Carbon dioxide absorbent and preparation method thereof
By using nanoparticles in carbon dioxide absorbers to combine polyorganic amines with organic silicon compounds onto the surface of silica, the problems of high energy consumption and poor thermal stability of existing absorbers are solved, and more efficient carbon dioxide absorption and low energy are achieved Regeneration is used to improve the overall performance of the absorbent.
Patent Information
- Application Number
- CN202411180842.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing carbon dioxide absorbers have high energy consumption and poor thermal stability during the regeneration process, which limits their further promotion and application in carbon dioxide capture technology.
The carbon dioxide absorber formed by combining nanoparticles with organic silicon compounds onto the surface of silica nanoparticles by using nanoparticles. The preparation method includes preparing a nanosilicon dioxide suspension, mixing it with the organic silicon compound, and reacting with the polyorganic amine. , a modified silica colloidal suspension is formed, and the component ratio and reaction conditions are optimized to improve absorption effect and regeneration efficiency.
A good carbon dioxide absorption effect and reduction of regeneration energy consumption have been achieved, the liquid-rich load and the liquid-leading load have been improved, and the overall performance has been significantly improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon dioxide capture, and in particular to a carbon dioxide absorbent and a preparation method thereof. Background Art
[0002] Carbon dioxide is one of the important causes of global warming. The Intergovernmental Panel on Climate Change of the United Nations proposed that the global average temperature increase should not exceed 2°C by 2050, and the corresponding carbon dioxide emissions should be reduced by 50%. In order to cope with the impact of carbon dioxide emissions on global climate change, a large number of carbon reduction technologies have emerged, among which carbon capture, utilization and storage have become one of the research focuses of carbon reduction technology due to its large-scale emission reduction and obvious emission reduction benefits.
[0003] The most critical step in carbon capture technology is the capture of carbon dioxide. Carbon dioxide capture technology can be divided into pre-combustion capture, oxygen-enriched combustion and post-combustion capture. Post-combustion carbon dioxide capture technology mainly includes adsorption, absorption, membrane separation, deep cooling and other methods. From the perspective of industrial practicality, the use of absorbent-based chemical absorption to absorb carbon dioxide in flue gas after combustion has the advantages of fast absorption rate and large absorption capacity. It is one of the most commercially promising carbon dioxide capture technologies. However, the absorbent currently used in this technology has disadvantages such as instability, corrosiveness and high regeneration energy consumption, which limits its further promotion and application.
[0004] In addition, there are other carbon dioxide capture technologies such as solid adsorption, membrane separation and low-temperature distillation, but more research and exploration are still needed before large-scale application. Therefore, from the perspective of absorbent development, it is an urgent problem to quickly identify and design efficient, energy-saving and environmentally friendly carbon dioxide absorbents. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of high regeneration energy consumption and poor thermal stability of the carbon dioxide absorbent in the prior art, and to provide a new carbon dioxide absorbent and a preparation method thereof. The carbon dioxide absorbent has good carbon dioxide absorption effect, low regeneration energy consumption and good overall performance.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a carbon dioxide absorber, which contains nanoparticles, wherein the nanoparticles are particles formed by the bonding of a polyvalent organic amine to the surface of a silica nanoparticle via an organic silicon compound, wherein the organic silicon compound has an organic silicon functional group -SiR3 and an organic acid functional group, and the three Rs are each a hydroxyl group or a C1-C6 alkyl group.
[0007] Preferably, the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(1.5-20):(2-20), and more preferably 1:(3-18):(3-20).
[0008] Preferably, the organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid.
[0009] Preferably, the polyvalent organic amine is at least one of C2-C12 alkyldiamine, C2-C12 alkylenediamine, C2-C12 alkylenetriamine, C2-C12 alkylenetetramine, C2-C12 alkylenepentamine and C6-C18 aryldiamine; more preferably, it is at least one of 1,4-butanediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylenepentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine.
[0010] A second aspect of the present invention provides a method for preparing the carbon dioxide absorbent as described above, the method comprising the following steps: (1) Preparation of nano-silicon dioxide suspension; (2) mixing the nano-silicon dioxide suspension with an organosilicon compound to obtain a modified silica colloidal suspension; (3) mixing the modified silica colloidal suspension with a polyvalent organic amine for reaction; The organosilicon compound has an organosilicon functional group -SiR3 and an organic acid functional group, and the three Rs are each a hydroxyl group or a C1-C6 alkyl group.
[0011] Preferably, the mass ratio of the nano-silicon dioxide suspension, calculated as silicon dioxide, the organosilicon compound and the polyamine is 1:(1.5-20):(2-20), and more preferably 1:(3-18):(3-20).
[0012] Preferably, the organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid.
[0013] Preferably, the polyvalent organic amine is at least one of C2-C12 alkyldiamine, C2-C12 alkylenediamine, C2-C12 alkylenetriamine, C2-C12 alkylenetetramine, C2-C12 alkylenepentamine and C6-C18 aryldiamine, preferably at least one of 1,4-butylenediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylenepentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine.
[0014] Preferably, in step (1), the process of preparing the nano-silicon dioxide suspension comprises: mixing silica sol with water.
[0015] Preferably, in step (2), the reaction conditions include: pH value of 4-8, more preferably 5-7; temperature of 40-80°C, more preferably 50-70°C; time of 4-48h, more preferably 6-42h.
[0016] Preferably, in step (2), the process of preparing the modified silica colloidal suspension comprises: mixing the nano-silica suspension with an aqueous solution of an organosilicon compound, adjusting the pH value of the resulting mixture to 4-8, then reacting, dialyzing the reaction mixture, and then treating the dialyzed liquid using an ion exchange resin.
[0017] Preferably, in step (2), the molecular weight cutoff of the dialysis membrane used in the dialysis process is 2000-5000, preferably 3000-4000.
[0018] Preferably, in step (3), the polyamine is used in the form of an aqueous solution, and the concentration of the aqueous solution of the polyamine is 10-50 wt %.
[0019] According to the carbon dioxide absorbent of the present invention, the polyvalent organic amine is bonded (chemically bonded) to the surface of the silicon dioxide nanoparticles through an organic silicon compound, so that the carbon dioxide absorbent has a better carbon dioxide absorption effect and lower regeneration energy consumption than a simple alcohol amine absorbent. Specifically, in the process of carbon dioxide absorption and desorption, the use of the carbon dioxide absorbent of the present invention can obtain a higher rich liquid load and a lower lean liquid load. DETAILED DESCRIPTION
[0020] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] The carbon dioxide absorbent of the present invention contains nanoparticles, which are particles formed by combining a polyvalent organic amine with the surface of a silicon dioxide nanoparticle via an organic silicon compound, wherein the organic silicon compound has an organic silicon functional group -SiR3 and an organic acid functional group, and the three Rs are each a hydroxyl group or a C1-C6 alkyl group.
[0023] In the carbon dioxide absorbent of the present invention, preferably, the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyamine is 1:(1.5-20):(2-20), more preferably 1:(3-18):(3-20); more preferably 1:(5-15):(6-18). The carbon dioxide absorbent according to the above composition ratio has significantly better carbon dioxide absorption effect, lower regeneration energy consumption and better overall performance.
[0024] In the carbon dioxide absorber described in the present invention, in a preferred case, the organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid, and triisopropylsilyltrifluoromethanesulfonic acid is most preferred.
[0025] In the carbon dioxide absorbent of the present invention, the polyvalent organic amine may be at least one of C2-C12 alkyl diamines, C2-C12 alkylene diamines, C2-C12 alkylene triamines, C2-C12 alkylene tetraamines, C2-C12 alkylene pentamines and C6-C18 aryl diamines. In a preferred embodiment, the polyvalent organic amine is at least one of 1,4-butanediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylene pentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine. In a more preferred embodiment, the polyvalent organic amine is at least one of 1,5-pentanediamine, 1,8-diaminooctane, 1,4-butanediamine and triethylenetetramine.
[0026] In the carbon dioxide absorbent of the present invention, preferably, the silicon dioxide nanoparticles are provided by silica sol.
[0027] In some embodiments, the silicon dioxide nanoparticles are provided by silica sol, the organosilicon compound is 3-(trihydroxysilyl)-1-propanesulfonic acid, the polyvalent organic amine is tetraethylenepentamine, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0028] In other embodiments, the silicon dioxide nanoparticles are provided by silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,8-diaminooctane, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0029] In other embodiments, the silicon dioxide nanoparticles are provided by silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,4-butanediamine, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0030] In other embodiments, the silicon dioxide nanoparticles are provided by silica sol, the organosilicon compound is 3-(trimethylsilyl) propiolic acid, the polyvalent organic amine is triethylenetetramine, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0031] In other embodiments, the silicon dioxide nanoparticles are provided by silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,5-pentanediamine, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0032] The preparation method of the carbon dioxide absorbent of the present invention comprises: (1) Preparation of nano-silicon dioxide suspension; (2) mixing the nano-silicon dioxide suspension with an organosilicon compound to obtain a modified silica colloidal suspension; (3) mixing the modified silica colloidal suspension with a polyvalent organic amine for reaction; The organosilicon compound has an organosilicon functional group -SiR3 and an organic acid functional group, and the three Rs are each a hydroxyl group or a C1-C6 alkyl group.
[0033] In the method of the present invention, the mass ratio of the nano-silicon dioxide suspension, the organosilicon compound and the polyamine can be 1:(1.5-20):(2-20), preferably 1:(3-18):(3-20), and more preferably 1:(5-15):(6-18). The carbon dioxide absorbent prepared according to the above dosage ratio has a significantly better carbon dioxide absorption effect, lower regeneration energy consumption and better overall performance.
[0034] In the method described in the present invention, in a preferred case, the organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid, and most preferably triisopropylsilyltrifluoromethanesulfonic acid.
[0035] In the method of the present invention, the polyvalent organic amine may be at least one of C2-C12 alkyl diamine, C2-C12 alkylene diamine, C2-C12 alkylene triamine, C2-C12 alkylene tetramine, C2-C12 alkylene pentamine and C6-C18 aryl diamine. In a preferred embodiment, the polyvalent organic amine is at least one of 1,4-butanediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylenepentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine. In a more preferred embodiment, the polyvalent organic amine is at least one of 1,5-pentanediamine, 1,8-diaminooctane, 1,4-butanediamine and triethylenetetramine.
[0036] In some embodiments, the silicon source for preparing the nano-silicon dioxide suspension is silica sol, the organosilicon compound is 3-(trihydroxysilyl)-1-propane sulfonic acid, the polyvalent organic amine is tetraethylenepentamine, and the mass ratio of the nano-silicon dioxide suspension to the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18) based on silicon dioxide. The carbon dioxide absorbent prepared according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0037] In other embodiments, the silicon source for preparing the nano-silicon dioxide suspension is silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,8-diaminooctane, and the mass ratio of the silicon dioxide nanoparticles, the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18). The carbon dioxide absorbent prepared according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0038] In other embodiments, the silicon source for preparing the nano-silicon dioxide suspension is silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,4-butanediamine, and the mass ratio of the nano-silicon dioxide suspension to the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18) based on silicon dioxide. The carbon dioxide absorbent prepared according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0039] In other embodiments, the silicon source for preparing the nano-silicon dioxide suspension is silica sol, the organosilicon compound is 3-(trimethylsilyl) propiolic acid, the polyvalent organic amine is triethylenetetramine, and the mass ratio of the nano-silicon dioxide suspension to the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18) based on silicon dioxide. The carbon dioxide absorbent prepared according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0040] In other embodiments, the silicon source for preparing the nano-silicon dioxide suspension is silica sol, the organosilicon compound is triisopropylsilyl trifluoromethanesulfonic acid, the polyvalent organic amine is 1,5-pentanediamine, and the mass ratio of the nano-silicon dioxide suspension to the organosilicon compound and the polyvalent organic amine is 1:(5-15):(6-18) based on silicon dioxide. The carbon dioxide absorbent prepared according to this embodiment has a good carbon dioxide absorption effect, low regeneration energy consumption, and better overall performance.
[0041] In the method of the present invention, in step (1), the process of preparing the nano-silicon dioxide suspension can be implemented in a conventional manner in the art, and the silicon source used can be a conventional silicon source in the art. In a preferred embodiment, the process of preparing the nano-silicon dioxide suspension includes: mixing silica sol with water. Further preferably, the mass volume ratio of the amount of silica sol to water is (1-20g):100mL, more preferably (2-15g):100mL, and further preferably (3-10g):100mL.
[0042] In the present invention, the particle size of the silica sol may be 1-200 nm, preferably 5-100 nm, and more preferably 10-50 nm. The silica sol may be a commercially available silica sol product, such as Grace LUDOX HS-30 silica sol.
[0043] In the method described in the present invention, in step (2), the reaction conditions may include: pH value of 4-8, preferably 5-7; temperature of 40-80°C, preferably 50-70°C; time of 4-48h, preferably 6-42h.
[0044] In the method of the present invention, in step (2), the preparation process of the modified silica colloidal suspension preferably includes: mixing the nano-silica suspension with an aqueous solution of an organosilicon compound, adjusting the pH value of the resulting mixture to 4-8, then reacting, dialyzing the reaction mixture, and then treating the dialyzed liquid using an ion exchange resin.
[0045] In the present invention, the molecular weight cutoff (MWCO) of the dialysis membrane used in the dialysis process may be 2000-5000, more preferably 3000-4000, most preferably 3200-3600. The dialysis time is preferably 10-48 hours, more preferably 12-24 hours.
[0046] In the present invention, the purpose of using the ion exchange resin for treatment is to remove Na + Ions. The ion exchange resin may be an ion exchange resin that can remove Na+ that is commonly used in the art. In a specific embodiment, the ion exchange resin is an HCR-W2 type ion exchange resin.
[0047] In the method of the present invention, in step (3), the polyamine is used in the form of an aqueous solution, and the concentration of the aqueous solution of the polyamine is preferably 10-50wt%, more preferably 20-40wt%.
[0048] In the method of the present invention, in step (3), the reaction can be carried out at room temperature. In a preferred embodiment, the operation process of the mixed reaction of the modified silica colloidal suspension and the polyvalent organic amine comprises: dropping the aqueous solution of the polyvalent organic amine into the modified silica colloidal suspension and reacting under stirring. The reaction time can be 10-48 hours, preferably 12-24 hours.
[0049] The carbon dioxide absorbent obtained by the preparation method of the present invention has a higher rich liquid load and a lower lean liquid load under the same absorption and desorption conditions, a better carbon dioxide absorption effect, lower regeneration energy consumption, and better overall performance.
[0050] The carbon dioxide absorbent and its preparation method of the present invention are further described by examples. The examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.
[0051] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.
[0052] Example 1 (1) Add 1.5 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0053] (2) Dissolve 15g of triisopropylsilyl trifluoromethanesulfonic acid (purchased from Shanghai Aladdin Reagent Company) in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate with 1mol / L NaOH solution to a pH value of 5. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Company, brand DOWEXHCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0054] (3) 27 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 35 wt% aqueous solution. The prepared 1,5-pentanediamine aqueous solution was added dropwise to the modified silica colloidal suspension and stirred for 24 hours to obtain the carbon dioxide absorber A1 of the present invention.
[0055] Example 2 (1) Add 2.7 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0056] (2) Dissolve 13.5 g of triisopropylsilyl trifluoromethanesulfonic acid (purchased from Shanghai Aladdin Reagent Company) in 100 ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate with 1 mol / L NaOH solution to a pH of 6. React at 60°C for 20 hours. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24 hours. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Company, brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0057] (3) 27 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 35 wt% aqueous solution. The prepared 1,5-pentanediamine aqueous solution was added dropwise to the modified silica colloidal suspension, and the mixture was stirred for 24 h to obtain the carbon dioxide absorbent A2 of the present invention.
[0058] Example 3 (1) Add 4.5 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silicon dioxide suspension.
[0059] (2) Dissolve 67.5g of triisopropylsilyl trifluoromethanesulfonic acid (purchased from Shanghai Aladdin Reagent Co., Ltd.) in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate to pH 7 with 1mol / L NaOH solution. React at 70°C for 18h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Co., Ltd., brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0060] (3) 27 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 35 wt% aqueous solution. The prepared 1,5-pentanediamine aqueous solution was added dropwise to the modified silica colloidal suspension, and the mixture was stirred for 24 h to obtain the carbon dioxide absorbent A3 of the present invention.
[0061] Example 4 (1) Add 4 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0062] (2) Dissolve 12g of triisopropylsilyl trifluoromethanesulfonic acid (purchased from Shanghai Aladdin Reagent Company) in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate with 1mol / L NaOH solution to a pH value of 5. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Company, brand DOWEXHCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0063] (3) 21.42 g of 1,4-butanediamine was added to 50 ml of water to prepare a 30 wt% aqueous solution. The prepared 1,4-butanediamine aqueous solution was added dropwise to the modified silica colloidal suspension and stirred for 24 hours to obtain the carbon dioxide absorbent A4 of the present invention.
[0064] Example 5 (1) Add 3 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0065] (2) Dissolve 8g of triisopropylsilyl trifluoromethanesulfonic acid (purchased from Shanghai Aladdin Reagent Company) in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate with 1mol / L NaOH solution to a pH value of 5. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Company, brand DOWEXHCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0066] (3) Take 21.42 g of 1,8-diaminooctane and add it to 50 ml of water to prepare a 30 wt% aqueous solution. The prepared 1,8-diaminooctane aqueous solution is added dropwise to the modified silica colloidal suspension, and the reaction is stirred for 24 hours to obtain the carbon dioxide absorber A5 of the present invention.
[0067] Example 6 The carbon dioxide absorbent was prepared according to the method of Example 1, except that the polyvalent organic amine used was diethylenetriamine (purchased from Shanghai Aladdin Company), thereby obtaining the carbon dioxide absorbent A6 of the present invention.
[0068] Example 7 A carbon dioxide absorbent was prepared according to the method of Example 1, except that the polyvalent organic amine used was triethylenetetramine (purchased from Shanghai Aladdin Company), thereby obtaining the carbon dioxide absorbent A7 of the present invention.
[0069] Example 8 The carbon dioxide absorbent was prepared according to the method of Example 1, except that the organosilicon compound used was 3-trihydroxysilylpropylmethylphosphonic acid (purchased from Shanghai Aladdin Reagent Company), thereby obtaining the carbon dioxide absorbent A8 of the present invention.
[0070] Example 9 (1) Add 5 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silicon dioxide suspension.
[0071] (2) Dissolve 10g of 3-(trihydroxysilyl)-1-propanesulfonic acid (purchased from Beijing Bailingwei Technology Co., Ltd.) in 100ml of deionized water, mix the nano-silica suspension obtained in step (1) with the aqueous solution of 3-(trihydroxysilyl)-1-propanesulfonic acid, and titrate with 1mol / L NaOH solution to a pH value of 5. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Co., Ltd., brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0072] (3) 21.42 g of tetraethylenepentamine was added to 50 ml of water to prepare a 30 wt% aqueous solution. The prepared tetraethylenepentamine aqueous solution was added dropwise to the modified silica colloidal suspension, and the mixture was stirred for 24 h to obtain the carbon dioxide absorbent A9 of the present invention.
[0073] Example 10 (1) Add 2 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0074] (2) Dissolve 15g of 3-(trimethylsilyl)propiolic acid in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of 3-(trimethylsilyl)propiolic acid, and titrate with 1mol / L NaOH solution to a pH of 5. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Co., Ltd., brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0075] (3) 33.34 g of triethylenetetramine was added to 50 ml of water to prepare a 40 wt% aqueous solution. The prepared triethylenetetramine aqueous solution was added dropwise to the modified silica colloidal suspension and stirred for 24 hours to obtain the carbon dioxide absorbent A10 of the present invention.
[0076] Embodiment 11 (1) Add 1 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0077] (2) Dissolve 1g of triisopropylsilyl trifluoromethanesulfonic acid in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate to pH 5 with 1mol / L NaOH solution. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Co., Ltd., brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0078] (3) 30 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 37.5 wt % aqueous solution. The prepared 1,5-pentanediamine aqueous solution was added dropwise to the modified silica colloidal suspension, and the mixture was stirred for 24 h to obtain the carbon dioxide absorbent A11 of the present invention.
[0079] Example 12 (1) Add 1 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0080] (2) Dissolve 22g of triisopropylsilyl trifluoromethanesulfonic acid in 100ml of deionized water, mix the nanosilica suspension obtained in step (1) with the aqueous solution of triisopropylsilyl trifluoromethanesulfonic acid, and titrate to pH 5 with 1mol / L NaOH solution. React at 50°C for 24h. Then use a dialysis membrane with a molecular weight cutoff of 3500 (purchased from Thermo Fisher Scientific) to dialyze the mixture after the above reaction in deionized water for 24h. Use HCR-W2 ion exchange resin (purchased from Shanghai Anpu Laboratory Co., Ltd., brand DOWEX HCR-W2, 16-40 mesh) to remove Na + ions to obtain a modified silica colloidal suspension.
[0081] (3) 1.5 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 3 wt % aqueous solution, and the prepared 1,5-pentanediamine aqueous solution was added dropwise to the modified silica colloidal suspension, and the reaction was stirred for 24 hours to obtain the carbon dioxide absorber A12 of the present invention.
[0082] Comparative Example 1 30 g of ethanolamine (purchased from Shanghai Aladdin Reagent Company) and 70 g of deionized water were mixed to obtain a 30 wt % ethanolamine aqueous solution as the carbon dioxide absorbent D1 for comparative experiments.
[0083] Comparative Example 2 The carbon dioxide absorbent was prepared according to the method of Example 1, except that the modification process of step (2) was not performed. The specific process is as follows: (1) Add 1.5 g of Grace LUDOX HS-30 silica sol (particle size 10-20 nm) into 100 ml of deionized water and disperse evenly to obtain a nano-silica suspension.
[0084] (2) 27 g of 1,5-pentanediamine was added to 50 ml of water to prepare a 35 wt% aqueous solution. The prepared 1,5-pentanediamine aqueous solution was added dropwise to the nano-silicon dioxide suspension, and the mixture was stirred for 24 hours to obtain a carbon dioxide absorbent D2.
[0085] Test Example 1 The rich liquid loading amount and the lean liquid loading amount of the carbon dioxide absorbent prepared in Examples 1-12 and Comparative Examples 1-2 were tested respectively, and the testing method was as follows: (1) The prepared carbon dioxide absorbent was placed in a constant temperature water bath at 40°C, and a mixture of carbon dioxide and nitrogen with a CO2 concentration of 13% was introduced at a gas flow rate of 1L / min, and the reaction was continued for 180 minutes. The product was then titrated with sulfuric acid to determine the carbon dioxide loading in the product, which was the loading of the absorbent rich liquid.
[0086] (2) Use a laboratory carbon dioxide desorption device to conduct a desorption experiment on the above absorption reaction product. Take 100g of the product and put it into a three-necked flask, insert a thermometer and a condenser, and connect the outlet of the condenser to a flowmeter. After the three-necked flask is sealed, it is placed in an oil bath at 100°C, and the flow rate of the desorbed gas is monitored in real time using a flowmeter. After 90 minutes of reaction, the liquid product after desorption is titrated with sulfuric acid to determine the carbon dioxide loading in the product. The value is the absorbent lean liquid loading. Among them, the flowmeter used is a MEMS four-in-one mass flowmeter purchased from Siargo, USA.
[0087] The test results of the rich liquid loading and lean liquid loading of the carbon dioxide absorbents prepared in Examples 1-12 and Comparative Examples 1-2 are shown in Table 1, wherein the absorbent circulating loading is the value of the absorbent rich liquid loading minus the absorbent lean liquid loading.
[0088] Table 1
[0089] From the results in Table 1, it can be seen that the carbon dioxide absorbent of the present invention has a higher rich liquid load and a lower lean liquid load under the same absorption and desorption conditions, and its circulation load is higher, and the effect of capturing carbon dioxide is better. At the same time, the carbon dioxide absorbent of the present invention has a lower lean liquid load at the same desorption temperature, so the carbon dioxide absorbent also has the advantage of low regeneration energy consumption.
[0090] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A carbon dioxide absorbent, characterized in that: The carbon dioxide absorbent contains nanoparticles, wherein the nanoparticles are particles formed by combining a polyvalent organic amine with the surface of a silicon dioxide nanoparticle through an organic silicon compound, wherein the organic silicon compound has an organic silicon functional group -SiR3 and an organic acid functional group, and three Rs are respectively hydroxyl groups or C1-C6 alkyl groups.
2. The carbon dioxide absorbent according to claim 1, characterized in that The mass ratio of the silicon dioxide nanoparticles, the organic silicon compound and the polyvalent organic amine is 1:(1.5-20):(2-20), preferably 1:(3-18):(3-20).
3. The carbon dioxide absorbent according to claim 1 or 2, characterized in that The organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid.
4. The carbon dioxide absorbent according to any one of claims 1 to 3, characterized in that The polyvalent organic amine is at least one of C2-C12 alkyldiamines, C2-C12 alkylenediamines, C2-C12 alkylenetriamines, C2-C12 alkylenetetramines, C2-C12 alkylenepentamines and C6-C18 aryldiamines, preferably at least one of 1,4-butylenediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylenepentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine.
5. A method for preparing a carbon dioxide absorbent, characterized in that: The method comprises the following steps: (1) Preparation of nano-silicon dioxide suspension; (2) mixing the nano-silicon dioxide suspension with an organosilicon compound to obtain a modified silica colloidal suspension; (3) mixing the modified silica colloidal suspension with a polyvalent organic amine for reaction; The organosilicon compound has an organosilicon functional group -SiR3 and an organic acid functional group, and the three Rs are each a hydroxyl group or a C1-C6 alkyl group.
6. The method according to claim 5, characterized in that The mass ratio of the nano-silicon dioxide suspension, calculated as silicon dioxide, the organic silicon compound and the polyvalent organic amine is 1:(1.5-20):(2-20), preferably 1:(3-18):(3-20).
7. The method according to claim 5 or 6, characterized in that: The organosilicon compound is at least one of 3-(trihydroxysilyl)-1-propanesulfonic acid, 3-(trimethylsilyl)propiolic acid, triisopropylsilyltrifluoromethanesulfonic acid and 3-trihydroxysilylpropylmethylphosphonic acid.
8. The method according to claim 5 or 6, characterized in that: The polyvalent organic amine is at least one of C2-C12 alkyldiamines, C2-C12 alkylenediamines, C2-C12 alkylenetriamines, C2-C12 alkylenetetramines, C2-C12 alkylenepentamines and C6-C18 aryldiamines, preferably at least one of 1,4-butylenediamine, 1,5-pentanediamine, 1,8-diaminooctane, tetraethylenepentamine, triethylenetetramine, diethylenetriamine and triethylenetetramine.
9. The method according to any one of claims 5 to 8, characterized in that: In step (1), the process of preparing the nano-silicon dioxide suspension includes: mixing silica sol with water.
10. The method according to any one of claims 5 to 9, characterized in that: In step (2), the reaction conditions include: pH value of 4-8, preferably 5-7; temperature of 40-80°C, preferably 50-70°C; time of 4-48h, preferably 6-42h.
11. The method according to any one of claims 5 to 9, characterized in that: In step (2), the process of preparing the modified silica colloidal suspension comprises: mixing the nano silica suspension with an aqueous solution of an organosilicon compound, adjusting the pH value of the resulting mixture to 4-8, then reacting, dialyzing the reaction mixture, and then treating the dialyzed liquid with an ion exchange resin; Preferably, the molecular weight cutoff of the dialysis membrane used in the dialysis process is 2000-5000, preferably 3000-4000.
12. The method according to any one of claims 5 to 9, characterized in that: In step (3), the polyamine is used in the form of an aqueous solution, and the concentration of the aqueous solution of the polyamine is 10-50 wt %.
13. A carbon dioxide absorbent prepared by the method according to any one of claims 5 to 12.
Citation Information
Patent Citations
Composite adsorbent, and preparation method and application thereof
CN104475060A
Regenerative adsorbents of modified amines on nano-structured supports
CN106660010A
Modified silicon dioxide adsorbent for capturing medium-low-concentration carbon dioxide
CN115228426A
Carbon dioxide absorbent and application thereof
CN118341227A
Cited By
Carbon dioxide absorbent, preparation method thereof and carbon dioxide trapping method
CN120838130A
Carbon dioxide absorbent, method for producing the same, and method for capturing carbon dioxide
CN120838130B