Method for producing a covering on an object and coated body produced therefrom

By using sulfur-containing gas and adjusting the precursor ratio in the CVD method, a stable cubic Al1-xTixN cover layer was solved, and the problem that the AlTiN cover layer in the prior art was difficult to maintain high aluminum content and cubic structure at low temperatures was improved. The wear resistance and oxidation resistance of the tool extend the service life.

CN119072558APending Publication Date: 2024-12-03BOEHLERIT GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380019815.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-01-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When the existing CVD method produces AlTiN cover layer, it is difficult to maintain high aluminum content and cubic structure at low temperatures, resulting in insufficient wear resistance and oxidation resistance. At the same time, the growth rate of the phase gradient layer is fast, resulting in an increase in thickness in the coating process. and cooling issues affect the service life of the tool.

Method used

Introduce sulfur-containing gases, especially hydrogen sulfide, adjust the precursor ratio of titanium and aluminum, control the temperature and gas flow rate to form a stable cubic Al1-xTixN covering layer, ensuring high aluminum content and alternating sheet structure, The TiCN or oxide layer is further deposited to improve toughness and wear resistance.

Benefits of technology

A stable cubic Al1-xTixN cover layer with high aluminum content is achieved under low temperature conditions, which improves the wear resistance and oxidation resistance of the tool, extends the service life, and optimizes the coating process, reducing thickness increase and cooling time .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072558A_ABST
    Figure CN119072558A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a cover on an object, in particular a cutting insert, such as a cutting board for a machining process, in which a cover having one or more cover layers is applied to the object, in which at least one Al1-xTixN cover layer is deposited by means of a CVD method, in which the nitrogen in the Al1-xTixN cover layer can be partially replaced. In order to obtain a cover layer having the highest possible proportion of cubic phase, it is provided according to the invention that the Al1-xTixN cover layer is deposited in the presence of a sulfur-containing gas. The invention also relates to a correspondingly produced coated body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing a covering on an object, in particular a cutting insert, such as a cutting plate for machining processes, wherein a covering having one or more covering layers is applied to the object, wherein at least one Al 1-x Ti x The N capping layer was deposited using CVD, where Al 1-x Ti x The nitrogen in the N capping layer may be partially substituted.

[0002] The present invention also relates to a coated body. Background Art

[0003] It is known from the prior art that cutting tools or cutting inserts are coated with a covering layer consisting of titanium, aluminum and nitrogen to increase the service life in cutting applications. In this regard, regardless of whether one or more phases are present in the covering layer, a TiAlN covering layer is generally referred to, wherein the average chemical composition consists of Ti:AlN. 1-x Al x N (where x>0). For overlays containing more aluminum than titanium, the designation AlTiN or more precisely Al x Ti 1-x N is universal (where x>0.50).

[0004] From WO 03 / 085152 A2 it is known to produce a single-phase covering layer with a cubic structure in the AlTiN system, wherein at a relative aluminum nitride (AlN) content of up to 67 mole percent (mol%), a cubic structure of the AlTiN is obtained. At a higher AlN content of up to 75 mol%, a mixture of cubic AlTiN and hexagonal AlN is produced, and at an AlN content of more than 75 mol%, only hexagonal AlN and cubic titanium nitride (TiN) are produced. According to the cited document, the AlTiN covering layer described is deposited by means of physical vapor deposition (PVD). With the PVD method, the maximum relative AlN content is thus in fact limited to 67 mol%, since otherwise it is possible to convert into a phase containing only aluminum in the form of hexagonal AlN. However, according to expert opinion, in order to maximize the wear resistance to the greatest possible extent, a higher relative content of AlN in the cubic phase is desirable.

[0005] Therefore, historically attempts have been made to overcome these disadvantages of the PVD method, and it is also known from the prior art to use chemical vapor deposition (CVD) methods instead of PVD methods, wherein the CVD method is carried out at relatively low temperatures, within a temperature window of 700° C. to 900° C., since cubic AlTiN covering layers cannot be produced at temperatures of, for example, ≥1000° C. due to the metastable structure of this type of covering layer.

[0006] If necessary, according to US Pat. No. 6,238,739 B1, the temperature can be even lower, ie within the temperature window of 550° C. to 650° C., but a high chlorine content in the cover layer must be accepted, which proves to be disadvantageous for the application case.

[0007] Therefore, attempts have been made to optimize the CVD method so that AlTiN covering layers with a high aluminum content and a cubic structure of the covering layer can be produced by the method (I. Endler et al., Proceedings Euro PM 2006, Ghent, Belgium, October 23-25, 2006, Vol. 1, 219). Although these covering layers have high microhardness and therefore fundamentally favorable properties for high wear resistance during use, it has been shown that the bonding strength of this type of covering layer may be too low. Therefore, in view of this, it is proposed in DE 10 2007 000 512 B3 that a 1 μm thick covering layer formed as a phase gradient layer and consisting of a phase mixture of hexagonal AlN, TiN and cubic AlTiN is provided below a 3 μm thick cubic AlTiN covering layer, wherein the cubic AlTiN content has an increasing proportion with the outward cubic AlTiN covering layer or towards the (exclusively) cubic AlTiN covering layer. Cutting plates coated in this way were used for milling steel, but only a slight improvement in wear resistance was achieved compared with covering layers produced by means of PVD methods.

[0008] In addition to the only slight improvement in wear resistance, a further disadvantage of the bonding layer according to DE 10 2007 000 512 B3 is that the bonding layer or phase gradient layer grows extremely fast even in laboratory-scale experiments (I. Endler et al., Proceedings Euro PM 2006, Ghent, Belgium, October 23-25, 2006, Vol. 1, 219). In the case of production in larger reactors designed for industrial cutting board coverings, since the temperature for forming the final desired cubic AlTiN covering layer must be lowered, it takes a lot of time, which leads to the bonding layer or phase gradient layer becoming extremely thick in the provided coating process.

[0009] However, during this reduction in process temperature, the thickness of the bonding layer or phase gradient layer increases rapidly, since rapid cooling is not possible in industrial reactors. It is conceivable to interrupt the coating process for a longer period or interrupt cooling, but this is not cost-effective. Therefore, the phase gradient layer not only leads to additional efforts for a slight increase in performance, but is also difficult to handle.

[0010] In the production of AlTiN covering layers by means of CVD and their optimization, the initial starting point was to achieve a wear-resistant and oxidation-resistant and therefore optimal covering layer if the aluminum content in the covering layer was as high as possible and the covering layer had as complete a cubic structure as possible.

[0011] In this regard, the formation of AlTiN covering layers is known from WO 2012 / 126030 A1, wherein the AlTiN covering layer can be formed mainly with a cubic structure. However, additional phases, such as hexagonal AlN, may also be present in the AlTiN covering layer. Interestingly enough, it has been shown that a lamellar structure may also be present within the corresponding AlTiN covering layer. Compared with conventional PVD-coated cutting tools, cutting plates coated with this type of AlTiN covering layer can lead to a significant increase in service life.

[0012] In further studies, according to WO 2013 / 134796 A1, it was possible to produce an AlTiN covering layer at least partially formed with a lamellar structure within the AlTiN covering layer, wherein it has been shown that the lamellar layers consist of alternating regions of different compositions, wherein the hexagonal high-aluminum phase is arranged so as to alternate with the cubic high-titanium phase in sections. Surprisingly, even in the presence of hexagonal aluminum nitride, it was found that it was possible to obtain excellent results in terms of milling service life using corresponding coated cutting tools. This can be attributed to the special lamellar formation, in which the inherently softer hexagonal aluminum nitride is apparently not particularly disadvantageous.

[0013] In further research and possible improvement of this AlTiN cover or more precisely Al 1-x Ti xIn an attempt to further understand the mechanism behind this, according to WO 2016 / 112417A1, it was found that under predetermined reaction conditions in terms of temperature, pressure, gas composition and gas flow rate, by targeted changes in the ratio of titanium and aluminum precursors, it is possible to adjust the formation sequence of lamellae with alternating layers of higher aluminum content and higher titanium content in a targeted manner. According to WO 2016 / 112417A1, for very high aluminum contents, it is possible to obtain structures with alternating hexagonal and cubic fragments at higher aluminum contents, while for lower aluminum contents, it is possible to obtain structures in which the individual fragments each have a cubic structure. Subsequently, the corresponding mechanism was elucidated in several scientific publications (A. etal.,Nanostructured coatings for tooling applications,Mat.Sci.Forum,Vols.825-826(2015)599;A. et al., Nanostructured coatings for tooling applications, Int. Journal of Refractory Metals and Hard Materials, 62, (2017) 219).

[0014] Original in Al 1-x Ti x The N capping system works with the following objectives: In order to obtain high oxidation resistance while retaining the cubic structure as much as possible, 1-x Ti x As much aluminum as possible is deposited in the N capping layer. However, as has become apparent from the above-mentioned references, in the case of relatively high aluminum contents, the formation of a lamellar structure with alternating hexagonal high-aluminum segments on the one hand and cubic high-titanium segments on the other hand occurs. The corresponding structure is very suitable for processing, although it is desirable to be able to 1-x Ti x A stable single cubic structure in the N coating, i.e., alternating cubic segments with a higher aluminum content and cubic segments with a higher titanium content, or even those with a higher average aluminum content, may lead to an increase in the service life of the correspondingly coated tool (e.g., a cutting plate). Summary of the invention

[0015] This is solved by the present invention. The object of the present invention is to further develop a method of the type mentioned at the outset so that a coated object, in particular a cutting insert such as a cutting plate, can be provided which has an Al2O3 coating formed with high wear resistance. 1-x Tix N covering layer.

[0016] A further object is to provide a correspondingly produced body of the type mentioned at the outset.

[0017] If, in a method of the type mentioned at the outset, Al 1-x Ti x The objectives associated with the method are achieved if the N capping layer is deposited in the presence of a sulfur-containing gas.

[0018] It can be seen that one advantage obtained by using the method according to the invention is that a coated object, in particular a cutting element such as a cutting plate, or a different cutting element or tool, can be provided which has a high wear resistance during use, in particular during machining of a workpiece, such as during turning or milling. Surprisingly, it was found that the presence of sulfur-containing gases leads to Al 1-x Ti x The lamellar structure in the N capping layer is stabilized as a cubic structure, i.e. directly following the cubic fragments, but with a different chemical composition. This means that in the presence of a sulfur-containing gas during the deposition process or the CVD coating step, the corresponding cubic formation of the lamellar structure with a higher aluminum content can be stabilized. The exact mechanism is not yet clear. However, it is clear that, overall, more cubic phases are present, or that a shift towards higher aluminum contents (relative to Al) can be achieved with the use of sulfur-containing gases, compared to process management without sulfur-containing gases. 1-x Ti x The higher the aluminum content, the better the oxidation resistance and thus also the wear properties during machining operations in which high temperatures occur (for example turning or milling workpieces made of metal or alloys).

[0019] Sulfur is present in the correspondingly produced Al 1-x Ti x N capping layer. Al 1-x Ti x The N capping layer may be embodied so that the nitrogen may be partially substituted. Carbon and / or oxygen may in particular be used for substitution. However, whatever the type of nitrogen substituent, it is preferred to provide that no more than 10% of the nitrogen atoms are replaced by carbon and / or oxygen. Sulfur may also be used as a nitrogen substituent, but it is also possible that, within the capping layer, for example, fine sulfides are deposited separately to facilitate the Al 1-x Ti x During the deposition of the N capping layer, a lamellar structure consisting of a single alternating cubic fragment or at least mainly alternating cubic fragments is formed.

[0020] In the process according to the invention, in principle, different sulfur-containing gases can be used, for example mercaptans, which decompose at process temperatures of generally more than 700° C. Another possible sulfur source is carbon disulfide. However, for the sake of simplifying process management, it is preferred to provide hydrogen sulfide as the sulfur-containing gas. Hydrogen sulfide is easy to handle and is already present in gaseous form; it can therefore be fed into the reaction zone without difficulty together with the other gases.

[0021] According to a preferred embodiment having alternating segments of respective cubic structures, it is advantageous to provide Al 1-x Ti x The N capping layer is deposited with a volume proportion of hexagonal aluminum nitride (AlN) of less than 20 volume percent (hereinafter referred to as: volume %), preferably less than 10 volume %, in particular less than 5 volume %. However, a specific proportion of hexagonal AlN can be provided, for example more than 1 volume %. Therefore, the hexagonal AlN can exist as a sheet (in which aluminum can be partially replaced by titanium) and / or as a separate hexagonal AlN.

[0022] Al 1-x Ti x It is advantageous for the N capping layer to be deposited as the outermost capping layer. The outermost capping layer is usually the working layer that comes into contact with the material to be processed (such as the casting material). 1-x Ti x The N coating is extremely wear-resistant and advantageously constitutes the outermost coating. However, it is possible to 1-x Ti x One or more additional covering layers are deposited on the N covering layer. For example, an oxide layer can be used for this purpose, or even a less wear-resistant covering layer, such as a cubic titanium nitride covering layer.

[0023] One or more capping layers are deposited on the Al 1-x Ti x N capping layers are advantageous, wherein preferably all capping layers are deposited using CVD methods. 1-x Ti x The one or more covering layers deposited below the N covering layer are used on the one hand for bonding to the substrate (usually cemented carbide, or possibly high-speed steel) and, if necessary, for further optimizing the overall covering layer in terms of wear resistance. Typically, a titanium nitride covering layer is used as a direct bonding layer on a substrate (e.g. a substrate made of cemented carbide). The bonding layer of titanium nitride usually has a thickness of no more than 2 microns and is deposited using a CVD method. The Al can then be provided directly 1-x Ti xIn some embodiments, the present invention provides a TiN covering layer, but at least one additional (intermediate) layer can also be provided. The intermediate layer can in particular be a titanium carbonitride (TiCN) covering layer. In particular, MT-TiCN known to the person skilled in the art can be used for this purpose. Therein MT stands for medium temperature, i.e. TiCN deposited at a relatively low temperature. In principle, a bonding layer of TiN is sufficient, so that it is possible to omit the intermediate layer, which enables a more efficient and material-saving production.

[0024] In this case, it is preferred that the TiCN covering layer is deposited at a temperature of 800° C. to 880° C. In principle, lower temperatures can also be selected for producing TiCN covering layers with elongated crystals, but in this case, for depositing TiCN with Al 1-x Ti x N covering layer needs to be heated again.

[0025] The optionally provided TiCN covering layer is advantageously deposited with a thickness of at most 7 μm, preferably 2 to 5 μm. The corresponding thickness is sufficient to give the covering layer as a whole the necessary toughness or to avoid potential tensile and / or compressive stresses to the greatest possible extent. x Ti 1-x The N covering layer has high hardness and thus relatively low toughness, so a certain toughness of the covering layer as a whole is also necessary.

[0026] The production of the TiCN covering layer can be carried out as is known per se from the prior art. In this respect, the TiCN covering layer can advantageously be deposited from a gas containing nitrogen, hydrogen, acetonitrile and titanium tetrachloride or consisting of nitrogen, hydrogen, acetonitrile and titanium tetrachloride. In order to control the thickness of this covering layer in a targeted manner at relatively high temperatures of 800° C. to 880° C. for the deposition of the TiCN covering layer, in contrast to the prior art, a gas having a higher nitrogen proportion than the hydrogen proportion can be used, so that the deposition rate can be kept low.

[0027] In this respect, it is advantageous if the nitrogen content is at least twice, preferably at least four times, and in particular six times, the hydrogen content. x Ti 1-x The TiCN covering layer is preferably deposited at a temperature equal to or lower than the deposition temperature of the TiCN covering layer. Therefore, the process for producing the covering layer can be designed efficiently in terms of temperature control. In this way, starting from the initial temperature, to a temperature that is continuously reduced during the production of the covering layer, it is possible to obtain a favorable covering layer in a short time. The TiCN covering layer thus formed has crystals that are elongated in cross section, and these crystals are preferably mainly dispersed in a direction that is at an angle of ±30° to the surface normal of the coated area. For the index a, the average composition TiCa N 1-a It has a range of 0.3 to 0.8, particularly 0.4 to 0.6.

[0028] In addition, it is also possible to deposit multiple Al 1-x Ti x N covering layers, which are separated by additional covering layers. This creates an alternating layer structure in which Al 1-x Ti x The N covering layer is arranged alternately with the additional covering layer. The additional covering layer can be embodied identically or differently when viewed individually. Advantageously, the alternating embodiments are designed with identical covering layers so that an abstract sequence of ABAB, etc. is given, where A represents Al. 1-x Ti x N represents a capping layer, and B represents an additional capping layer. The additional capping layer may be, for example, an oxide capping layer.

[0029] For this method, it is preferred to deposit Al from a first mixture of nitrogen, hydrogen, titanium tetrachloride, aluminum trichloride and hydrogen sulfide and a second mixture of nitrogen and ammonia. 1-x Ti x The two mixtures are fed separately into a reaction zone. In particular, the reaction zone may be the interior of a reactor (e.g. an industrial reactor). Reactors of this type for CVD processes are known to those skilled in the art and are used, for example, in It is sold under the trade name VIZOL®. When using titanium tetrachloride and aluminum trichloride on the one hand and ammonia on the other hand, it is advantageous to feed the reaction gases separately into the reaction zone of the reactor, because the reaction of the metal chlorides with ammonia takes place rapidly and because there is otherwise a risk of the feed lines becoming blocked. The hydrogen sulfide provided is therefore advantageously fed in along with the first mixture.

[0030] The reactor used can be embodied essentially as a vertical reactor in the form of a cylinder, in which the objects to be coated, in particular the cutting board, are arranged in a horizontal plane. So-called trays are used for this purpose. The cutting board can also be placed in a suspended manner in a plane transverse to the vertically extending longitudinal axis of the reactor. In a corresponding vertical embodiment of the reactor, the feed of the two gas mixtures can then be provided centrally, wherein the gas mixture enters the reaction zone of the reactor from the pipeline, roughly in the plane of the arranged objects to be coated. It is thus ensured that the reaction gases fed separately can first be mixed in the actual reaction zone of the reactor.

[0031] Preferably, Al 1-x Ti xThe N capping layer is deposited at a temperature of 800° C. to 850° C., preferably at a temperature of 810° C. to 830° C. This temperature range of deposition is very suitable for the production of the desired structure.

[0032] In the reaction zone or Al 1-x Ti x The pressure during the deposition of the N capping layer is advantageously set to 10 mbar to 80 mbar, in particular 15 mbar to 40 mbar.

[0033] Preferably, Al 1-x Ti x The N capping layer is at least partially produced with lamellae, wherein the lamellae preferably have an average size determined according to the Debye-Scherrer formula of less than 150 nm, preferably less than 100 nm, in particular less than 80 nm. 1-x Ti x The embodiment of the N covering layer is a particularly advantageous structure suitable for coating processing tools (such as cutting plates, etc.). Here, it can also be the case that the lamellar structure is only present in the region. However, if at least Al 1-x Ti x It is inherently advantageous that the major part of the N-covering layer, i.e. more than 50% by volume, is embodied with a preferred lamellar structure. A corresponding verification can be carried out without difficulty in cross section using imaging methods. Fundamentally, the finest possible formation of the lamellar structure is preferred.

[0034] For example, the lamellae may be embodied with a thickness of 15 nm to 75 nm, in particular approximately 20 nm to 65 nm.

[0035] In principle, any desired object can be made of Al 1-x Ti x N coating. However, in various applications, it is advantageous to directly or indirectly coat objects or bodies made of cemented carbide. In particular, cemented carbide has proven to be resistant for tools that are used in air at high temperatures and are therefore subject to oxidation stresses in addition to high temperatures. This is particularly true for tools used for turning, drilling and / or milling operations (e.g. cutting plates, etc.).

[0036] Although the method according to the invention is designed so that objects made of cemented carbide can be advantageously coated, other objects which, as mentioned above, are subject to abrasive, thermal and / or oxidative wear during use can also be coated. Forming tools, punching tools, rollers or other tools for forming work are mentioned here only as examples.

[0037] If Al 1-xTi x The inclusion of sulfur in the N coating results in a further object of the invention, a coated body of the type mentioned at the outset. Thus, the coated body can be produced in particular with the method according to the invention, or the method according to the invention can be used for this purpose.

[0038] The main body according to the invention has the following advantages in particular: 1-x Ti x The at least predominantly cubic structure in the N-coating layer is simultaneously embodied with a relatively high aluminum content. Thus, the corresponding coated body can be used particularly advantageously for operations or process steps involving high thermal and oxidation loads on the body (usually a tool such as a cutting plate or other cutting element).

[0039] Since the preferred embodiment has Al 1-x Ti x The at least predominant, preferably more than 70% by volume, in particular more than 85% by volume cubic structure of the N capping layer will generally also result in a small volume fraction of hexagonal AlN. Advantageously, a volume fraction of hexagonal AlN of less than 20% by volume, preferably less than 10% by volume, in particular less than 5% by volume is provided. The hexagonal AlN can thus be present both in a lamellar structure, as a fragment with hexagonal AlN (the fragment with hexagonal AlN includes or can include a partial substitution of aluminum by titanium), or as a separate AlN outside the lamellar structure, wherein in the latter case the aluminum can also be partially replaced by titanium.

[0040] Al 1-x Ti x The proportion of sulfur in the N cap layer is usually less than 5 atomic percent (hereinafter referred to as: atomic %), preferably less than 4 atomic %, and in particular less than 3 atomic %. Sulfide enters the Al layer through the production process. 1-x Ti x N capping layer, in particular using the method according to the invention, is provided in order to obtain Al 1-x Ti x Basically, it is not assumed that sulfur in Al 1-x Ti x The N capping layer itself has a functional purpose, but in the case of Al 1-x Ti xThe deposition process of the N capping layer previously had a functional purpose. Therefore, it seems advantageous that sulfur is present in the previous step of the deposition only in the necessary content in order to obtain the desired structure. Therefore, it is advantageous to keep the sulfur proportion as low as possible. However, the process management provided makes it possible to obtain a specific minimum content, which allows the formation of a lamellar structure with alternating cubic lamellar fragments of different compositions and up to an aluminum content higher than previously allowed.

[0041] Preferably Al is provided 1-x Ti x The N-covering layer at least partially embodies the region of the lamellae, wherein the lamellae preferably have an average size determined according to the Debye-Scherrer formula of less than 150 nm, preferably less than 100 nm, in particular less than 80 nm. As mentioned above, with regard to good performance in use, in particular for processing, the embodiment of the lamellae that is as thin as possible is advantageous.

[0042] In the corresponding coated body, relative to Al 1-x Ti x The average composition of the N capping layer is Al 1-x Ti x The proportion of N, aluminum may be relatively high, preferably in the range of X=0.85 to 0.99, preferably in the range of 0.885 to 0.975, in particular in the range of 0.89 to 0.95. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Additional features, advantages and effects of the present invention follow from the exemplary embodiments described below.

[0044] Figure 1 A schematic diagram showing a coated cut plate;

[0045] Figure 2 shows an image of a coated cemented carbide body taken using a scanning electron microscope;

[0046] Figure 3 shows additional images of the coated cemented carbide body taken using a scanning electron microscope;

[0047] Figure 4 The images of Al2O3 with different sulfur ratios taken using a scanning electron microscope are shown. 1-x Ti x Image of a cemented carbide body coated with an N overlay;

[0048] Figure 5 Show according to Figure 4 Visualization of the reflections in the X-ray diffraction pattern as a function of the H2S concentration during deposition of the capping layer and the associated domain size according to the Debye-Scherrer equation;

[0049] Figure 6 An X-ray diffraction pattern is shown;

[0050] Figure 7 Additional images taken using a scanning electron microscope are shown, with spectral positions marked;

[0051] Figure 8 Show about Figure 7 Plot of oxygen and sulfur contents at the spectral positions marked in . DETAILED DESCRIPTION

[0052] exist Figure 1 In the figure, a body 1 or an object is illustrated by way of example. The object is a cutting element, but it can also be a different body 1. The body 1, which is illustrated only in cross section, comprises a substrate 2. The substrate 2 is usually made of a cemented carbide. The cemented carbide can, for example, be a cemented carbide based on tungsten carbide as a hard material, wherein the tungsten carbide can be partially replaced by titanium carbide. In addition, a metal binder is provided, usually cobalt, but nickel and / or iron can also be provided, possibly in combination with one of the other metal binders (for example cobalt and iron) or all of these metals. Typically, the proportion of hard material (for example tungsten carbide) as described above is 85% to 95%. The remainder is essentially formed by the metal binder.

[0053] The substrate 2 is provided with a plurality of cover layers, wherein a first cover layer 3 is formed of titanium nitride (TiN). The TiN cover layer serves as a bonding layer. The bonding layer generally has a layer thickness of not more than 2 μm. An additional cover layer 4 of MT-TiCN is deposited on the TiN bonding layer. For example, this cover layer may have a thickness of 2 μm to 7 μm, but is only optional. Finally, a further additional cover layer 5 is deposited on the MT-TiCN cover layer. The additional cover layer 5 is formed of Al 1-x Ti x N cover layer formation. As illustrated, this additional cover layer 5 can constitute the outermost cover layer, which is however not mandatory. It is possible that, on this additional cover layer 5, at least one additional cover layer is deposited on the outside.

[0054] For Al 1-x Ti x The production of the N covering layer first provides a substrate 2, then deposits a TiN bonding layer, and then provides an additional covering layer 4 of MT-TiCN applied at a reduced temperature. Finally, the Al 1-x Ti xAll covering layers (even if other covering layers need to be provided) are deposited in a CVD process, which enables all covering layers to be formed in one reactor by simply lowering the temperature and switching the process gases.

[0055] In Al 1-x Ti x In the production of the N-coating, two reaction gases are fed separately into the reactor and allowed to react in the reaction zone. This can be achieved, for example, if a separate feed pipe with a corresponding outlet opens into the reactor. A first mixture of reaction gases consists of nitrogen, hydrogen, titanium tetrachloride, aluminum trichloride and hydrogen sulfide. The titanium tetrachloride is thus supplied based on liquid titanium tetrachloride. The aluminum trichloride is generated in situ by passing hydrochloric acid through aluminum pellets for the reaction. A second mixture consisting of ammonia and nitrogen is introduced into the reaction zone separately from the first mixture and subsequently reacts with the first mixture in the reaction zone, wherein Al2O3 is formed. 1-x Ti x N covering layer.

[0056] Typical reaction conditions are presented below in Table 1. If no MT-TiCN capping layer or other intermediate layer is provided (which is advantageous for the simplest possible capping system), only a TiN bonding layer is provided.

[0057] Table 1: For Al 1-x Ti x Typical reaction conditions of N capping layer (for H2S, see Table 3)

[0058]

[0059] In Table 2 below, general parameters corresponding to the deposited cover layers are presented by way of example.

[0060] Table 2: General parameters of the covering layer

[0061]

[0062] To test the Al corresponding to the previous statement 1-x Ti x Effect of hydrogen sulfide on the deposition of N capping layer. Al with different contents of hydrogen sulfide were produced during the deposition process. 1-x Ti x N capping layer. In Table 3 below, the corresponding reaction conditions are detailed, wherein a TiAlN capping layer as bonding layer is provided.

[0063] Table 3: Al in the presence of hydrogen sulfide 1-x Ti x Reaction conditions for the deposition of the N capping layer.

[0064] TiN AlTiN AlTiN Batch temperature [℃] 890 800 800 <![CDATA[AlCl3 temperature, generator]]> [℃] 365 365 365 <![CDATA[Flow rate of AlCl3]]> [L / min] 0 1.2 1.2 <![CDATA[H2S flow rate]]> [mL / min] 0 0 10* HCl flow rate [L / min] 0 0.35 0.35 <![CDATA[Flow rate of N2]]> [L / min] 14 5.5 5.5 <![CDATA[H2 flow rate]]> [L / min] 17 61 61 <![CDATA[Flow rate of TiCl4]]> [mL / min] 2.2 0.7 0.7 <![CDATA[NH3 flow rate]]> [L / min] 0 1 1 pressure [mbar] 160 23 23

[0065] * Subsequently, the H2S bypass was increased at 10 mL / min in each step, ultimately reaching 100 mL / min, to obtain the gradient layer.

[0066] exist Figure 2 In FIG. 1 , an image taken using a scanning electron microscope is shown, in which the corresponding covering layer on the cemented carbide body can be seen. Figure 3 As mentioned in , the coating is deposited in the presence of different amounts of hydrogen sulfide.

[0067] exist Figure 3 In the figure, a scanning electron microscope is used to magnify the Al 1-x Ti x N capping layer. Al 1-x Ti x The N capping layer comprises lamellae having a lamella thickness of less than 100 nm (the sum of each of one high-aluminum segment and one high-titanium segment), as is known from the corresponding capping layers. Figure 4 , which is shown in further magnification, is visible again.

[0068] Figure 5 Show according to Figure 4 Visualization of the reflections in the X-ray diffraction pattern during the deposition of the capping layer as a function of the H2S concentration, and the associated domain size according to the Debye-Scherrer formula. As can be seen, the typical cubic reflections become stronger with increasing H2S concentration, which indicates that the cubic phase is stabilized by the increase in H2S concentration. The domain size shows certain fluctuations, but it can be observed that the sheet size is approximately in the range of 20nm to 60nm. It can be said that the presence of H2S facilitates the formation of the cubic phase, i.e. alternating sheets of cubic fragments with higher aluminum concentration and cubic fragments with higher titanium concentration. This in turn provides the possibility to form a corresponding capping layer with a higher aluminum content, since the collapse in the hexagonal AlN structure is hindered. As shown in Figure 2 Figure 6 As shown, the X-ray diffraction pattern confirms the formation of the corresponding cubic structure.

[0069] Al 1-x Ti x The sulfur content in the N overburden is relatively low, as can be seen from Figure 7 and Figure 8 As can be seen from the combination of 1-x Ti x Oxygen concentration in the N capping layer. Figure 7 In the figure, the corresponding overlay can be seen, in which the different measurement positions of the spectrum were recorded and in which the measurement position is associated with an increase in the H2S content in the first reaction mixture. Figure 8 As can be seen in the figure, with the increase of H2S concentration, the generated Al 1-x Ti x The aluminum content in the N capping layer also increased. The sulfur content remained within the predetermined range within statistical significance.

[0070] In Al 1-x Ti x During the deposition of the N capping layer, in the presence of hydrogen sulfide, a Figure 1 or cut panels of the overlay system as described above and compared with similar coated cut panels produced in the absence of hydrogen sulfide during the deposition process. The corresponding processing results are presented in Table 4 below.

[0071] Table 4: Processing results

[0072]

[0073] As can be seen, with an external Al that already functions well in any case 1-x Ti x In a coating system with a N overlay, if Al 1-x Ti x Additional improvements can be achieved by deposition of an N capping layer.

Claims

1. A method for producing a covering on an object, in particular a cutting insert such as a cutting plate for machining technology, wherein a covering having one or more covering layers is applied to the object, wherein at least one Al 1- x Ti x The N capping layer was deposited using CVD, where the Al 1-x Ti x The nitrogen in the N capping layer can be partially replaced, characterized in that The Al 1-x Ti x The N capping layer is deposited in the presence of a sulfur-containing gas.

2. The method according to claim 1, characterized in that Hydrogen sulfide is used as the sulfur-containing gas.

3. The method according to claim 1 or 2, characterized in that: The Al 1-x Ti x The N capping layer is deposited with a volume fraction of hexagonal AlN of less than 20% by volume, preferably less than 10% by volume, in particular less than 5% by volume.

4. The method according to claim 1, characterized in that The Al 1-x Ti x The proportion of sulfur in the N capping layer is less than 5 atom %, preferably less than 4 atom %, in particular less than 3 atom %.

5. The method according to one of claims 1 to 4, characterized in that The Al 1-x Ti x The N capping layer is deposited as the outermost capping layer.

6. The method according to claim 1, characterized in that One or more capping layers are deposited on the Al 1-x Ti x Below the N capping layer, wherein preferably all capping layers are deposited using a CVD method.

7. The method according to claim 6, characterized in that The Al 1-x Ti x The N capping layer is deposited at a temperature of 800°C to 850°C, preferably 810°C to 830°C.

8. The method according to one of claims 1 to 7, characterized in that The Al is deposited from a first mixture of nitrogen, hydrogen, titanium tetrachloride, aluminum trichloride and hydrogen sulfide and a second mixture of nitrogen and ammonia. 1-x Ti x N covering layer.

9. The method according to claim 1, characterized in that The Al 1-x Ti x The N-capping layer at least partially embodies regions of lamellae, wherein the lamellae preferably have an average size determined according to the Debye-Scherrer formula of less than 150 nm, preferably less than 100 nm, in particular less than 80 nm.

10. The method according to one of claims 1 to 9, characterized in that An object made of cemented carbide is coated.

11. A coated body having a covering, the covering comprising at least one Al deposited using a CVD method. 1- x Ti x N capping layer, wherein the Al 1-x Ti x The nitrogen in the N capping layer can be partially replaced, characterized in that The Al 1-x Ti x The N capping layer includes sulfur.

12. The coated body according to claim 11, characterized in that: The Al 1-x Ti x The N capping layer exhibits a volume fraction of hexagonal AlN of less than 20% by volume, preferably less than 10% by volume, in particular less than 5% by volume.

13. The coated body according to claim 11 or 12, characterized in that: The Al 1-x Ti x The proportion of sulfur in the N capping layer is less than 5 atom %, preferably less than 4 atom %, in particular less than 3 atom %.

14. The coated body according to any one of claims 11 to 13, characterized in that The Al 1-x Ti x The N-capping layer at least partially embodies regions of lamellae, wherein the lamellae preferably have an average size determined according to the Debye-Scherrer formula of less than 150 nm, preferably less than 100 nm, in particular less than 80 nm.

15. The coated body according to any one of claims 11 to 14, characterized in that x is in the range of 0.85 to 0.99.