Catalytic functionalized roll type micro-filtration membrane element as well as preparation method and application thereof
By introducing zero-valent nickel catalytic particles and cation exchange functional functional groups in membrane separation technology, the problems of low efficiency and high energy consumption of toxic organic compounds in the prior art are solved, and a high efficiency and low cost chlorobenzene conversion rate is achieved. , suitable for industrial production.
Patent Information
- Application Number
- CN202411209846.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
Existing membrane separation technology cannot completely deal with the intercepted toxic organic matter or heavy metal ions, and the high-temperature oxidation technology of catalytic films has problems of exposure risks and high energy consumption.
The catalytic functional rolled microfiltration membrane element is adopted to achieve the reduction and conversion of chlorine-containing organic matter by growing zero-valent nickel catalytic particles inside the membrane element and grafting reaction containing cation exchange functional functional groups and reducing agents.
Under mild conditions, efficient reduction and conversion of chlorine-containing organic matter is achieved, which reduces operating pressure and energy consumption, avoids secondary pollution, and is suitable for industrial production.
Smart Images

Figure CN119075686A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution control, and in particular relates to a catalytic functionalized rolled microfiltration membrane element and a preparation method and application thereof. Background Art
[0002] Membrane separation technology has attracted much attention due to its high selectivity, ease of operation and no phase change. By screening different pore sizes and surface charge properties, it can intercept a variety of organic matter and inorganic heavy metal ions, and is widely used in water pollution control and high-value product separation. However, membrane separation technology cannot completely treat the intercepted toxic organic matter or heavy metal ions, and often needs to be coupled with other degradation technologies to achieve complete degradation of pollutants. This process increases the complexity of the process and requires additional energy consumption and carbon emissions.
[0003] Chlorinated organic matter is a common toxic pollutant in industrial wastewater. Due to its small molecular size, it often requires a dense membrane material (nanofiltration membrane or reverse osmosis membrane) to achieve effective interception, resulting in the treatment process requiring a higher operating pressure to overcome the mass transfer resistance (0.5-7MPa) caused by the dense structure; at the same time, if the intercepted pollutants are not subsequently degraded, they are prone to secondary pollution. In contrast, microfiltration membranes with larger pore sizes have a small mass transfer resistance and show better screening effects on suspended matter and bacterial interception, but they cannot effectively intercept small molecular organic matter and ions. Therefore, the coupling of membrane separation with other degradation technologies has attracted widespread attention, especially the research on the integration of membrane separation and degradation technology. However, at present, catalytic membranes mainly achieve organic degradation by catalyzing advanced oxidation degradation and producing singlet oxygen. For example, Chinese patents (CN116283359A, CN115999546A, CN115608403A, CN117643806) disclose a wastewater treatment method using catalytic membrane activated persulfate. This method will cause halogenated hydrocarbons to oxidize and degrade into small molecular halogenated hydrocarbons, increasing exposure risks. At the same time, most of these oxidation technologies involve high-temperature calcination modification (250°C to 700°C). Summary of the invention
[0004] The purpose of the embodiments of the present invention is to provide a catalytically functionalized rolled microfiltration membrane element, aiming to solve the problems raised in the above-mentioned background technology.
[0005] The embodiment of the present invention is implemented as follows: a catalytically functionalized rolled microfiltration membrane element, wherein zero-valent nickel catalytic particles grow inside the membrane element, and the size of the zero-valent nickel catalytic particles is 10 to 200 nm.
[0006] Another object of the present invention is to provide a method for preparing a catalytically functionalized spiral microfiltration membrane element, comprising the following steps:
[0007] Rinse the rolled microfiltration membrane element and let air in to dry out excess moisture inside;
[0008] Mixing a monomer containing a cation exchange functional group, an initiator, a cross-linking agent, a pH regulator and water, injecting the mixed solution into a spiral microfiltration membrane element at low pressure, and collecting the permeate for reuse;
[0009] The wound microfiltration membrane element wetted by the mixed solution is heated to complete the thermally induced free radical polymerization reaction;
[0010] The solution containing nickel ions and the solution containing a reducing agent are sequentially introduced into the polymerized spiral microfiltration membrane element to complete the catalytic functionalization of the spiral microfiltration membrane element.
[0011] Preferably, the membrane material of the spiral microfiltration membrane element is polysulfone.
[0012] Preferably, the monomer containing a cation exchange functional group is one or more of 3-pentenoic acid, 5-hexenoic acid, vinyl acetic acid, and allyl acetic acid;
[0013] The initiator is one or more of sodium persulfate and ammonium persulfate;
[0014] The cross-linking agent is one or more of 1,3-dimethylguanidine diisocyanate and N-methyl-N'-oxy-4-bromoaniline;
[0015] The pH regulator is one or more of sodium hydroxide and potassium hydroxide.
[0016] Preferably, the mass ratio of the monomer containing cation exchange functional groups, the initiator, the cross-linking agent and water is 1-2: 0.02-0.1: 0.01-0.05:10.
[0017] Preferably, the mass ratio of the monomer containing cation exchange functional groups, the initiator and the cross-linking agent is 1:0.02-0.05:0.01-0.025.
[0018] Preferably, the pH value of the mixed solution is 8-10, and the pressure of the mixed solution when injected into the spiral microfiltration membrane element at low pressure flow is 0.05-0.2 MPa.
[0019] Preferably, the temperature of the thermal free radical polymerization reaction is 40-50° C., and the time is 2-8 hours.
[0020] Preferably, the solution containing nickel ions is one or more of nickel chloride, nickel nitrate, nickel sulfate, and nickel carbonate, with a concentration of 0.5 to 2 g / L;
[0021] The solution containing the reducing agent is tea polyphenol, the concentration ratio between the solution containing nickel ions and the solution containing the reducing agent is 1:1.5-3.5, and the injection pressure is 0.25-0.4 MPa.
[0022] Another object of the embodiments of the present invention is to provide a catalytically functionalized spiral microfiltration membrane element for use in catalytic conversion of chlorine-containing organic matter.
[0023] A catalytically functionalized rolled microfiltration membrane element provided in an embodiment of the present invention can be grafted with a functional group containing a cation exchange function in the membrane pores of the membrane element by injecting a mixed solution including a monomer containing a cation exchange functional group, an initiator, a cross-linking agent, a pH regulator, etc. into the rolled microfiltration membrane element to perform thermally initiated free radical polymerization, thereby achieving subsequent capture of nickel ions; and then successively passing a solution containing nickel ions and a reducing agent into the membrane element to complete the conversion of nickel ions into zero-valent nickel catalytic particles, thereby achieving the growth of zero-valent nickel catalytic particles inside the membrane element;
[0024] The embodiment of the present invention breaks through the traditional complicated process of first making a membrane and then assembling it into a membrane element. The mixed solution to be polymerized, the nickel ion solution and the reducing agent solution can be directly passed into the membrane element without disassembling the membrane element, thereby completing the grafting of functional groups containing cation exchange functions, the exchange of nickel ions, and the growth of zero-valent nickel catalytic particles under mild conditions. The method is simple to operate, low in cost, and has little environmental pollution, and is suitable for industrial production.
[0025] The prepared catalytically functionalized membrane component has the ability to reduce and convert chlorine-containing organic matter, and can achieve a 98% conversion rate of chlorobenzene within a residence time of just 4 seconds. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A flow chart of a method for preparing a catalytically functionalized spiral microfiltration membrane element provided in an embodiment of the present invention;
[0027] Figure 2 This is a SEM image of catalytic particles in the internal pores of the catalytically functionalized spiral microfiltration membrane element provided in Example 1 of the present invention;
[0028] Figure 3 This is a test chart of chlorobenzene conversion rate of the spiral microfiltration membrane element provided in Examples 1-7 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0030] A catalytically functionalized spiral microfiltration membrane element, the preparation process of which is as follows Figure 1 As shown, the specific steps include:
[0031] (1) Select a commercially available spiral microfiltration membrane element with a size of 4080 or 8040 and a membrane material of polysulfone, rinse it, and blow air through it to dry the excess water inside;
[0032] (2) Mixing a monomer containing a cation exchange functional group (one or more of 3-pentenoic acid, 5-hexenoic acid, vinyl acetic acid, and allyl acetic acid), an initiator (one or more of sodium persulfate and ammonium persulfate), a crosslinking agent (one or more of 1,3-dimethylguanidine diisocyanate and N-methyl-N'-oxo-4-bromoaniline), a pH adjuster (one or more of sodium hydroxide and potassium hydroxide) and water (the mass ratio of the monomer, the initiator, the crosslinking agent and the water is 1-2: 0.02-0.1: 0.01-0.05: 10, and more preferably, the mass ratio of the monomer, the initiator and the crosslinking agent is 1: 0.02-0.05: 0.01-0.025), injecting the mixed solution into a spiral membrane element at a low pressure (0.05-0.2 MPa), and collecting the permeate for reuse; wherein the pH value of the mixed solution is 8-10;
[0033] (3) transferring the membrane element wetted with the mixed solution to an oven for heating to carry out thermally induced free radical polymerization at 40 to 50° C. for 2 to 8 hours;
[0034] (4) A nickel ion-containing solution (one or more of nickel chloride, nickel nitrate, nickel sulfate, and nickel carbonate, with a concentration of 0.5 to 2 g / L) and a tea polyphenol solution (the concentration ratio of the nickel ion-containing solution to the tea polyphenol solution is 1:1.5 to 3.5) are sequentially introduced into the polymerized membrane element to complete the catalytic functionalization of the membrane element.
[0035] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0036] Example 1: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0037] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0038] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 1:0.04:0.02:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0039] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0040] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 2.5 g / L were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0041] The catalytic functionalized spiral microfiltration membrane element prepared in Example 1 was analyzed by scanning electron microscope, and the SEM image of the internal catalytic particles was obtained as shown in the following figure: Figure 2 As shown, according to Figure 2 It can be seen that the average diameter of the zero-valent nickel catalytic particles in the membrane pores of the membrane element is 35.8 nm, and the size distribution is right-skewed, which is beneficial to increasing the specific surface area of the catalyst.
[0042] Example 2: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0043] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0044] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 1.5:0.06:0.03:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0045] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0046] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 2.5 g / L were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0047] Example 3: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0048] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0049] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 2:0.08:0.04:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0050] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0051] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 2.5 g / L were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0052] Example 4: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0053] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0054] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 2:0.08:0.05:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0055] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0056] (4) After cooling to room temperature, 1 g / L nickel sulfate and 2.5 g / L tea polyphenols were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0057] Example 5: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0058] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0059] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 2:0.08:0.03:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0060] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0061] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 2.5 g / L were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0062] Example 6: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0063] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0064] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 2:0.08:0.04:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0065] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0066] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 1.5 g / L were successively introduced into the polymerized membrane element at a pressure of 0.35 MPa, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0067] Example 7: A catalytically functionalized spiral microfiltration membrane element, the specific preparation method is as follows:
[0068] (1) Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040 and allow air to blow away excess moisture inside;
[0069] (2) mixing allyl acetic acid containing a cation exchange functional group, an initiator sodium persulfate, a cross-linking agent N-methyl-N'-oxo-4-bromoaniline and water in a mass ratio of 2:0.08:0.04:10, adding sodium hydroxide to adjust the solution pH to 9, passing the solution into a membrane element at a pressure of 0.15 MPa, and collecting the permeate for reuse;
[0070] (3) transferring the wetted membrane element to a 45°C oven and heating it for 6 h to perform thermally induced free radical polymerization;
[0071] (4) After cooling to room temperature, nickel sulfate with a concentration of 1 g / L and tea polyphenols with a pressure of 0.35 MPa were successively introduced into the polymerized membrane element, thereby completing the catalytic functionalization of the spiral microfiltration membrane element. Nitrogen was introduced into the catalytic functionalized membrane element for standby use.
[0072] Comparative Example 1: A commercially available rolled polysulfone microfiltration membrane element of size 4040 was rinsed and dried for later use.
[0073] Comparative Example 2: Rinse a commercially available rolled polysulfone microfiltration membrane element of size 4040, and allow air to blow dry excess moisture inside; stir and mix allyl acetic acid, a monomer containing a cation exchange functional group, sodium persulfate as an initiator, N-methyl-N'-oxo-4-bromoaniline, a cross-linking agent, and water in a mass ratio of 1:0.04:0.02:10, add sodium hydroxide to adjust the solution pH to 9, pass the solution into the membrane element at a pressure of 0.15 MPa, and collect the permeate for reuse; transfer the wetted membrane element to a 45°C oven and heat for 6 hours to perform thermally induced free radical polymerization; after cooling to room temperature, pass nitrogen into the polymerized membrane element for standby use.
[0074] Performance Test:
[0075] (1) Chlorobenzene, sodium dihydrogen phosphate, sodium chloride and humic acid were added to distilled water to simulate the actual water environment. The concentration of chlorobenzene in the obtained solution was 1 mg / L, the concentration of humic acid was 20 mg / L, the pH of the solution was 7.5, and the conductivity was 1200 μS / cm;
[0076] (2) The feed and discharge ports of the membrane element samples prepared in Examples 1 to 7 and Comparative Examples 1 to 2 were connected in sequence, and the above-mentioned solutions simulating the actual water environment were respectively introduced for testing. The test pressure was 0.2 MPa, and the purge and trap method and gas chromatography-mass spectrometry were used for quantitative testing. The results are as follows: Figure 3 shown.
[0077] according to Figure 3It can be seen from the data of Comparative Examples 1 to 2 that the commercial spiral microfiltration membrane element without the introduction of catalytic functionalization does not have the ability to treat chlorobenzene, and the free radical polymerization process completed in the membrane pores of the membrane element does not significantly improve the treatment capacity of chlorobenzene;
[0078] In Examples 1 to 7, catalytic ions are introduced by performing free radical polymerization, ion exchange, and in-situ reduction of nickel ions inside the membrane element, thereby having the ability to catalytically convert chlorine-containing organic matter (chlorobenzene). In Examples 3 and 4, the ratio of monomers containing cation exchange functional groups, initiators, cross-linking agents, and water is adjusted to obtain catalytic functionalized membrane elements with a removal rate of more than 98% for chlorobenzene within a residence time of 4 seconds, which has a significant advantage in removal rate compared to Comparative Examples 1 to 2.
[0079] It can be seen from the data of Examples 1 to 3 that the amount of allyl acetic acid introduced into the monomer containing a cation exchange functional group is a key factor in improving the conversion rate of chlorobenzene, and the optimal ratio within the range is 2:10 (monomer: water);
[0080] It can be seen from the data of Examples 3 to 5 that the amount of cross-linking agent used will partially affect the conversion rate, wherein when the ratio is 0.04 to 0.05:10 (cross-linking agent: water), the marginal benefit is not obvious.
[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A catalytically functionalized spiral microfiltration membrane element, It is characterized in that Zero-valent nickel catalytic particles grow inside the membrane element, and the size of the zero-valent nickel catalytic particles is 10-200 nm.
2. A method for preparing the catalytically functionalized spiral wound microfiltration membrane element according to claim 1, It is characterized in that The following steps are involved: Rinse the rolled microfiltration membrane element and let air in to dry out excess moisture inside; Mixing a monomer containing a cation exchange functional group, an initiator, a cross-linking agent, a pH regulator and water, injecting the mixed solution into a spiral microfiltration membrane element at low pressure, and collecting the permeate for reuse; The wound microfiltration membrane element wetted by the mixed solution is heated to complete the thermally induced free radical polymerization reaction; A solution containing nickel ions and a solution containing a reducing agent are sequentially introduced into the polymerized spiral microfiltration membrane element to complete the catalytic functionalization of the spiral microfiltration membrane element.
3. The preparation method according to claim 2, It is characterized in that The membrane material of the rolled microfiltration membrane element is polysulfone.
4. The preparation method according to claim 2, It is characterized in that The monomer containing a cation exchange functional group is one or more of 3-pentenoic acid, 5-hexenoic acid, vinyl acetic acid, and allyl acetic acid; The initiator is one or more of sodium persulfate and ammonium persulfate; The cross-linking agent is one or more of 1,3-dimethylguanidine diisocyanate and N-methyl-N'-oxy-4-bromoaniline; The pH regulator is one or more of sodium hydroxide and potassium hydroxide.
5. The preparation method according to claim 4, It is characterized in that The mass ratio of the monomer containing the cation exchange functional group, the initiator, the crosslinking agent and water is 1-2: 0.02-0.1: 0.01-0.05:
10.
6. The preparation method according to claim 2, It is characterized in that The pH value of the mixed solution is 8-10, and the pressure of the mixed solution when it is injected into the wound microfiltration membrane element at low pressure flow is 0.05-0.2 MPa.
7. The preparation method according to claim 2, It is characterized in that The temperature of the thermal free radical polymerization reaction is 40-50° C. and the time is 2-8 hours.
8. The preparation method according to claim 2, It is characterized in that The nickel ion-containing solution is one or more of nickel chloride, nickel nitrate, nickel sulfate, and nickel carbonate, with a concentration of 0.5 to 2 g / L; The solution containing the reducing agent is tea polyphenol, the concentration ratio between the solution containing nickel ions and the solution containing the reducing agent is 1:1.5-3.5, and the injection pressure is 0.25-0.4 MPa.
9. Use of the catalytically functionalized spiral microfiltration membrane element as claimed in claim 1 in catalytic conversion of chlorine-containing organic matter.