Poly (butylene succinate) (PBS)-based resin vaporization accelerator and composition comprising same
A PBS-based resin composition with a vaporization accelerator enhances biodegradation by increasing carbon dioxide production, addressing slow decomposition rates and environmental pollution from PBS-based plastics.
Patent Information
- Application Number
- CN202380030405.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-12-03
AI Technical Summary
PBS-based resins have low decomposition rates under natural conditions, particularly at room temperature, posing environmental pollution challenges due to slow biodegradation.
A composition comprising a polybutylene succinate (PBS)-based resin with a vaporization accelerator, such as a PHA resin, to enhance biodegradation by increasing the vaporization degree, measured by carbon dioxide production, to at least 20% over 12 weeks at 30°C.
The composition accelerates the biodegradation of PBS-based resins, achieving a significant biodegradation effect even at room temperature, effectively addressing environmental pollution issues while maintaining excellent physical properties.
Smart Images

Figure BDA0005059673540000021 
Figure BDA0005059673540000022 
Figure BDA0005059673540000031
Abstract
Description
Technical Field
[0001] The present invention relates to a vaporization accelerator for accelerating the vaporization of a polybutylene succinate (PBS)-based resin and a composition containing the vaporization accelerator. Background Art
[0002] The general-purpose plastics currently on the market have excellent physical properties, and due to stable supply and prices, demand is increasing. However, the problem of the disposal of waste plastics continues to arise in life. Since they do not decompose under natural conditions such as oceans and soil, they are becoming a factor causing serious environmental pollution problems.
[0003] In order to solve these environmental pollution problems, research on biodegradable plastics has been actively carried out in recent years.
[0004] Biodegradable plastics refer to materials that can be decomposed into low molecular weight substances by microorganisms existing in nature and ultimately decomposed into water and carbon dioxide, or water and methane gas.
[0005] The polymer resin commonly used as such biodegradable plastic is polylactic acid (PLA) resin. In recent years, research is being actively conducted using polybutylene succinate (PBS)-based resins such as polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and polybutylene succinate terephthalate (PBST), which have superior decomposition rates and moldability to PLA resins.
[0006] However, these PBS-based resins actually take a long time to decompose. In particular, it is difficult to achieve complete biodegradation under natural conditions such as oceans and soils, and there are still limitations in increasing the decomposition rate under room temperature conditions. Summary of the invention
[0007] Technical issues
[0008] The present invention is designed to solve the above-mentioned problems of the prior art.
[0009] The present invention aims to provide a vaporization accelerator for polybutylene succinate (PBS)-based resin to increase the vaporization degree of polybutylene succinate (PBS)-based resin having a low vaporization degree at room temperature of 30°C, thereby accelerating the biodegradation effect (rate) of the polybutylene succinate (PBS)-based resin even at room temperature. The present invention also aims to provide a composition comprising the vaporization accelerator.
[0010] Solution to the problem
[0011] According to aspects of the present invention, there is provided a composition comprising a polybutylene succinate (PBS)-based resin in an amount of 10 wt % to less than 100 wt % based on the total weight of the composition, wherein when the cumulative amount of carbon dioxide (CO2) generated at 30° C. over 12 weeks is measured according to ISO 14855, the vaporization degree (V) represented by the following formula 1 is 10w ) is 20% or more:
[0012] [Formula 1]
[0013]
[0014] In formula 1, (CO2) S is the cumulative amount of carbon dioxide (CO2) produced in the test container containing the compost and the sample (in grams), based on the total dry weight of the sample and compost, the amount of the sample being 14.3% by weight; (CO2) B is the cumulative amount of carbon dioxide (CO2) (grams) produced in the inoculated container containing only compost, (CO2) THV is the theoretical cumulative amount of carbon dioxide (CO2) produced in the test container and is expressed by the following formula 2,
[0015] [Formula 2]
[0016]
[0017] In Formula 2, Cw is the mass (gram) of organic carbon contained in the sample.
[0018] In embodiments, the composition may further include a vaporization accelerator for the polybutylene succinate (PBS) based resin.
[0019] In another embodiment, a weight ratio of the polybutylene succinate (PBS)-based resin to the vaporization accelerator for the polybutylene succinate (PBS)-based resin may be 10:90 to 90:10.
[0020] In another embodiment, the composition may have a vaporization enhancement improvement (ΔVID) of 0.1% or more. 10W ), as shown in Formula 3 below:
[0021] [Formula 3]
[0022] ΔVID 10W (%) = V 10w –V THV10w
[0023] In Formula 3, V 10w As defined above, and V THV10w It is expressed by the following formula 4:
[0024] [Formula 4]
[0025]
[0026] In Formula 4, x is the weight percentage of the polybutylene succinate (PBS)-based resin included in the composition, based on the total weight of the composition.
[0027] In another embodiment, the vaporization accelerator for the polybutylene succinate (PBS)-based resin may satisfy at least one of the following properties: a glass transition temperature (Tg) of -45°C to 80°C, a crystallization temperature (Tc) of 60°C to 120°C, and a melting temperature (Tm) of 100°C to 170°C.
[0028] In another embodiment, the polybutylene succinate (PBS)-based resin may include at least one selected from polybutylene succinate (PBS), polybutylene succinate adipate (PBSA) and polybutylene succinate terephthalate (PBST), and the vaporization promoter for the polybutylene succinate (PBS)-based resin may include a resin containing repeating units derived from 4-hydroxybutyrate (4-HB) monomers and repeating units derived from at least one monomer selected from the following: 3-hydroxybutyrate (3-HB), 3-hydroxypropionate (3-HP), 3-hydroxyvalerate (3-HV), 3-hydroxyhexanoate (3-HH), 4-hydroxyvalerate (4-HV), 5-hydroxyvalerate (5-HV) and 6-hydroxyhexanoate (6-HH).
[0029] In another embodiment, the vaporization accelerator for a polybutylene succinate (PBS)-based resin may include a resin containing repeating units derived from a 3-hydroxybutyrate (3-HB) monomer and repeating units derived from a 4-hydroxybutyrate (4-HB) monomer.
[0030] In another embodiment, the resin may contain repeating units derived from 4-hydroxybutyrate (4-HB) monomers in an amount of 1 mol % to 80 mol %, based on the total moles of repeating units derived from 3-hydroxybutyrate (3-HB) monomers and repeating units derived from 4-hydroxybutyrate (4-HB) monomers.
[0031] According to another aspect of the present invention, there is provided a vaporization accelerator for a polybutylene succinate (PBS)-based resin, comprising a resin containing repeating units derived from a 3-hydroxybutyrate (3-HB) monomer and a repeating unit derived from a 4-hydroxybutyrate (4-HB) monomer.
[0032] In an embodiment, a molar ratio of a repeating unit derived from a 3-hydroxybutyrate (3-HB) monomer to a repeating unit derived from a 4-hydroxybutyrate (4-HB) monomer contained in the resin may be 40:60 to 99:1.
[0033] Advantageous Effects of the Invention
[0034] The composition according to an embodiment of the present invention includes a polybutylene succinate (PBS)-based resin having a low vaporization degree at a room temperature of 30° C., wherein the vaporization degree reaches a specific level or more when the cumulative amount of carbon dioxide (CO 2 ) generated over 12 weeks is measured, thereby achieving an excellent biodegradation effect at room temperature.
[0035] In addition, the vaporization accelerator for the polybutylene succinate (PBS)-based resin can significantly accelerate the vaporization of the polybutylene succinate (PBS)-based resin having a low vaporization degree at a room temperature of 30°C.
[0036] Therefore, the composition and the vaporization accelerator for polybutylene succinate (PBS)-based resin can be used in various fields to effectively protect the environment while having excellent physical properties. DETAILED DESCRIPTION
[0037] Hereinafter, the present invention will be described in detail with reference to the embodiments. Here, the embodiments are not limited to those described below. On the contrary, they can be modified into various forms as long as the gist of the present invention is not changed.
[0038] Throughout the specification, when a part is referred to as “comprising” a certain element, it should be understood that it may include other elements rather than excluding other elements, unless specifically stated otherwise.
[0039] Additionally, unless otherwise indicated, all numbers expressing physical properties, dimensions, and so forth of elements used herein are to be understood as being modified by the term "about."
[0040] The present invention relates to a composition (a vaporizable composition or a biodegradable composition) in which the vaporization degree (V) calculated by applying the cumulative amount of carbon dioxide (CO2) generated under aerobic composting conditions is 10w ) is controlled within a specific range or higher, so that even if the composition contains a polybutylene succinate (PBS)-based resin that is difficult to biodegrade at room temperature (e.g., 25±5°C), the composition can be easily biodegraded at room temperature (e.g., 25±5°C). The present invention also relates to a vaporization accelerator for the polybutylene succinate (PBS)-based resin contained in the composition, which will be described in detail below.
[0041] [Composition]
[0042] The composition according to an embodiment of the present invention comprises a polybutylene succinate (hereinafter referred to as "PBS")-based resin in an amount of 10 wt% to less than 100 wt% based on the total weight of the composition, wherein when the cumulative amount of carbon dioxide (CO2) generated at 30°C for 12 weeks is measured according to ISO 14855, the vaporization degree (V) represented by the following formula 1 is 10w ) is 20% or more:
[0043] [Formula 1]
[0044]
[0045] In formula 1, (CO2) S is the cumulative amount of carbon dioxide (CO2) produced in the test container containing the compost and the sample (composition sample), the amount of the sample being 14.3% by weight, (CO2) based on the total dry weight of the sample and the compost. B is the cumulative amount of carbon dioxide (CO2) (grams) produced in the inoculated container containing only compost, (CO2) THV is the theoretical cumulative amount (g) of carbon dioxide (CO2) generated in the test container (the test container (a+b) containing the compost (a) and the sample (b), the amount of the sample (b) is 14.3 wt% based on the total dry weight of the sample and the compost (the dry weight of the sample + the dry weight of the compost)) and is represented by the following formula 2,
[0046] [Formula 2]
[0047]
[0048] In Formula 2, Cw is the mass (gram) of organic carbon (carbon element) contained in the sample (based on the total weight (x+y) of the dry weight of the sample (x) and the dry weight of the compost (y), the amount of the sample is 14.3 wt%). Specifically, Cw refers to the content (gram) of carbon element measured when the sample is subjected to elemental analysis.
[0049] For measuring (CO2) S and (CO2) B The weight of the compost can be the same. In addition, the dry weight of the compost can be calculated by the loss on drying (LOD) based on the thermogravimetric measurement principle of moisture. That is, the difference in weight loss is measured when the compost is dried, and the dry weight can be calculated by moisture analysis using a drying oven or a halogen moisture analyzer (HMA).
[0050] Vaporization degree (V 10w ) is a value measured when the composition is decomposed into low molecular weight substances and finally completely decomposed into carbon dioxide and vaporized, rather than the biodisintegration degree (biodisintegration effect) when the composition is decomposed into small pieces or small molecules.
[0051] Specifically, the vaporization degree (V 10w ) is a value obtained by measuring the cumulative amount of carbon dioxide (CO2) generated (which is the final decomposition product of the composition) and substituting the measured cumulative amount of carbon dioxide (CO2) into Formula 1 and Formula 2 in accordance with the provisions of ISO 14855 notification (specifically, the aerobic biodegradability evaluation method of ISO14855-1), which is an indicator of the degree of biodegradation of the composition at room temperature of 30°C.
[0052] The composition according to an embodiment of the present invention may further include a vaporization accelerator for polybutylene succinate (PBS)-based resin (hereinafter referred to as "vaporization accelerator for PBS-based resin"). Specifically, the composition further including the vaporization accelerator for PBS-based resin may have a vaporization degree (V) of 20% or more represented by Formula 1. 10w More specifically, the vaporization degree (V 10w ) may be an indicator of the biodegradation degree of a composition comprising a PBS-based resin and a vaporization accelerator for the PBS-based resin.
[0053] That is, the vaporization degree (V 10w ) may be a value obtained by the following procedure: as an evaluation group, a composition sample comprising a PBS-based resin and a vaporization accelerator for a PBS-based resin at a specific content ratio is mixed with compost and placed in a test container, and then the cumulative amount (g) of carbon dioxide (CO2) generated by the composition sample under aerobic composting conditions at 30°C for 12 weeks is measured using a measuring and evaluating device (ECHO's permeameter device) ((CO2) S ); as a control group, the cumulative amount of carbon dioxide (CO2) produced in an inoculated container containing only compost but not a composition sample was obtained under the same conditions as the evaluation group ((CO2) B ); Measurement (CO2) S With (CO2) B The difference between (CO2) S and (CO2) B The cumulative amount of carbon dioxide (CO2) produced in the evaluation group and the control group respectively (g); divided by the theoretical cumulative amount of carbon dioxide (CO2) produced (g) as expressed in Formula 2 ((CO2) THV ) and convert it into a percentage.
[0054] The composition according to an embodiment of the present invention includes a PBS-based resin, and when the cumulative amount of carbon dioxide (CO2) generated over 12 weeks is measured, the composition has a vaporization degree (V) of a specific level or higher. 10w); therefore, even if it contains a PBS-based resin having a low vaporization degree, it can produce an excellent biodegradation effect under aerobic composting conditions at room temperature of 30° C. The pressure condition in the aerobic composting condition may be normal pressure.
[0055] Specifically, the vaporization degree (V 10w ) can be, for example, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, 48% or more, 50% or more, 55% or more, 60% or more, or 65% or more (e.g., 20% to 80%, 25% to 75%, 30% to 70%, or 40% to 69%).
[0056] At the same time, (CO2) in Formula 1 S It can be, for example, 5 grams or more, 10 grams or more, 20 grams or more, 30 grams or more, 35 grams or more, 40 grams or more, 45 grams or more, 50 grams or more, 55 grams or more, or 60 grams or more. In addition, (CO2) S It can be, for example, 65 grams or less, 63 grams or less, 60 grams or less, 58 grams or less, or 55 grams or less.
[0057] In formula 1, (CO2) S and (CO2) B The difference between refers to the actual cumulative amount of carbon dioxide (CO2) produced by the sample (composition sample) itself, which can be, for example, 1 gram or more, 2 grams or more, 3 grams or more, 5 grams or more, or 10 grams or more. In addition, (CO2) S and (CO2) B The difference therebetween may be, for example, 80 grams or less, 70 grams or less, 60 grams or less, 50 grams or less, 40 grams or less, or 30 grams or less.
[0058] (CO2) in Formula 1 THV It refers to the theoretical maximum cumulative amount (g) of carbon dioxide (CO2) produced when the sample (composition sample) is completely oxidized in a test container containing compost and sample (when 100% of the organic carbon contained in the sample is converted into carbon dioxide (CO2)), which can be expressed by Formula 2. That is, (CO2) THV It can be the mass of organic carbon (carbon atoms) contained in the sample (Cw) multiplied by the ratio of the molecular weight of carbon dioxide (44) to the atomic weight of carbon atoms (12) (44 / 12). (CO2) THV It can be, for example, 5 grams or more, 6 grams or more, 7 grams or more, 10 grams or more, 15 grams or more, 20 grams or more, 30 grams or more, 40 grams or more, or 50 grams or more. In addition, (CO2)THV It can be, for example, 80 grams or less, 70 grams or less, 60 grams or less, 55 grams or less, 50 grams or less, 45 grams or less, or 42 grams or less.
[0059] Meanwhile, the composition according to the embodiment of the present invention may have a vaporization promotion improvement degree (ΔVID 10W ), as shown in Formula 3 below:
[0060] [Formula 3]
[0061] ΔVID 10W (%) = V 10w –V THV10w
[0062] In Formula 3, V 10w As defined above, V THV10w It is represented by the following formula 4:
[0063] [Formula 4]
[0064]
[0065] In Formula 4, x is the weight percentage of the PBS-based resin contained in the composition, based on the total weight of the composition. Meanwhile, in Formula 4, 3% refers to the cumulative amount of carbon dioxide (CO2) generated by a composition consisting of 100 weight % of the PBS-based resin (composition containing only the PBS-based resin) at 30° C. for 12 weeks according to ISO 14855, and the vaporization degree (V 10w )(%); and 97% refers to the cumulative amount of carbon dioxide (CO2) generated by a composition composed of 100 wt% of a vaporization accelerator for PBS-based resin (composition containing only a vaporization accelerator for PBS-based resin) at 30°C for 12 weeks according to ISO 14855, and the vaporization degree (V 10w )(% ).
[0066] The improvement of vaporization promotion (ΔVID 10W ) is the vaporization degree of the composition actually measured (V 10w ) minus the theoretical vaporization degree of the composition (V THV10w ) and the value obtained (V 10w –V THV10w ), which can be used as an indicator of the degree to which the vaporization promoter used for PBS-based resin promotes the vaporization of PBS-based resin.
[0067] The improvement of vaporization promotion (ΔVID 10W) may be, for example, 0.2% or more, 0.3% or more, 0.5% or more, 0.6% or more, 0.7% or more, 0.8% or more, 1% or more, 2% or more, 3% or more, 5% or more, 10% or more, 12% or more, 13% or more, 15% or more, 20% or more, 22% or more, 23% or more, 24% or more, 25% or more, 30% or more, 33% or more, or 35% or more. In addition, the degree of improvement in vaporization promotion (ΔVID 10W ) can be, for example, 50% or less, 48% or less, 46% or less, 45% or less, 43% or less, 40% or less, or 38% or less.
[0068] The improvement degree of vaporization promotion (ΔVID 10W ) may vary according to the content or physical properties of the PBS-based resin contained in the composition, or may vary according to the content, component or physical properties of the vaporization accelerator for the PBS-based resin contained in the composition.
[0069] Meanwhile, in Formula 3, the theoretical vaporization degree (V THV10w ) may vary depending on the content (weight) of the PBS-based resin and the vaporization promoter for the PBS-based resin contained in the composition. Specifically, the theoretical vaporization degree (V THV10w ) can be, for example, 1% or more, 2% or more, 3% or more, 5% or more, 6% or more, 7% or more, 8% or more, 10% or more, 15% or more, or 20% or more, as well as 90% or less, 80% or less, 70% or less, 65% or less, 55% or less, 45% or less, 40% or less, or 35% or less.
[0070] When the composition according to an embodiment of the present invention is compared with cellulose (a representative standard biodegradable material), in terms of vaporization degree, it can have a vaporization degree (V) equivalent to or higher than that of cellulose. 10w ).
[0071] Specifically, the composition according to an embodiment of the present invention includes a PBS-based resin having a low vaporization degree at room temperature of 30° C., wherein the vaporization degree (V 10w ) is at a certain level or higher (e.g., 20% or higher), thereby producing an excellent biodegradation effect at room temperature.
[0072] Therefore, the composition according to an embodiment of the present invention can be used in various fields to effectively protect the environment, and has excellent physical properties.
[0073] Hereinafter, each component of the composition according to an embodiment of the present invention will be described in detail.
[0074] Polybutylene succinate (PBS) based resin
[0075] The composition according to an embodiment of the present invention may include a PBS-based resin.
[0076] The PBS-based resin is a representative polycondensation aliphatic polyester or aliphatic-aromatic polyester, and is a heat-resistant polymer having a relatively higher melting point than other polyesters synthesized from diols and dibasic acids.
[0077] Specifically, the PBS-based resin may be synthesized through an esterification reaction of 1,4-butanediol (1,4-BDO) and succinic acid and an ester exchange reaction (polycondensation reaction) of an oligomer obtained by the esterification reaction.
[0078] The PBS-based resin may include at least one selected from the group consisting of polybutylene succinate (PBS), i.e., a binary copolymer of 1,4-butanediol (1,4-BDO) and succinic acid; polybutylene succinate adipate (PBSA), i.e., a terpolymer of 1,4-butanediol (1,4-BDO), succinic acid and adipic acid; and polybutylene succinate terephthalate (PBST), i.e., a tetrapolymer of 1,4-butanediol (1,4-BDO), succinic acid, adipic acid and terephthalic acid or dimethyl terephthalate.
[0079] The weight average molecular weight (Mw) of the PBS-based resin can be about 100,000 to 500,000 g / mole, about 120,000 to 500,000 g / mole, about 150,000 to 450,000 g / mole, about 150,000 to 430,000 g / mole, or about 150,000 to 400,000 g / mole. The weight average molecular weight (Mw) can be measured by gel permeation chromatography (GPC).
[0080] The composition according to an embodiment of the present invention may include the PBS-based resin in an amount of 10 wt % to less than 100 wt %, based on the total weight of the composition.
[0081] Specifically, based on the gross weight of the composition, the composition may include the PBS-based resin in an amount of 10 wt % or more, 20 wt % or more, 30 wt % or more, 40 wt % or more, 50 wt % or more, 60 wt % or more, 70 wt % or more, 80 wt % or more, or 90 wt % or more, and less than 100 wt %, 98 wt % or less, 95 wt % or less, 93 wt % or less, 92 wt % or less, or 90 wt % or less. For example, based on the gross weight of the composition, the composition may include the PBS-based resin in an amount of 10 wt % to 99 wt %, 20 wt % to 97 wt %, 30 wt % to 95 wt %, 40 wt % to 93 wt %, 50 wt % to 92 wt %, 60 wt % to 91 wt %, or 70 wt % to 90 wt %.
[0082] When the cumulative amount of carbon dioxide (CO2) generated by a composition composed of 100 wt% of a PBS-based resin at 30°C for 12 weeks is measured according to ISO 14855, the vaporization degree (V 10w ) may be significantly lower.
[0083] Therefore, the composition according to an embodiment of the present invention further includes the vaporization accelerator for the PBS-based resin described below, thereby accelerating the vaporization of the PBS-based resin having a low vaporization degree at room temperature, resulting in a further enhanced biodegradation effect.
[0084] Vaporization accelerator for polybutylene succinate (PBS) based resins
[0085] The composition according to an embodiment of the present invention may further include a vaporization accelerator for the PBS-based resin.
[0086] The vaporization accelerator for PBS-based resin may be used as an accelerator capable of accelerating the vaporization of a PBS-based resin having a low vaporization degree at a room temperature of 30°C.
[0087] Based on the gross weight of the composition, the composition according to the embodiment of the present invention can include the following amount of vaporization promoter for PBS-based resin: greater than 0 wt %, 1 wt % or more, 2 wt % or more, 3 wt % or more, 4 wt % or more, 5 wt % or more, 10 wt % or more, 20 wt % or more, or 30 wt % or more, and less than 100 wt %, 90 wt % or less, 80 wt % or less, 70 wt % or less, 60 wt % or less, 50 wt % or less, 40 wt % or less, or 30 wt % or less. For example, based on the gross weight of the composition, the composition can include 1 wt % to 90 wt %, 3 wt % to 80 wt %, 5 wt % to 70 wt %, 7 wt % to 60 wt %, 8 wt % to 50 wt %, 9 wt % to 40 wt %, or 10 wt % to 30 wt % of the amount of vaporization promoter for PBS-based resin.
[0088] When the content of the vaporization accelerator for the PBS-based resin satisfies the above range, the vaporization of the PBS-based resin is effectively accelerated, so that the composition according to an embodiment of the present invention can produce an excellent biodegradation effect at a room temperature of 30° C., even if the composition contains the PBS-based resin in an amount of 10 wt % or more, 20 wt % or more, 40 wt % or more, 60 wt % or more, 70 wt % or more, 80 wt % or more, or 90 wt % or more.
[0089] The vaporization promoter for PBS-based resin may include polyhydroxyalkanoate (hereinafter referred to as "PHA") resin. Since PHA resin has specific physical properties (e.g., specific crystal structure, components derived from specific monomers, etc.), it can effectively promote the vaporization of PBS-based resin.
[0090] PHA resin has similar physical properties to synthetic resins such as polybutylene succinate (PBS), polybutylene succinate terephthalate (PBST), and polybutylene succinate adipate (PBSA), while exhibiting complete biodegradability and excellent biocompatibility.
[0091] Specifically, PHA resin is a natural thermoplastic polyester polymer that can accumulate in microbial cells. Because it is biodegradable, it can be composted and eventually decomposed into carbon dioxide, water and organic waste without producing toxic waste. In particular, PHA resin is biodegradable in soil and ocean. Therefore, when the composition according to an embodiment of the present invention includes PHA resin, it is biodegradable under any environmental conditions such as soil and ocean, and is environmentally friendly.
[0092] For example, when the cumulative amount of carbon dioxide (CO2) generated by a composition composed of 100 wt% of a PHA resin at 30°C for 12 weeks is measured according to ISO 14855, the vaporization degree (V 10w ) can be, for example, 90% or more, 91% or more, 91.5% or more, 92% or more, 93.5% or more, 95% or more, or 97% or more, thereby producing a significantly excellent biodegradation effect at room temperature.
[0093] PHA resins can be formed by enzyme-catalyzed polymerization of one or more monomers in living cells.
[0094] Specifically, the PHA resin may be a copolymerized polyhydroxyalkanoate resin (hereinafter referred to as a "PHA copolymer"), and more specifically, may be a copolymer in which repeating units derived from two or more different monomers are randomly distributed in the polymer chain. In addition, the PHA resin may contain isomers. For example, the PHA resin may contain structural isomers, enantiomers, or geometric isomers. Specifically, the PHA resin may contain structural isomers.
[0095] Examples of monomers that can be used to prepare PHA specifically include: 2-hydroxybutyrate, lactic acid, glycolic acid, 3-hydroxybutyrate (hereinafter referred to as "3-HB"), 3-hydroxypropionate (hereinafter referred to as "3-HP"), 3-hydroxyvalerate (hereinafter referred to as "3-HV"), 3-hydroxyhexanoate (hereinafter referred to as "3-HH"), 3-hydroxyheptanoate (hereinafter referred to as "3-HHep"), 3-hydroxyoctanoate (hereinafter referred to as "3-HO"), 3-hydroxynonanoate (hereinafter referred to as "3-HN"), 3-hydroxydecanoate (hereinafter referred to as "3-HD"), 3-hydroxydodecanoate (hereinafter referred to as "3-HDd"), 4-hydroxybutyrate (hereinafter referred to as "4-HB"), 4-hydroxyvalerate (hereinafter referred to as "4-HV"), 5-hydroxyvalerate (hereinafter referred to as "5-HV"), and 6-hydroxyhexanoate (hereinafter referred to as "6-HH"). The PHA resin may comprise repeating units derived from one or more monomers selected from the above.
[0096] Specifically, the PHA resin may include a repeating unit (at least one repeating unit) derived from one or more monomers selected from 3-HB, 4-HB, 3-HP, 3-HV, 3-HH, 4-HV, 5-HV, and 6-HH.
[0097] More specifically, the PHA resin may include repeating units derived from a 4-HB monomer. That is, the PHA resin may be a PHA copolymer including repeating units derived from a 4-HB monomer.
[0098] The PHA resin may be a PHA copolymer comprising repeating units derived from a 4-HB monomer and further comprising repeating units derived from a monomer different from the 4-HB monomer, or further comprising repeating units derived from two, three, four, five, six or more monomers different from each other (2 or more repeating units different from each other).
[0099] Specifically, the vaporization promoter for PBS-based resin according to an embodiment of the present invention may include a resin (PHA copolymer), which includes a repeating unit derived from a 4-HB monomer, and a repeating unit (at least one repeating unit) derived from at least one monomer selected from 3-HB monomer, 3-HP monomer, 3-HV monomer, 3-HH monomer, 4-HV monomer, 5-HV monomer and 6-HH monomer. More specifically, the vaporization promoter for PBS-based resin may include a resin (PHA copolymer), which includes a repeating unit derived from a 3-HB monomer (hereinafter referred to as "3-HB repeating unit") and a repeating unit derived from a 4-HB monomer (hereinafter referred to as "4-HB repeating unit"). For example, it may include a poly-3-hydroxybutyrate-to-4-hydroxybutyrate (hereinafter referred to as "P3-HB-to-4-HB") copolymer.
[0100] According to an embodiment of the present invention, in order to promote vaporization of a PBS-based resin while increasing biodegradability of the composition in soil and ocean, it is important to control the content ratio of 3-HB repeating units and 4-HB repeating units contained in the PHA resin.
[0101] For example, in the PHA resin comprising 3-HB repeating units and 4-HB repeating units, the molar ratio of 3-HB repeating units to 4-HB repeating units may be 20:80 to 99:1, 30:70 to 99:1, 40:60 to 99:1, 50:50 to 95:5, 50:50 to 94:6, 50:50 to 92:8, 55:45 to 92:8, or 55:45 to 90: 10. When the molar ratio of 3-HB repeating units to 4-HB repeating units meets the above range, it may be more conducive to achieving the desired biodegradation effect of the present invention.
[0102] Specifically, based on the total mole (number of moles) of 3-HB repeating units and 4-HB repeating units, the content of 4-HB repeating units may be 1 mol% to 80 mol%, 2 mol% to 70 mol%, 3 mol% to 60 mol%, 5 mol% to 50 mol%, 8 mol% to 45 mol%, or 10 mol% to 45 mol%. In addition, based on the total weight of 3-HB repeating units and 4-HB repeating units, the content of 4-HB repeating units may be 1 wt% to 80 wt%, 2 wt% to 70 wt%, 3 wt% to 60 wt%, 5 wt% to 50 wt%, 8 wt% to 45 wt%, or 10 wt% to 45 wt%.
[0103] In addition, in a PHA resin comprising at least one 4-HB repeating unit, the crystallinity of the PHA resin can be adjusted according to the content of the 4-HB repeating unit. That is, the PHA resin can be a PHA copolymer with controlled crystallinity. Specifically, according to the content of the 4-HB repeating unit, the PHA resin can be divided into a semi-crystalline PHA (scPHA) copolymer or an amorphous PHA (aPHA) copolymer.
[0104] The PHA resin with regulated crystallinity may be a PHA resin whose crystallinity and amorphism are regulated as the irregularity in its molecular structure increases. Specifically, the crystallinity and amorphism may be determined by the type of monomer, the ratio of repeating units derived from the monomer, or the type and / or content of isomers.
[0105] Specifically, the PHA resin may be an amorphous PHA (aPHA) copolymer including a 4-HB repeating unit. Since the vaporization accelerator of the PBS-based resin includes such an amorphous PHA (aPHA) copolymer, the vaporization of the PBS-based resin may be more effectively promoted.
[0106] Meanwhile, the glass transition temperature (Tg) of the PHA resin may be, for example, -45°C to 80°C, -35°C to 80°C, -30°C to 80°C, -25°C to 75°C, -20°C to 70°C, -35°C to 5°C, -25°C to 5°C, -35°C to 0°C, -25°C to 0°C, -30°C to -10°C, -35°C to -15°C, -35°C to -20°C, -20°C to 0°C, -15°C to 0°C, or -15°C to -5°C.
[0107] The crystallization temperature (Tc) of the PHA resin may not be measured, or may be, for example, 60 to 120°C, 70 to 120°C, 75 to 120°C, 75 to 115°C, 75 to 110°C, or 90 to 110°C.
[0108] The melting temperature (Tm) of the PHA resin may not be measured, or may be, for example, 100 to 170°C, 105 to 160°C, 110 to 150°C, 115 to 155°C, or 120 to 140°C.
[0109] The weight average molecular weight (Mw) of the PHA resin may be, for example, 10,000 g / mol to 1,200,000 g / mol. Specifically, the weight average molecular weight of the PHA resin may be 50,000 g / mol to 1,200,000 g / mol, 100,000 g / mol to 1,200,000 g / mol, 50,000 g / mol to 1,000,000 g / mol, 100,000 g / mol to 1,000,000 g / mol, 200,000 g / mol to 1,200,000 g / mol, 250,000 g / mol to 1,150,000 g / mol, 300,000 g / mol to 1,100,000 g / mol, 350,000 g / mol to 1,000,000 g / mol, 350,000 g / mol to 950,000 g / mol, 100,000 g / mol to 900,000 g / mol, 200,000 g / mol to 800,000 g / mol, 200,000 g / mol to 700,000 g / mol, 250,000 g / mol to 650,000 g / mol, 200,000 g / mol to 400,000 g / mol, 300,000 g / mol to 800,000 g / mol, 300,000 g / mol to 600, In some embodiments, the present invention relates to an aqueous solution of at least one iodine-containing compound and an aqueous solution of at least one iodine-containing compound. The aqueous solution of at least one iodine-containing compound can be substituted with at least one iodine-containing compound.
[0110] Meanwhile, the composition according to an embodiment of the present invention may include a PBS-based resin and a vaporization promoter for the PBS-based resin at a specific content ratio. Specifically, the content ratio (weight ratio) of the PBS-based resin and the vaporization promoter for the PBS-based resin may be, for example, 10:90 to 99:1, 20:80 to 98:2, 30:70 to 95:5, 45:55 to 94:6, 50:50 to 93:7, 55:45 to 90:10, 60:40 to 90:10, 65:35 to 90:10 or 70:30 to 90:10. When the content ratio (weight ratio) of the PBS-based resin and the vaporization promoter for the PBS-based resin satisfies the above range, the vaporization of the PBS-based resin may be significantly accelerated.
[0111] additive
[0112] The composition according to an embodiment of the present invention may further include at least one additive selected from the group consisting of an antioxidant, a compatibilizer, a weighting agent, a nucleating agent, a melt strength enhancer, and a slip agent.
[0113] The content of the additive can be adjusted according to the desired effect and purpose of the composition. Based on the gross weight of the composition, the content of the additive can be 0.1 wt % or more, 0.5 wt % or more, 1 wt % or more, 1.5 wt % or more, or 2 wt % or more, and 30 wt % or less, 28 wt % or less, 25 wt % or less, 20 wt % or less, 15 wt % or less, 10 wt % or less, 8 wt % or less, or 5 wt % or less.
[0114] The additives may be publicly known additives depending on the desired effects and uses.
[0115] Mode for Carrying Out the Invention
[0116] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, the following examples are intended to illustrate the present invention, and the scope of the examples is not limited thereto.
[0117] <Example>
[0118] Example 1
[0119] As shown in Table 1 below, PBS resin (MITSUBISHI, BioPBS TM ) and a polyhydroxyalkanoate (PHA) resin (P3-HB-co-4-HB, aPHA) (CJ Cheil Jedang, Korea) as a vaporization accelerator for a PBS-based resin were mixed in a weight ratio of 70:30 to prepare a composition.
[0120] Example 2
[0121] As shown in Table 1 below, PBS resin (MITSUBISHI, BioPBS TM ) and a polyhydroxyalkanoate (PHA) resin (P3-HB-co-4-HB, aPHA) (CJ Cheil Jedang, Korea) as a vaporization accelerator for a PBS-based resin were mixed in a weight ratio of 80:20 to prepare a composition.
[0122] Example 3
[0123] As shown in Table 1 below, PBS resin (MITSUBISHI, BioPBS TM) and a polyhydroxyalkanoate (PHA) resin (P3-HB-co-4-HB, aPHA) (CJ Cheil Jedang, Korea) as a vaporization accelerator for a PBS-based resin were mixed in a weight ratio of 90:10 to prepare a composition.
[0124] Comparative Example 1
[0125] As shown in Table 1 below, 100 wt% of PBS resin (MITSUBISHI, BioPBS) was prepared. TM ) composition.
[0126] Comparative Example 2
[0127] As shown in Table 1 below, a composition consisting of 100 wt % of a polyhydroxyalkanoate (PHA) resin (P3-HB-co-4-HB, scPHA) (CJ, Korea) as a vaporization accelerator for a PBS-based resin was prepared.
[0128] Comparative Example 3
[0129] As shown in Table 1 below, poly(butylene adipate terephthalate) (PBAT) resin and polyhydroxyalkanoate (PHA) resin (P3-HB-co-4-HB, aPHA) (CJ, Korea) as a vaporization accelerator for the PBAT resin were mixed in a weight ratio of 70:30 to prepare a composition.
[0130] The contents and physical properties of the compositions obtained in Examples and Comparative Examples are summarized in Table 1 below.
[0131] [Table 1]
[0132]
[0133]
[0134] Evaluation Example
[0135] Evaluation Example 1: Vaporization Degree
[0136] According to ISO 14855, the cumulative amount of carbon dioxide produced under aerobic composting conditions is measured to calculate the degree of vaporization (V 10w ).
[0137] Specifically, as an evaluation group, each composition sample in the embodiment and the comparative example was sampled at 14.3% by weight based on the total dry weight of the composition sample and the compost, and a test container was prepared, wherein the test container contained a mixture obtained by mixing the composition sample with the compost (Abnexo Co., Ltd.). In this case, the initial moisture content of the compost was measured by LOD moisture measurement using an HMA or a drying oven. Additional moisture was added to adjust the final moisture content to 50% to adjust the dry weight. In addition, a mixture was prepared by the following method: 20 grams of dried composition samples (0% moisture content) were uniformly mixed with 240 grams of compost (dry weight: 120 grams) having a moisture content of 50%, thereby adjusting the ratio of the sample to the compost to 1:6 according to the ISO 14855 notification.
[0138] In addition, as a control group, an inoculation container containing only compost without containing the composition sample was prepared.
[0139] Thereafter, after 12 weeks at 30°C under normal pressure and aerobic conditions, the carbon dioxide produced in each container was collected using ECHO's permeameter device and titrated with an NIR (near infrared sensor) through a system within the device to measure the cumulative amount of carbon dioxide produced in each container.
[0140] The measured cumulative amount of generated carbon dioxide is used to calculate the vaporization degree (V 10w ):
[0141] [Formula 1]
[0142]
[0143] In formula 1, (CO2) S is the cumulative amount of carbon dioxide (CO2) produced in the test container containing the compost and the sample (in grams), based on the total dry weight of the sample and compost, the amount of the sample being 14.3% by weight; (CO2) B is the cumulative amount of carbon dioxide (CO2) (grams) produced in the inoculated container containing only compost, (CO2) THV is the theoretical cumulative amount of carbon dioxide (CO2) produced in the test container and is expressed by the following formula 2,
[0144] [Formula 2]
[0145]
[0146] In Formula 2, Cw is the mass (g) of organic carbon contained in the sample. Specifically, Cw is the content (g) of carbon element contained in the sample.
[0147] Evaluation Example 2: Improvement of Vaporization Promotion
[0148] In order to measure the degree of improvement of vaporization promotion of PBS-based resin by vaporization promoter, the degree of improvement of vaporization promotion (ΔVID 10W ).
[0149] Specifically, the degree of vaporization (V 10w ) and the theoretical vaporization degree (V THV10w ), the improvement degree of vaporization promotion (ΔVID 10W ). Theoretical vaporization degree (V THV10w ) is calculated by the following formula 4:
[0150] [Formula 3]
[0151] ΔVID 10W (%) = V 10w –V THV10w
[0152] In Formula 3, V 10w As defined in Evaluation Example 1, V THV10w It is represented by the following formula 4:
[0153] [Formula 4]
[0154]
[0155] In Formula 4, x is the weight percentage of the PBS-based resin included in the composition, based on the total weight of the composition.
[0156] Meanwhile, when the improvement degree of vaporization promotion (ΔVID 10W ), x in Formula 4 is the weight percentage of the PBAT resin contained in the composition based on the total weight of the composition.
[0157] [Table 2]
[0158]
[0159] [Table 3]
[0160]
[0161]
[0162] Referring to Table 3 above, when the cumulative amount of carbon dioxide (CO2) generated at 30°C for 12 weeks was measured, the vaporization degrees (V 10w) were 20% or more. In particular, in Examples 1 to 3 (wherein a composition comprising a PBS-based resin and a vaporization accelerator for a PBS-based resin was used), the vaporization degree (V 10w ), the improvement degree of vaporization promotion (ΔVID 10W ) significantly increased to 30% or more.
[0163] Meanwhile, in Comparative Example 3 (in which the PHA resin of the vaporization accelerator for PBS-based resin according to the present invention is used together with the PBAT resin), the degree of improvement in vaporization promotion (ΔVID 10W ) is a negative value, indicating that the PHA resin specifically promotes the vaporization of the PBS-based resin.
Claims
1. A composition comprising a polybutylene succinate (PBS) based resin in an amount of 10 wt % to less than 100 wt % based on the total weight of the composition, wherein: When the cumulative amount of carbon dioxide (CO2) generated at 30°C for 12 weeks is measured according to ISO 14855, the vaporization degree (V 10w ) is 20% or more: [Formula 1] In formula 1, (CO2) S is the cumulative amount of carbon dioxide (CO2) produced in the test container containing the compost and the sample (in grams), and the amount of the sample is 14.3% by weight based on the total dry weight of the sample and the compost, (CO2) B is the cumulative amount of carbon dioxide (CO2) produced in the inoculated container containing only compost (in grams), and (CO2) THV is the theoretical cumulative amount of carbon dioxide (CO2) produced in the test container and is expressed by the following formula 2, [Formula 2] In Formula 2, Cw is the mass (gram) of organic carbon contained in the sample.
2. The composition according to claim 1, further comprising a vaporization accelerator for the polybutylene succinate (PBS) based resin.
3. The composition according to claim 2, wherein The weight ratio of the polybutylene succinate (PBS)-based resin to the vaporization accelerator for the polybutylene succinate (PBS)-based resin is 10:90 to 90:
10.
4. The composition according to claim 2, wherein The improvement of vaporization promotion (ΔVID 10W ) is 0.1% or more, as shown in Formula 3 below: [Formula 3] ΔVID 10W (%)=V 10w –V THV10w In Formula 3, V 10w As defined in claim 1, V THV10w It is represented by the following formula 4: [Formula 4] In Formula 4, x is the weight percentage of the polybutylene succinate (PBS)-based resin included in the composition, based on the total weight of the composition.
5. The composition according to claim 2, wherein The vaporization accelerator for polybutylene succinate (PBS)-based resin satisfies at least one of the following characteristics: Glass transition temperature (Tg) from -45°C to 80°C, a crystallization temperature (Tc) of 60°C to 120°C, and Melting temperature (Tm) from 100°C to 170°C.
6. The composition according to claim 2, wherein The polybutylene succinate (PBS)-based resin comprises at least one selected from the group consisting of polybutylene succinate (PBS), polybutylene succinate adipate (PBSA) and polybutylene succinate terephthalate (PBST), and The vaporization accelerator for a polybutylene succinate (PBS)-based resin comprises a resin containing repeating units derived from a 4-hydroxybutyrate (4-HB) monomer and repeating units derived from at least one monomer selected from the group consisting of 3-hydroxybutyrate (3-HB), 3-hydroxypropionate (3-HP), 3-hydroxyvalerate (3-HV), 3-hydroxyhexanoate (3-HH), 4-hydroxyvalerate (4-HV), 5-hydroxyvalerate (5-HV) and 6-hydroxyhexanoate (6-HH).
7. The composition according to claim 6, wherein The vaporization accelerator for a polybutylene succinate (PBS)-based resin includes a resin containing a repeating unit derived from a 3-hydroxybutyrate (3-HB) monomer and a repeating unit derived from a 4-hydroxybutyrate (4-HB) monomer.
8. The composition according to claim 7, wherein The resin includes the repeating unit derived from the 4-hydroxybutyrate (4-HB) monomer in an amount of 1 mol % to 80 mol % based on the total moles of the repeating unit derived from the 3-hydroxybutyrate (3-HB) monomer and the repeating unit derived from the 4-hydroxybutyrate (4-HB) monomer.
9. A vaporization accelerator for a polybutylene succinate (PBS)-based resin, comprising a resin containing a repeating unit derived from a 3-hydroxybutyrate (3-HB) monomer and a repeating unit derived from a 4-hydroxybutyrate (4-HB) monomer.