 9. The results are shown in Table 2.
[0169] (Determination of thermal conductivity)
[0170] A resin composition obtained by kneading 30 parts of a mixed solution of an epoxy resin (manufactured by Mitsubishi Chemical Corporation) and an amine curing agent (manufactured by DIC Corporation) and 70 parts of a thermally conductive oxide was molded and pressed into a circular sheet having a diameter of 100 mm or more and a thickness of 4 mm or more. After that, it was dried for 30 minutes at a set temperature of 120°C, and after natural cooling, it was cut into four equal parts in a fan-shaped manner with a central angle of 90° to prepare a test piece. The thermal conductivity of the prepared test piece was measured using a hot plate method thermal property measuring device (trade name "TPS-2500S", manufactured by Kyoto Electronics Industry Co., Ltd.). The results are shown in Table 2.
[0171] (Insulation)
[0172] The test piece of the epoxy resin composition for evaluation used in the measurement of thermal conductivity was used to measure the volume resistivity with a resistivity meter. Based on the measurement results, the insulation properties were evaluated according to the following evaluation criteria. The results are shown in Table 2.
[0173] A: Volume resistivity is 10 10 Ω·cm or more
[0174] B: Volume resistivity is 10 5 Ω·cm or more and less than 10 10 Ω·cm
[0175] F: Volume resistivity is less than 10 5 Ω·cm
[0176] [Table 2]
[0177]
[0178] (Reference example)
[0179] When measuring the thermal conductivity, 60 parts of the powder obtained in Example 21 and 10 parts of Example 3 of Japanese Patent No. 6209695 were used for 70 parts of the thermally conductive oxide to prepare a test piece. As a test method for thermal conductivity, a resin composition obtained by mixing 30 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR: 20 g / 10 minutes) and 70 parts of the thermally conductive oxide was placed in a plastomill and melt-kneaded at a set temperature of 200°C.
[0180] Next, a test piece was produced by mold pressure molding at 175°C using a mold of 20 mm in length × 20 mm in width × 6 mm in height. The thermal conductivity of the produced test piece was measured using a thermal property measuring device (trade name "TPS-2500S", manufactured by Kyoto Electronics Industry Co., Ltd.). At this time, the filling property was AA, the wear formability was A, the insulation property was A, and the thermal conductivity was 1.12 W / m·K. Even if particles of different shapes were mixed, the results were basically the same as those in the case of using only disc-shaped particles, which were within the scope of the embodiment.
[0181] <Preparation and evaluation of coating liquid> (Application example 1, comparative application example 1)
[0182] 15 parts of each powder (thermal conductive oxide) obtained in Example 21 and Comparative Example 4, 62 parts of urethane resin with a viscosity of 3500 mPa·s, and 23 parts of ethyl acetate were mixed and dispersed with a disperser to prepare a coating liquid. After each prepared coating liquid was evenly applied to release paper using a glass rod, it was placed in an oven at 100°C for 2 minutes to volatilize the solvent component to form a coating film with a thickness of 50 μm (Application Example 1, Comparative Application Example 1). The thermal conductivity of the coating film was measured, and the result showed that the thermal conductivity of the coating film of Comparative Application Example 1 formed with α-alumina of Comparative Example 4 was 0.29 W / m·K. In contrast, it can be seen that the thermal conductivity of the coating film of Application Example 1 formed with the thermal conductive oxide of Example 21 is as high as 0.36 W / m·K. In addition, the coating liquid prepared using the thermal conductive oxide of Example 21 was applied to a nylon film for battery exterior materials using a gravure coater and used as a topcoat for battery exterior materials. As a result, it was found that heat can be efficiently dissipated and the temperature rise of the battery can be reduced.
[0183] <Preparation and evaluation of adhesive> (Application example 2, comparative application example 2)
[0184] 35 parts of each of the powders (thermally conductive oxides) obtained in Example 21 and Comparative Example 4 were mixed with 65 parts of a polyester polyol having a viscosity of 300 mPa·s, and dispersed using a disperser to prepare a dispersion. 98 parts of the prepared dispersion were mixed with 2 parts of polyisocyanate having a viscosity of 2600 mPa·s, and stirred using a dissolver to obtain a chemical reaction type adhesive of a urethane resin system. After applying each of the obtained adhesives evenly on release paper using a glass rod, the adhesives were placed in an oven at 100°C for 2 minutes to volatilize the solvent component. Furthermore, the adhesives were placed in an oven at 40°C for 96 hours to form a cured film of the adhesive (Application Example 2, Comparative Application Example 2). The thermal conductivity of the cured film was measured, and the thermal conductivity of the cured film of Comparative Application Example 2 formed using the α-alumina of Comparative Example 4 was 0.53 W / m·K. In contrast, it can be seen that the thermal conductivity of the cured film of Application Example 2 formed using the thermally conductive oxide of Example 21 is as high as 0.63 W / m·K.
[0185] <Production of Liquid Composition> (Application Example 3, Comparative Application Example 3)
[0186] 20 parts of each of the powders (thermally conductive oxides) obtained in Example 21 and Comparative Example 4, 63 parts of a polyurethane resin (trade name "SANPRENE IB-1700D", manufactured by Sanyo Chemical Industries, Ltd., 30% resin component, 70% solvent component) as a film-forming resin, and 17 parts of a methyl ethyl ketone / toluene / isopropyl alcohol mixed solvent as a solvent were mixed and stirred with a paint shaker (using glass beads (diameter 2 mm)) to obtain a dispersion. After adding 3 parts of a polyisocyanate resin (trade name "TAKENATE D-160N", manufactured by Mitsui Chemicals, Inc., 75% resin component, 25% solvent component) to 100 parts of the obtained dispersion, the mixture was stirred to obtain a liquid composition (Application Example 3, Comparative Application Example 3).
[0187] <Evaluation (2)> (Formation of coating film for evaluation)
[0188] The liquid compositions were applied onto release paper using a multi-functional coater (trade name "K-303", manufactured by RK Print Coat Instruments), and then dried with hot air to remove the solvent. Subsequently, the compositions were aged in a dryer at 40°C for 48 hours to form a coating film for evaluation having a concentration of 48% of a thermally conductive component (filler) and a film thickness of about 100 μm.
[0189] (Determination of thermal conductivity (thin film))
[0190] The coating film for evaluation was cut into a size of 40 mm in length and 40 mm in width to obtain a test piece. The thermal conductivity of the obtained test piece was measured by the "thin film measurement module" of the thermal property measurement device (trade name "TPS-2500S", manufactured by Kyoto Electronics Industry Co., Ltd.). The thermal conductivity of the cured film of Comparative Application Example 3 formed using the α-alumina of Comparative Example 4 was 0.33 W / m·K. In contrast, it can be seen that the thermal conductivity of the cured film of Application Example 3 formed using the thermally conductive oxide of Example 21 is as high as 0.53 W / m·K.
[0191] (Determination of thermal conductivity (bulk))
[0192] A resin composition obtained by mixing 50 parts of polypropylene (manufactured by Prime Polymer Co., Ltd., MFR 20g / 10 minutes) and 50 parts of each thermally conductive component was placed in a Plastomill and melt-kneaded at a set temperature of 200°C. Next, a test piece was obtained by mold compression molding at 175°C using a mold of 20 mm in length × 20 mm in width × 6 mm in height. The thermal conductivity of the obtained test piece was measured by the "standard isotropic measurement module" of a thermal property measuring device (trade name "TPS-2500S", manufactured by Kyoto Electronics Industry Co., Ltd.). The thermal conductivity of Comparative Application Example 3 formed using the α-alumina of Comparative Example 4 is 0.47 W / m·K. In contrast, it can be seen that the thermal conductivity of Application Example 3 formed using the thermally conductive oxide of Example 21 is as high as 0.62 W / m·K.
[0193] (Chemical resistance)
[0194] The coating film for evaluation was cut into a size of 40 mm in length × 40 mm in width × 100 μm in thickness to obtain a test piece. The obtained test pieces were immersed in 5% hydrochloric acid, 5% sulfuric acid aqueous solution, 5% nitric acid aqueous solution and 5% sodium hydroxide aqueous solution, respectively, stirred once a day, and left to stand for one week. The mass of the test piece before and after immersion was measured and the mass change rate (%) based on the mass of the test piece before immersion was calculated, and the chemical resistance was evaluated according to the evaluation criteria shown below. As a result, both Application Example 3 and Comparative Application Example 3 were all A.
[0195] A: Quality change rate is less than 5%
[0196] B: Mass change rate is 5% or more and less than 20%
[0197] F: Mass change rate is more than 20%
[0198] (Adhesion)
[0199] The liquid composition was applied to the corona treated surface (treated PET, treated NY) and the non-corona treated surface (untreated PET, untreated NY) of a biaxially stretched polyester film (trade name "ESTER FILME-5102", manufactured by Toyobo Co., Ltd.) and a biaxially stretched nylon film (trade name "Harden FILM N1102", manufactured by Toyobo Co., Ltd.) using a rod coater #5. After hot air drying to remove the solvent, the film was aged in a dryer at 40°C for 48 hours to obtain a test piece having a thin film formed on the film surface. A transparent tape (trade name "Cellotape (registered trademark)", manufactured by Nichiban Co., Ltd., 24 mm wide) was pasted on the film surface of the test piece, and the peeling operation in the vertical direction was performed 3 times at the same position, and then the state of the film was confirmed. The adhesion was evaluated according to the evaluation criteria shown below. As a result, both Application Example 3 and Comparative Application Example 3 were A.
[0200] A: No peeling
[0201] B: There is partial peeling
[0202] F: Mostly peeled off
Claims
1. Alumina-based thermally conductive disc-shaped particles, which are particles of alumina-based thermally conductive oxide obtained by calcining a raw material mixture containing an aluminum raw material and a glass powder, in, The raw material mixture excludes those containing boric acid compounds, The aluminum raw material is at least one selected from the group consisting of boehmite and aluminum hydroxide, The sag temperature of the glass powder is 300° C. or higher and 800° C. or lower. The content of the glass powder in the raw material mixture is 0.5 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the aluminum raw material. The primary particles of the alumina-based thermally conductive oxide have an average particle size of 1 μm to 50 μm, an average thickness of 0.1 μm to 5 μm, an aspect ratio of more than 1 to 50, and a disc shape.
2. The alumina-based thermally conductive disc-shaped particles according to claim 1, in, The raw material mixture further contains an oxide raw material other than the glass frit, and the oxide raw material includes at least one selected from the group consisting of titanium compounds, phosphorus compounds, tungsten compounds, and bismuth compounds.
3. The alumina-based thermally conductive disc-shaped particles according to claim 1, in, The alumina-based thermally conductive oxide contains at least one element selected from the group consisting of iron, cobalt, copper, manganese, and nickel, and is colored.
4. The alumina-based thermally conductive disc-shaped particles according to claim 1, in, The glass powder does not contain lead.
5. A method for producing alumina-based thermally conductive disc-shaped particles, the method being the method for producing alumina-based thermally conductive disc-shaped particles according to any one of claims 1 to 4, the method comprising the following steps: A step of mixing at least one aluminum raw material selected from the group consisting of boehmite and aluminum hydroxide with glass powder to obtain a raw material mixture; and, The obtained raw material mixture is calcined. The content of the glass powder in the raw material mixture is 0.5 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the aluminum raw material. In the step of calcining the raw material mixture, the raw material mixture is calcined in air at 1000° C. or higher and 1400° C. or lower. 6 . A thermally conductive composition comprising: a thermally conductive filler and the alumina-based thermally conductive disc-shaped particles according to claim 1 . 7 . An article comprising the alumina-based thermally conductive disc-shaped particles according to claim 1 .
8. The article of claim 7, further comprising a thermally conductive filler.
9. The article according to claim 7, in, The article is any one of a gravure ink, a coating liquid, a resin composition, and an adhesive composition.
10. A liquid composition for forming a thermally conductive thin film, The liquid composition contains: A film-forming resin, a liquid medium, and a thermally conductive component comprising the alumina-based thermally conductive disc-shaped particles according to any one of claims 1 to 4.
11. The liquid composition according to claim 10, in, The thermally conductive component further contains a thermally conductive filler, The thermally conductive filler is at least one selected from the group consisting of barium sulfate, talc, and boron nitride.
12. The liquid composition according to claim 10, in, The content of the thermally conductive component is 50 parts by mass or more and 600 parts by mass or less relative to 100 parts by mass of the film-forming resin.
13. The liquid composition according to claim 10, in, The film-forming resin is at least one solvent-soluble resin selected from the group consisting of acrylic resins, urethane resins, urea resins, epoxy resins, rubber resins, fluorine resins, polyamide resins, polyimide resins, silicone resins, cellulose resins and thermoplastic elastomers.
14. A thermally conductive film formed by coating the liquid composition according to claim 10. 15 . An electronic device member comprising: a metal member; and the thermally conductive film according to claim 14 disposed on a surface of the metal member.
Citation Information
Patent Citations
Thermally conductive complex oxide, production method therefor, thermally conductive complex oxide-containing composition, and use therefor
CN106103346A
Alumina-based heat conductive oxide and method for producing same
CN108025980A
Alumina-based thermally conductive oxide and method for producing same
CN110352178A
Heat-conductive composite oxide, heat-conductive resin composition and coating liquid
JP2016135841A