Antibacterial dressing containing copper ions and preparation method thereof

Through the design of the double-layer structure of calcium alginate fiber and copper alginate fiber and the modified bamboo fiber core sheath structure, the problem of silver ions and copper ions release safety is solved, and the sustained release of copper ions and wound healing effect is achieved, improving the improvement of copper ions The safety and durability of antibacterial dressings.

CN119074988APending Publication Date: 2024-12-06QINGDAO ZHONGTENG BIOTECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411263773.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The potential toxicity and insecurity of silver ions in existing antibacterial dressings, the immune toxicity of copper ions and the rapid release of copper ions in copper alginate fibers have limited its effectiveness and safety in wound healing process. .

Method used

Antibacterial dressing with double-layer structure of calcium alginate fiber and copper alginate fiber is used to isolate copper alginate fibers through calcium alginate fibers, and the sustained release of copper ions is regulated by the core sheath structure of modified bamboo fibers and chitosan quaternary ammonium salts. , combined with the hemostatic effect of graphene oxide and promotes healing, it forms a dressing with excellent hygroscopic, breathable and antibacterial properties.

Benefits of technology

It achieves the sustained release effect of copper ions, extends the use time of the dressing, improves wound healing efficiency and safety, enhances the mechanical strength and durability of the dressing, and maintains good antibacterial and antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the technical field of medical dressings, and particularly discloses an antibacterial dressing containing copper ions and a preparation method of the antibacterial dressing. The antibacterial dressing containing the copper ions comprises a dressing layer A close to one side of the skin and a dressing layer B far away from one side of the skin, the raw material of the dressing layer A comprises 100-150g / m < 2 > of calcium alginate fibers; the dressing layer B is prepared from the following raw materials: 30 to 120 g / m < 2 > of copper alginate fibers. The antibacterial dressing containing the copper ions can be used for promoting wound healing and has the advantages of being excellent in antibacterial property, high in safety and excellent in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of medical dressings, and more specifically, to an antibacterial dressing containing copper ions and a preparation method thereof. Background Art

[0002] Dressings, even if used as a covering outside the wound, can temporarily replace damaged skin during wound healing, avoid or control wound infection, and provide a suitable healing environment for the injured body surface. Traditional dressings can play a role in monitoring and covering wounds, but cannot be used for infected wounds, have no effect on wound healing, have limited exudate management capabilities, adhere to wounds, re-injure new epithelial tissue and cause bleeding, and cause pain to patients after changing dressings.

[0003] In order to provide a good wound healing environment, reduce scars, and improve user comfort, new medical dressings have gradually replaced traditional dressings that can only provide the simplest isolation and protection in recent years. Antibacterial dressings are one of them.

[0004] At present, the inorganic antibacterial materials used in the market are mainly Ag, Cu, and Zn, among which silver-containing dressings are the main ones. However, people gradually discovered that silver is not as safe as people imagined. Silver ions or nanosilver enter the human body through the skin, and silver compounds are basically insoluble except for silver nitrate, so they will cause heavy metal accumulation in the body, which will be harmful to health in the long run. In addition to having antibacterial properties similar to silver, copper can also use a variety of other mechanisms to fight microorganisms, such as releasing electrons, generating reactive oxygen, and causing serious damage to viruses, fungi and bacteria; in addition, copper shows excellent effectiveness in environments where the efficacy of silver is weakened. More importantly, copper is an essential trace element for the human body. Copper that enters the human body can be excreted from the body with metabolism; copper is also an important raw material for human hematopoiesis, which can catalyze the synthesis of hemoglobin and play an important role in human metabolism. It can enhance skin activity and stimulate the skin to form new capillaries. Using copper-containing medical dressings on wounds can ensure effective antibacterial while accelerating wound healing.

[0005] In addition, alginate, a biomass resource mainly composed of marine organisms, has the characteristics of abundant reserves, renewable, and no secondary pollution. It is an ideal biological resource for mankind in the future. Seaweed fiber developed with seaweed salt as raw material has excellent high hygroscopic gelation, overall easy removal, high oxygen permeability, biocompatibility, biodegradable absorbability, high ion adsorption and environmentally friendly production process, making seaweed fiber a hot spot in the field of new materials research today. Since alginate is a polymer carboxylic acid, alginate can be combined with different metal ions to form salts, and the generated alginate has good ion exchange properties. Copper alginate fiber is a new type of alginate fiber made of sodium alginate as raw material through a series of ion exchanges and wet spinning. It has excellent characteristics such as high hygroscopicity, high oxygen permeability, blocking gelation, biocompatibility, etc. It has certain medical care and antibacterial functions and has broad application prospects in the field of medical dressings.

[0006] Regarding the above-mentioned related technologies, the inventors found that copper ions have certain immunotoxicity and will have a negative impact on the immune system of animals (see "Immunotoxicity of Copper Alginate Fibers in Guinea Pigs and Mice", Biol Trace Elem Res, 2011, edited by Ying Gong et al.). When copper alginate fibers are used as wound dressings, the copper ions therein will be absorbed by the human body, which indicates that the release of copper ions needs to be controlled to avoid potential immunotoxicity. Summary of the invention

[0007] In order to promote the sustained release of copper ions and enhance the antibacterial property and safety of medical dressings prepared with copper alginate, the present application provides an antibacterial dressing containing copper ions and a preparation method thereof.

[0008] In a first aspect, the present application provides an antibacterial dressing containing copper ions, which adopts the following technical solution: An antibacterial dressing containing copper ions, comprising a dressing layer A on a side close to the skin and a dressing layer B on a side away from the skin; The raw materials of the dressing layer A include 100-150g / m 2 Calcium alginate fiber; The raw materials of the dressing layer B include 30-120 g / m 2 Copper alginate fibers.

[0009] By adopting the above technical solution, the medical dressing prepared by alginate fiber has good liquid absorption and air permeability on the one hand, which can accelerate the absorption of wound exudate, prevent the wound from being overly moist, and reduce the chance of bacterial growth; on the other hand, alginate dressing has natural excellent adhesion, is relatively gentle, can fit tightly on the wound surface to form a protective barrier, is not easy to fall off, and can move with the movement of the skin around the wound, reducing wound strain caused by too tight adhesion of the dressing, and is easy to remove, reducing damage to new tissue when changing the dressing.

[0010] In addition to having antibacterial capabilities similar to those of silver ions used in traditional antibacterial dressings, copper ions can also inhibit and kill bacteria growing in wound exudate by releasing electrons, generating reactive oxygen species, inhibiting bacterial growth mechanisms, and inhibiting DNA to RNA transcription, thereby promoting wound healing. At the same time, the copper in the dressing can also isolate bacteria and virus sources in the air to prevent wound infection.

[0011] The copper ions in copper alginate are released quickly and in large amounts at one time, which does not meet the requirements for safe use by the human body. However, since the complexing force of alginate on copper ions is much stronger than that of calcium ions, using calcium alginate as dressing layer A to isolate copper alginate and the wound can effectively delay the release of copper ions and achieve a sustained-release effect. The release amount is in the ppm order, which acts on the wound for a long time and promotes wound healing.

[0012] Optionally, the raw materials of the dressing layer B include copper alginate fiber and modified bamboo fiber, and the mass ratio of the copper alginate fiber to the modified bamboo fiber is 1:(0.4-0.8).

[0013] By adopting the above technical solution, the strength and elasticity of the dressing prepared by alginate fiber are poor. The addition of modified bamboo fiber can effectively improve the mechanical strength and softness of the dressing and prevent the dressing from breaking during use.

[0014] Optionally, the modified bamboo fiber includes a core layer and a sheath layer with a diameter ratio of (0.8-2.4):1; the raw materials of the core layer include bamboo pulp fiber and chitosan quaternary ammonium salt in a mass ratio of (12-16):(1-3); the raw materials of the sheath layer include 1:(12-17) graphene oxide and polymer matrix.

[0015] By adopting the above technical scheme, chitosan quaternary ammonium salt is used as the core layer raw material, which can significantly enhance the antibacterial and bactericidal effect of the dressing layer B formed by the composite of modified bamboo fiber and copper alginate fiber. Chitosan quaternary ammonium salt has good water solubility, flocculation, biocompatibility, moisture absorption and antibacterial properties. After absorbing liquid, chitosan quaternary ammonium salt can be adsorbed on the cell surface to form a layer of polymer film, which hinders the transport of nutrients to the inside, thereby inhibiting the growth and reproduction of bacteria.

[0016] On the one hand, chitosan quaternary ammonium salt and copper ions in copper alginate form an antibacterial and bactericidal system, which significantly enhances the antibacterial and bactericidal effect of the dressing; on the other hand, chitosan quaternary ammonium salt can be used as a carrier of copper ions to further adjust the release rate of copper ions and promote the sustained release effect of copper ions. In addition, alginate fiber has high hygroscopicity, while chitosan has good moisturizing properties. The combined use of the two can provide better moisture absorption and moisturizing effects, which helps maintain a moist environment for the wound.

[0017] As a raw material for the sheath layer, graphene oxide can not only enhance the antibacterial effect of dressing layer B, but also, on the one hand, graphene oxide has a large specific surface area and strong physical adsorption capacity, which can quickly absorb blood at the wound, adsorb platelets and coagulation factors in the blood, promote blood coagulation, and accelerate hemostasis at the wound; on the other hand, graphene oxide can promote cell proliferation and migration, which helps the wound to heal quickly.

[0018] The dressing layer B prepared by designing the core layer and sheath layer raw materials and compositely preparing the core-sheath structure modified bamboo fiber and copper alginate can significantly improve the strength and elasticity of the dressing layer, improve the mechanical strength and softness of the dressing, prevent the dressing from breaking during use, etc., and improve the durability of the dressing.

[0019] Optionally, the preparation method of the modified bamboo fiber comprises the following steps: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution, chitosan quaternary ammonium salt is added and ultrasonically stirred for 1-1.5 hours to obtain a core layer spinning solution; The graphene oxide is evenly dispersed in an ethanol B solution, a polymer matrix is ​​added, and the mixture is stirred evenly to obtain a sheath spinning solution; the core layer spinning solution and the sheath layer spinning solution are coaxially electrospun, and after being collected, they are solidified, stretched, and dried to obtain a core-sheath structure modified bamboo fiber in which the core layer is wrapped by the sheath layer.

[0020] Optionally, the solid-liquid ratio of the bamboo pulp fiber to the ethanol A solution is 1:(6-8); the solid-liquid ratio of the graphene to the ethanol B solution is 1:(6-8).

[0021] Optionally, the polymer matrix is ​​selected from any one of polyurethane, polytetrafluoroethylene, polycaprolactone, and polyetheretherketone.

[0022] By adopting the above technical scheme, polyurethane, polytetrafluoroethylene, polycaprolactone, and polyetheretherketone all have good biocompatibility and can be safely used in the biomedical field. They are used as polymer matrices to prepare sheath fibers with a core-sheath structure, which have good strength and chemical stability, and help to improve the mechanical strength and elasticity of the modified bamboo fibers, and improve the strength, elasticity and durability of the final antibacterial dressings.

[0023] Optionally, it also includes a backing layer arranged on the side of the dressing layer B away from the skin.

[0024] By adopting the above technical solution, the use of the backing layer provides additional protection and support for the antibacterial dressing, has a waterproof effect, and helps to improve the overall durability and ease of use of the dressing.

[0025] Optionally, the backing layer is a PU film.

[0026] In a second aspect, the present application provides a method for preparing an antibacterial dressing containing copper ions, using the following technical solution: A method for preparing an antibacterial dressing containing copper ions comprises the following steps: The calcium alginate fibers are cut to form short fibers, and the short fibers are opened and then mixed with cotton; the mixed fibers are combed into a fiber web A, and then needle-punched to form a calcium alginate non-woven dressing layer A; The copper alginate fibers are cut to form short fibers, the short fibers are opened and then mixed with cotton; and the mixed fibers are combed into a fiber web B; The copper alginate fiber mesh B is evenly laid on the surface of the calcium alginate non-woven fabric dressing layer A to form a dressing layer B, which is then acupunctured, cut, packaged, disinfected and sterilized to obtain the dressing layer B.

[0027] By adopting the above technical scheme, a copper calcium alginate double-layer structure non-woven dressing is prepared by combing and needling the fibers after mixing with cotton. The process is simple, easy to promote, and can ensure the quality and performance of the dressing.

[0028] Optionally, the method for preparing the dressing layer B comprises the following steps: The copper alginate fiber and the modified bamboo fiber are cut into short fibers respectively, the copper alginate short fibers are mixed with the modified bamboo fiber short fibers, and then loosened and blended with cotton; the blended fibers are combed into a fiber web, and then needle-punched to form a copper alginate composite non-woven fabric dressing layer B.

[0029] In summary, this application has the following beneficial effects: 1. In the present application, a two-layer copper-calcium alginate antibacterial dressing is formed by acupuncture using calcium alginate fiber and copper alginate fiber as raw materials. Calcium alginate is used as dressing layer A to isolate copper alginate and wounds, which can effectively delay the release of copper ions, making the release amount in the ppm order of magnitude, achieving a sustained release effect, and can effectively act on the wound for a long time to promote wound healing.

[0030] 2. In the present application, the dressing layer B is prepared by compounding modified bamboo fiber with a core-sheath structure and copper alginate fiber, which significantly improves the shortcomings of alginate fiber, such as lightness, poor elasticity and insufficient durability, and can prevent the dressing from breaking during use, thereby improving the durability of the dressing.

[0031] 3. The core layer of the modified bamboo fiber in the present application contains chitosan quaternary ammonium salt, which can act as a carrier of copper ions to further regulate the release effect of copper ions, promote the sustained release of copper ions, and further enhance the antibacterial and bactericidal effect of the dressing layer B; the graphene oxide in the sheath layer can enhance the hemostatic and coagulation effect of the dressing, promote cell proliferation and migration, and accelerate wound healing. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 1 is an antibacterial effect diagram of the antibacterial dressing of the present application on Escherichia coli (Gram-negative bacteria) in an antibacterial liquid experiment, and ae are respectively Example 1-2, Comparative Example 1-2 and a blank control group.

[0033] Figure 2 1 is an antibacterial effect diagram of the antibacterial dressing of the present application on Staphylococcus aureus (Gram-positive bacteria) in an antibacterial liquid experiment, and ae are respectively Example 1-2, Comparative Example 1-2 and a blank control group.

[0034] Figure 3 1 is an antibacterial experimental effect diagram of the antibacterial dressing of the present application on Escherichia coli (Gram-negative bacteria) in the antibacterial ring experiment, and ae are Example 1-2, Comparative Example 1-2 and blank control group respectively.

[0035] Figure 4 1 is an antibacterial experimental effect diagram of the antibacterial dressing of the present application on Staphylococcus aureus (Gram-positive bacteria) in the antibacterial ring experiment, and ae are Example 1-2, Comparative Example 1-2 and blank control group respectively. DETAILED DESCRIPTION

[0036] The present application is further described in detail below in conjunction with embodiments.

[0037] raw material Unless otherwise specified, the raw materials used in the preparation examples, embodiments and comparative examples in this application are all commercially available products, specifically: Copper alginate fiber, selected from the State Key Laboratory of Biopolysaccharide Fiber Forming and Eco-textiles of Qingdao University, with a copper ion content of 1-5 mg / g; Calcium alginate fiber, selected from Qingdao Zhongteng Biotechnology Co., Ltd.; Bamboo pulp fiber, average diameter 50μm, average length 2mm; Graphene oxide, selected from Shanghai Shifeng Biotechnology Co., Ltd., A16225-1g; Chitosan quaternary ammonium salt, selected from Xi'an Yahua Biotechnology Co., Ltd., YH-2023031601; Polyurethane, selected from Guangdong 137 Chemical Technology Co., Ltd., MR-879; Polytetrafluoroethylene, selected from Daikin, Japan, F-104; Polycaprolactone, selected from Suzhou Renfu Plastic Co., Ltd., FUPAIPCL 6500; Ethanol A solution and ethanol B solution are both 50% ethanol.

[0038] Preparation example of modified bamboo fiber Preparation Example 1 The modified bamboo fiber comprises a core layer and a sheath layer. The raw materials of the core layer comprise bamboo pulp fiber and chitosan quaternary ammonium salt in a mass ratio of 12:1, and the raw materials of the sheath layer comprise graphene oxide and polyurethane in a mass ratio of 1:15.

[0039] The preparation method of the modified bamboo fiber comprises the following steps: S1: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution at a solid-liquid ratio of 1:6, chitosan quaternary ammonium salt is added, and ultrasonic stirring is performed for 1.5 hours to obtain a core layer spinning solution; S2: Evenly disperse graphene oxide in ethanol B solution at a material-liquid ratio of 1:6, add polyurethane, and stir evenly for 2 hours to obtain a sheath spinning solution; S3: The core layer spinning solution and the sheath layer spinning solution are coaxially electrospun, and the diameter ratio of the core layer and the sheath layer is 1.5:1. After collection, they are cured, stretched and dried to obtain a core-sheath structure modified bamboo fiber with the sheath layer wrapping the core layer.

[0040] Preparation Example 2 The modified bamboo fiber comprises a core layer and a sheath layer. The raw materials of the core layer comprise bamboo pulp fiber and chitosan quaternary ammonium salt in a mass ratio of 15:3, and the raw materials of the sheath layer comprise graphene oxide and polyurethane in a mass ratio of 1:17.

[0041] The preparation method of the modified bamboo fiber comprises the following steps: S1: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution at a solid-liquid ratio of 1:8, chitosan quaternary ammonium salt is added, and ultrasonic stirring is performed for 1 h to obtain a core layer spinning solution; S2: Evenly disperse graphene oxide in ethanol B solution at a material-liquid ratio of 1:7, add polyurethane, and stir evenly for 2 hours to obtain a sheath spinning solution; S3: The core layer spinning solution and the sheath layer spinning solution are coaxially electrospun, and the diameter ratio of the core layer and the sheath layer is 0.8:1. After collection, they are cured, stretched and dried to obtain a core-sheath structure modified bamboo fiber with the sheath layer wrapping the core layer.

[0042] Preparation Example 3 The modified bamboo fiber comprises a core layer and a sheath layer. The raw materials of the core layer comprise bamboo pulp fiber and chitosan quaternary ammonium salt in a mass ratio of 16:2, and the raw materials of the sheath layer comprise graphene oxide and polycaprolactone in a mass ratio of 1:12.

[0043] The preparation method of the modified bamboo fiber comprises the following steps: S1: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution at a solid-liquid ratio of 1:7, chitosan quaternary ammonium salt is added, and ultrasonic stirring is performed for 1.5 hours to obtain a core spinning solution; S2: graphene oxide is uniformly dispersed in ethanol B solution at a material-liquid ratio of 1:8, polycaprolactone is added, and the mixture is uniformly stirred for 2 hours to obtain a sheath spinning solution; S3: The core layer spinning solution and the sheath layer spinning solution are coaxially electrospun, and the diameter ratio of the core layer and the sheath layer is 2.4:1. After collection, they are cured, stretched and dried to obtain a core-sheath structure modified bamboo fiber with the sheath layer wrapping the core layer.

[0044] Preparation Example 4 The modified bamboo fiber includes a core layer and a sheath layer. The difference from Preparation Example 1 is that chitosan quaternary ammonium salt is not added to the core layer raw material, and the chitosan quaternary ammonium salt is replaced by polyurethane of equal mass. The other steps are the same as Preparation Example 1.

[0045] Preparation Example 5 The modified bamboo fiber includes a core layer and a sheath layer. The difference from Preparation Example 1 is that graphene oxide is not added to the sheath layer raw material, and the graphene oxide is replaced by bamboo fiber of equal mass. The other steps are the same as Preparation Example 1.

[0046] Preparation Example 6 The modified bamboo fiber comprises a raw material component A and a raw material component B, wherein the raw material component A comprises bamboo pulp fiber and chitosan quaternary ammonium salt in a mass ratio of 12:1, and the raw material component B comprises graphene oxide and polyurethane in a mass ratio of 1:15.

[0047] The preparation method of the modified bamboo fiber comprises the following steps: S1: The bamboo pulp fiber was crushed and uniformly dispersed in an ethanol A solution at a solid-liquid ratio of 1:6, chitosan quaternary ammonium salt was added, and ultrasonic stirring was performed for 1.5 h to obtain a spinning solution A; S2: Evenly disperse graphene oxide in ethanol B solution at a material-liquid ratio of 1:6, add polyurethane, and stir evenly for 2 hours to obtain spinning solution B; S3: Spinning solution A and spinning solution B are respectively subjected to electrostatic spinning, and after collection, they are solidified, stretched, and dried to obtain fiber A and fiber B, which are then mixed.

[0048] Preparation Example 7 The modified bamboo fiber comprises bamboo pulp fiber and polyurethane in a mass ratio of 12:1, and the preparation method thereof comprises the following steps: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution at a solid-liquid ratio of 1:6. Polyurethane is added and ultrasonically stirred for 1.5 hours to obtain a spinning solution. The spinning solution is electrospun, collected, solidified, stretched, and dried. Example

[0049] Example 1 An antibacterial dressing containing copper ions comprises a dressing layer A on a side close to the skin, a dressing layer B on a side away from the skin, and a backing layer, wherein the backing layer is a medical PU film. The preparation method of the antibacterial dressing containing copper ions comprises the following steps: S1: cutting calcium alginate fibers to form short fibers, opening the short fibers and placing them in a cotton blending machine for blending; combing the blended fibers into a fiber web A in a carding machine, and then placing the fiber web in a needle punching machine for needle punching to form a calcium alginate non-woven fabric dressing layer A; S2: cutting the copper alginate fibers into short fibers, opening the short fibers and blending them with cotton; combing the blended fibers into a fiber web B; S3: unfold the calcium alginate nonwoven fabric in front of the needling machine, enter the needling state, evenly lay the copper alginate fiber mesh B on the surface of the calcium alginate nonwoven dressing layer A to form a dressing layer B, and obtain a double-layer copper calcium alginate dressing after needling, cutting, packaging, disinfection and sterilization, wherein the weight of the calcium alginate fiber is 100g / m 2 The weight of copper alginate fiber is 100g / m 2 ; S4: stacking the PU film and the side of the dressing layer B away from the dressing layer A together, and heating so that the PU film is pressed onto the outside of the dressing layer B as a backing layer.

[0050] Example 2 An antibacterial dressing containing copper ions comprises a dressing layer A on a side close to the skin, a dressing layer B on a side away from the skin, and a backing layer, wherein the backing layer is a medical PU film. The preparation method of the antibacterial dressing containing copper ions comprises the following steps: S1: cutting calcium alginate fibers to form short fibers, opening the short fibers and placing them in a cotton blending machine for blending; combing the blended fibers into a fiber web in a carding machine, and then placing the fiber web in a needle punching machine for needle punching to form a calcium alginate non-woven fabric dressing layer A; S2: cutting the copper alginate fibers into short fibers, opening the short fibers and blending them with cotton; combing the blended fibers into a fiber web B; S3: unfold the calcium alginate nonwoven fabric in front of the needling machine, enter the needling state, evenly lay the copper alginate fiber mesh B on the surface of the calcium alginate nonwoven dressing layer A to form a dressing layer B, and obtain a double-layer copper calcium alginate dressing after needling, cutting, packaging, disinfection and sterilization, wherein the weight of the calcium alginate fiber is 100g / m2 The weight of copper alginate fiber is 50g / m 2 ; S4: stack the PU film and the side of the dressing layer B away from the dressing layer A, and heat the PU film so that it is pressed onto the outside of the dressing layer B as a backing layer.

[0051] Example 3 An antibacterial dressing containing copper ions comprises a dressing layer A on a side close to the skin, a dressing layer B on a side away from the skin, and a backing layer, wherein the backing layer is a medical PU film. The preparation method of the antibacterial dressing containing copper ions comprises the following steps: S1: cutting calcium alginate fibers to form short fibers, opening the short fibers and placing them in a cotton blending machine for blending; combing the blended fibers into a fiber web in a carding machine, and then placing the fiber web in a needle punching machine for needle punching to form a calcium alginate non-woven fabric dressing layer A; S2: cutting the copper alginate fibers into short fibers, opening the short fibers and blending them with cotton; combing the blended fibers into a fiber web B; S3: unfold the calcium alginate nonwoven fabric in front of the needling machine, enter the needling state, evenly lay the copper alginate fiber mesh B on the surface of the calcium alginate nonwoven dressing layer A to form a dressing layer B, and obtain a double-layer copper calcium alginate dressing after needling, cutting, packaging, disinfection and sterilization, wherein the weight of the calcium alginate fiber is 150g / m 2 The weight of copper alginate fiber is 100g / m 2 ; S4: stacking the PU film and the side of the dressing layer B away from the dressing layer A together, and heating so that the PU film is pressed onto the outside of the dressing layer B as a backing layer.

[0052] Example 4 An antibacterial dressing containing copper ions comprises a dressing layer A on a side close to the skin, a dressing layer B on a side away from the skin, and a backing layer, wherein the backing layer is a medical PU film. The preparation method of the antibacterial dressing containing copper ions comprises the following steps: S1: cutting calcium alginate fibers to form short fibers, opening the short fibers and placing them in a cotton blending machine for blending; combing the blended fibers into a fiber web in a carding machine, and then placing the fiber web in a needle punching machine for needle punching to form a calcium alginate non-woven fabric dressing layer A; S2: cutting the copper alginate fibers into short fibers, opening the short fibers and blending them with cotton; combing the blended fibers into a fiber web B; S3: unfold the calcium alginate nonwoven fabric in front of the needling machine, enter the needling state, evenly lay the copper alginate fiber mesh B on the surface of the calcium alginate nonwoven dressing layer A to form a dressing layer B, and obtain a double-layer copper calcium alginate dressing after needling, cutting, packaging, disinfection and sterilization, wherein the weight of the calcium alginate fiber is 125g / m 2The weight of copper alginate fiber is 75g / m 2 ; S4: stack the PU film and the side of the dressing layer B away from the dressing layer A, and heat the PU film so that it is pressed onto the outside of the dressing layer B as a backing layer.

[0053] Example 5 An antibacterial dressing containing copper ions, which is different from Example 1 in that the weight of calcium alginate fiber in dressing layer A is 100 g / m 2 The weight of copper alginate fiber in dressing layer B is 30g / m 2 , the other steps are the same as those in Example 1.

[0054] Example 6 An antibacterial dressing containing copper ions, which is different from Example 1 in that the weight of calcium alginate fiber in dressing layer A is 150 g / m 2 The weight of copper alginate fiber in dressing layer B is 120g / m 2 , the other steps are the same as those in Example 1.

[0055] Example 7 An antibacterial dressing containing copper ions, which is different from Example 1 in that the specific steps of step S2 are: cutting the copper alginate fiber and the modified bamboo fiber prepared in Preparation Example 1 to form short fibers respectively, mixing the copper alginate short fibers and the modified bamboo fiber short fibers at a mass ratio of 1:0.4, placing them in a cotton mixer for opening and then blending, combing the blended fibers into a fiber web B, and the other steps are the same as Example 1.

[0056] Example 8 An antibacterial dressing containing copper ions, which differs from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 2, the mass ratio of copper alginate short fibers to modified bamboo fiber short fibers is 1:0.6, and the other steps are the same as Example 7.

[0057] Example 9 An antibacterial dressing containing copper ions, which differs from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 3, the mass ratio of copper alginate short fibers to modified bamboo fiber short fibers is 1:0.8, and the other steps are the same as Example 7.

[0058] Example 10 An antibacterial dressing containing copper ions, which is different from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 4, and the other steps are the same as those of Example 7.

[0059] Embodiment 11 An antibacterial dressing containing copper ions, which is different from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 5, and the other steps are the same as Example 7.

[0060] Example 12 An antibacterial dressing containing copper ions, which is different from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 6, and the other steps are the same as Example 7.

[0061] Example 13 An antibacterial dressing containing copper ions, which is different from Example 7 in that the modified bamboo fiber is prepared by Preparation Example 7, and the other steps are the same as Example 7.

[0062] Comparative Example Comparative Example 1 A calcium alginate dressing comprises a dressing layer on a side close to the skin and a backing layer, wherein the backing layer is a medical PU film, and a preparation method thereof comprises the following steps; S1: cutting the calcium alginate fibers into short fibers, opening the short fibers and placing them in a cotton blending machine for blending; S2: The mixed cotton fibers are combed into a fiber web in a carding machine, and then the fiber web is placed in a needle punching machine for needle punching to form a calcium alginate non-woven dressing layer, and then cut, package, disinfect and sterilize to obtain a calcium alginate dressing. The weight of the calcium alginate fiber is 100g / m 2 ; S3: stacking the PU film and the dressing layer together, heating the PU film so that it is pressed onto the outside of the dressing layer as a backing layer.

[0063] Comparative Example 2 A copper alginate dressing comprises a dressing layer on a side close to the skin and a backing layer, wherein the backing layer is a medical PU film, and a preparation method thereof comprises the following steps: S1: cutting the copper alginate fibers into short fibers, opening the short fibers and placing them in a cotton blending machine for blending; S2: Combing the mixed cotton fibers into a fiber web in a carding machine, and then putting the fiber web into a needle punching machine for needle punching to obtain a copper alginate non-woven dressing layer, cutting, packaging, disinfecting and sterilizing to form a copper alginate dressing, the weight of the copper alginate fiber is 100g / m 2 ; S3: stack the PU film and the dressing layer together, heat the PU film so that it is pressed onto the outside of the dressing layer as a backing layer.

[0064] Performance testing Test Example 1: Copper ion sustained release experiment The antibacterial dressings containing copper ions in Examples 1-13 and Comparative Examples 1-2 without backing layer lamination were placed on the surface of physiological saline (0.9% NaCl) respectively to ensure that the antibacterial dressings were in contact with the liquid surface. When the antibacterial dressings containing copper ions in Examples 1-13 were tested, the antibacterial dressings were in contact with the liquid surface and the liquid surface did not exceed the dressing layer A of calcium alginate. They were placed at 37° C. and the extracts were taken every day for 1 week.

[0065] The copper ion concentration in the extract was detected by BCO (dicyclohexanone oxalyldihydrazone) photometry, and the copper ion release per unit mass of the antibacterial dressing was calculated. The test results are recorded in Table 1.

[0066] Table 1 According to the performance test results in Table 1, it can be seen that the antibacterial dressing containing copper ions in the present application has an excellent sustained-release effect of copper ions. The amount of copper ions released every day is in the ppm order of magnitude, which is much lower than the 340 μg / day specified by FDA and ISO. Moreover, it can be released for a long time and play an effective role for a long time. After continuous measurement for one week, the release of copper ions still remains in the ppm order of magnitude.

[0067] It can be seen from the performance test results of Examples 1-6 and Examples 7-9 that the present application can further regulate the release amount of copper ions by adding modified bamboo fiber to the dressing layer B, thereby effectively delaying the release of copper ions.

[0068] According to the performance test results of Examples 7 and 10-13, it can be seen that the modified bamboo fiber with a shell-sheath structure has a better sustained-release effect on copper ions as one of the raw materials for the dressing layer than the modified bamboo fiber obtained by blending. Chitosan quaternary ammonium salt, as one of the core layer raw materials of the modified bamboo fiber, can be used as a carrier of copper ions to further regulate the release rate of copper ions and adjust the sustained-release effect of copper ions.

[0069] Test Example 2 Antibacterial Liquid Experiment An antibacterial experiment was performed on the antibacterial dressing containing copper ions in Examples 1-13 and Comparative Examples 1-2 without backing layer lamination, and the antibacterial rate was calculated. The antibacterial experiment adopted the colony counting method, with reference to the corporate standard of Qingdao Zhongteng Biotechnology Co., Ltd. and the document published by Ning Chengyun et al. "Concentration ranges of antibacterial cations for showing the highest antibacterial efficacy but the least cytotoxicity against mammalian cells: implications for a new antibacterial mechanism. Chem Res Toxicol. 2015. 28 (9): 1815-1822", and the bacterial species selected were Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria).

[0070] Experimental methods: Experimental group: The antibacterial dressings containing copper ions of Examples 1-13 and Comparative Examples 1-2 were placed in physiological saline (0.9% NaCl) to release copper ions and calcium ions. After 24 hours, the released liquid was taken out, filtered and sterilized through a 0.22 μm filter membrane, and stored at 4°C.

[0071] Under sterile conditions, the test bacteria were cultured in the slant medium for 24 h and then eluted with PBS buffer and diluted to 10 -6 CFU / mL of bacterial solution is reserved.

[0072] Under sterile conditions, take 100 μL of release solution and 900 μL of 10 -6 CFU / mL bacterial solution was mixed to obtain culture solution, and incubated at 37°C for 24 h; 100 μL of the above culture solution was added dropwise to a sterile nutrient agar plate, spread evenly, and cultured at 37°C for 24 h. The colonies were counted and the inhibition rate was calculated.

[0073] A blank control group was set up: 100 μL PBS buffer and 900 μL 10 -6 CFU / mL of bacterial liquid was mixed to obtain culture solution, and incubated at 37°C for 24 h; 100 μL of the above culture solution was added dropwise to a sterile nutrient agar plate, spread evenly, and cultured at 37°C for 24 h. The colonies were counted and the inhibition rate was calculated.

[0074] Antibacterial rate calculation formula: Antibacterial rate (%) = (number of colonies 空白对照组 - Colony count 实验组 ) / colony count 空白对照组 ×100% Attached Figure 1-2 These are pictures of the experimental effects of the antibacterial liquid of Example 1-2, Comparative Example 1-2 and the blank control group on Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria).

[0075] Table 2 According to Table 2 and Appendix Figure 1-2 It can be seen from the performance test results that pure calcium alginate has almost no antibacterial activity. The antibacterial rates of the copper ion-containing antibacterial dressing of the present application and the pure copper alginate dressing for Staphylococcus aureus both reach 100%, and the antibacterial rates for Escherichia coli reach more than 95%. This shows that the copper calcium alginate dressing only delays the release of copper ions, so that the release amount of copper ions is within a controllable range, without reducing its antibacterial performance. The copper ion-containing antibacterial dressing of the present application can be used as an excellent medical antibacterial dressing.

[0076] According to the performance test results of Examples 1-6 and Examples 7-13, it can be seen that the addition of modified bamboo fiber helps to further improve the antibacterial properties of the copper ion-containing antibacterial dressing, and the addition of chitosan quaternary ammonium salt and graphene oxide both contribute to the improvement of the antibacterial and antibacterial properties of the dressing.

[0077] Test Example 3: Antibacterial ring experiment The antibacterial ring test experiment was carried out on the dressings in Example 1-2 and Comparative Example 1-2 without the backing layer laminated, and the antibacterial ring test was carried out by the agar plate diffusion method, referring to the standard GB / T20944.1-2007 "Evaluation of Antibacterial Properties of Textiles", and the bacterial species selected were Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria).

[0078] Experimental method: After Escherichia coli and standard strains of Staphylococcus aureus were revived (cultured for 18-24 hours), they were streaked on plates to obtain single colonies.

[0079] Experimental group: Typical single colonies were inoculated into broth test tubes and cultured at 37°C for 6 h. 0.1 mL of culture solution was added dropwise to a sterile nutrient agar plate and evenly spread. The dressings obtained in Example 1-2 and Comparative Example 1-2 without backing layer were placed flat in the center of the culture dish. After culture at 37°C for 24 h, the size of the inhibition ring was observed.

[0080] Set up a blank control group: take typical single colonies and inoculate them into broth test tubes, culture them at 37℃ for 6h, add 0.1mL of culture solution on a sterile nutrient agar plate, spread it evenly, and culture it at 37℃ for 24h to observe the size of the inhibition ring.

[0081] Attached Figure 3-4 The pictures are the antibacterial ring experimental effects of Example 1-2, Comparative Example 1-2 and the blank control group on Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria).

[0082] according to Figure 3-4 It can be seen from the antibacterial ring test results that the pure calcium alginate fiber dressing group in comparative example 1 showed no obvious antibacterial ring against Escherichia coli and Staphylococcus aureus, which indicates that pure calcium alginate dressing has almost no antibacterial activity.

[0083] Compared with the copper alginate fiber dressing of Comparative Example 2, the copper calcium alginate fiber dressing group of Examples 1-2 showed an obvious antibacterial ring and the area of ​​the antibacterial ring slowly expanded and extended around the dressing, which shows that the copper ion-containing antibacterial dressing of the present application has excellent antibacterial properties. The main antibacterial effect is copper ions. The composite with calcium alginate fiber can ensure that the copper ions exert their antibacterial properties while delaying the release rate of copper ions, thereby improving the safety of antibacterial dressings in the medical field.

[0084] Test Example 4 Mechanical Properties Test The mechanical properties of the antibacterial dressings containing copper ions without backing layer lamination in Examples 1-13 were tested.

[0085] Tensile strength test method: Cut the material into a rectangle of 75×15mm, measure its thickness with a thickness meter at room temperature and 60% humidity, and then use a universal material testing machine to measure its tension and elongation at break. The set parameters are as follows: stretching speed is 10mm / min, clamping distance is 65mm, and sample width is 15mm.

[0086] The tensile strength and elongation at break were calculated. Each test was performed 3 times. The average results were calculated and recorded in Table 3. The tensile strength was the ratio of the maximum tensile stress to the cross-sectional area of ​​the sample; the elongation at break was the ratio of the deformation length of the sample at tensile fracture to the initial length.

[0087] Table 3 According to the performance test data results in Table 3, it can be seen from the comparison results of the performance test data of Examples 1-6 and Examples 7-9 that the addition of modified fibers significantly improves the mechanical properties of the antibacterial dressing, can effectively make up for the disadvantages of poor strength and elasticity of alginate fibers, prevent the antibacterial dressing from breaking during use, and improve the durability of the antibacterial dressing.

[0088] According to the comparison results of the performance test data of Example 7, Example 10-11 and Example 13, it can be seen that when chitosan quaternary ammonium salt is used as the core layer raw material and graphene oxide is used as the wall layer raw material, the tensile strength and elongation at break of the antibacterial dressing are improved. This is because the addition of chitosan quaternary ammonium salt can increase the binding force between the antibacterial dressing fibers through ionic bonding, thereby improving the mechanical properties of the antibacterial dressing. The addition of graphene oxide plays the interaction between the van der Waals force, hydrogen bond and the like between the graphene oxide sheets, forms a stable network structure inside the fiber, and can form a stronger interface bond with other matrix materials, thereby improving the mechanical properties of the antibacterial dressing.

[0089] According to the comparison results of the performance test data of Example 7 and Examples 12-13, it can be seen that the modified bamboo fiber with a core-sheath structure can give the antibacterial dressing greater tensile strength and elongation at break. The sheath structure provides additional support and protection for the core structure, and when mixed with other fibers, it can form a more stable inter-fiber structure, enhance the overall stability of the fiber network, and thus improve the mechanical properties of the antibacterial dressing.

[0090] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An antibacterial dressing containing copper ions, characterized in that: It includes a dressing layer A on the side close to the skin and a dressing layer B on the side away from the skin; The raw materials of the dressing layer A include 100-150g / m 2 Calcium alginate fiber; The raw materials of the dressing layer B include 30-120 g / m 2 Copper alginate fibers.

2. The antibacterial dressing containing copper ions according to claim 1, characterized in that: The raw materials of the dressing layer B include copper alginate fiber and modified bamboo fiber, and the mass ratio of the copper alginate fiber to the modified bamboo fiber is 1:(0.4-0.8).

3. The antibacterial dressing containing copper ions according to claim 2, characterized in that: The modified bamboo fiber comprises a core layer and a sheath layer with a diameter ratio of (0.8-2.4):1; the raw materials of the core layer comprise bamboo pulp fiber and chitosan quaternary ammonium salt with a mass ratio of (12-16):(1-3); the raw materials of the sheath layer comprise 1:(12-17) graphene oxide and a polymer matrix.

4. The antibacterial dressing containing copper ions according to claim 3, characterized in that: The preparation method of the modified bamboo fiber, The following steps are involved: The bamboo pulp fiber is crushed and evenly dispersed in ethanol A solution, chitosan quaternary ammonium salt is added and ultrasonically stirred for 1-1.5 hours to obtain a core layer spinning solution; The graphene oxide is uniformly dispersed in the ethanol B solution, the polymer matrix is ​​added, and the mixture is stirred uniformly to obtain a sheath spinning solution; The core layer spinning solution and the sheath layer spinning solution are coaxially electrospun, and after being collected, they are solidified, stretched and dried to obtain a core-sheath structure modified bamboo fiber in which the sheath layer wraps the core layer.

5. The antibacterial dressing containing copper ions according to claim 4, characterized in that: The solid-liquid ratio of the bamboo pulp fiber to the ethanol A solution is 1:(6-8); the solid-liquid ratio of the graphene to the ethanol B solution is 1:(6-8).

6. The antibacterial dressing containing copper ions according to claim 3, characterized in that: The polymer matrix is ​​selected from any one of polyurethane, polytetrafluoroethylene, polycaprolactone and polyetheretherketone.

7. The antibacterial dressing containing copper ions according to claim 1, characterized in that , also includes a backing layer arranged on the side of the dressing layer B away from the skin.

8. The antibacterial dressing containing copper ions according to claim 7, characterized in that , the backing layer is a PU film.

9. A method for preparing an antibacterial dressing containing copper ions according to any one of claims 1 to 8, characterized in that: The following steps are involved: The calcium alginate fibers are cut to form short fibers, and the short fibers are opened and then mixed with cotton; the mixed fibers are combed into a fiber web A, and then needle-punched to form a calcium alginate non-woven dressing layer A; The copper alginate fibers are cut to form short fibers, the short fibers are opened and then mixed with cotton; and the mixed fibers are combed into a fiber web B; The copper alginate fiber mesh B is evenly laid on the surface of the calcium alginate non-woven fabric dressing layer A to form a dressing layer B, which is then acupunctured, cut, packaged, disinfected and sterilized to obtain the dressing layer B.

10. The method for preparing an antibacterial dressing containing copper ions according to claim 9, characterized in that: The preparation method of the dressing layer B comprises the following steps: The copper alginate fiber and the modified bamboo fiber are cut into short fibers respectively, the copper alginate short fibers are mixed with the modified bamboo fiber short fibers, and then loosened and blended with cotton; the blended fibers are combed into a fiber web, and then needle-punched to form a copper alginate composite non-woven fabric dressing layer B.