Hydroxyapatite nanorod modified carbon nanosphere composite material as well as preparation method and application thereof

By loading hydroxyapatite nanorods on carbon nanospheres, the problem of insufficient adsorption capacity of hydroxyapatite materials is solved, and efficient enrichment and separation of uranium and heavy metal ions in wastewater is achieved, which significantly improves the adsorption capacity.

CN119075914APending Publication Date: 2024-12-06NANHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411371558.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing hydroxyapatite materials are small in specific surface area and prone to agglomeration, resulting in insufficient adsorption capacity of uranium and heavy metal ions in wastewater, which cannot meet the practical application needs.

Method used

By loading hydroxyapatite nanorods on carbon nanospheres, controlling their mass ratio will significantly improve the specific surface area and adsorption sites of the composite material, avoiding the agglomeration of hydroxyapatite, and enhancing its adsorption ability to uranium and heavy metal ions.

Benefits of technology

The high-efficiency enrichment and separation of uranium and heavy metal ions in wastewater was achieved, and the adsorption capacity was significantly improved. The adsorption capacity of uranium reached 2660.3 mg/g, and the adsorption capacity of heavy metal ions Cd2+, Pb2+ and Cr2+ reached 1062.3 mg/g and 1553.7 mg respectively. /g.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005070206130000011
    Figure HDA0005070206130000011
  • Figure HDA0005070206130000012
    Figure HDA0005070206130000012
  • Figure HDA0005070206130000013
    Figure HDA0005070206130000013
Patent Text Reader

Abstract

The invention provides a hydroxyapatite nanorod modified carbon nanosphere composite material as well as a preparation method and application thereof, and belongs to the field of adsorption materials. The hydroxyapatite nanorod modified carbon nanosphere composite material provided by the invention comprises a carbon nanosphere and a hydroxyapatite nanorod loaded on the surface of the carbon nanosphere, the mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is (23 to 68): (32 to 73). The hydroxyapatite nanorods are loaded on the carbon nanospheres, so that the specific surface area of the composite material is remarkably increased, and adsorption sites are increased; by controlling the mass ratio of the hydroxyapatite nanorods to the carbon nanospheres, uniform loading of the hydroxyapatite nanorods is realized, so that enrichment and separation of uranium and heavy metal ions in the wastewater are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adsorption materials, and in particular to a hydroxyapatite nanorod modified carbon nanosphere composite material and a preparation method and application thereof. Background Art

[0002] With the development of uranium mining and smelting industry, a large amount of radioactive and heavy metal wastes such as uranium waste rock and uranium tailings are produced in the process of uranium mining and smelting. These wastes enter the water environment and cause serious pollution to the surrounding environment. Moreover, uranium and heavy metal pollution is toxic, persistent and bioaccumulative, which will seriously endanger the ecosystem and public health and safety. Therefore, the treatment and restoration of uranium and heavy metal polluted environment has become one of the hot topics of global concern.

[0003] Currently, the commonly used methods for removing uranium and heavy metal ions from wastewater include photocatalysis, adsorption, coprecipitation and ion exchange. Among them, adsorption has become a promising treatment technology due to its simple operation, high stability, environmental friendliness and low cost. Hydroxyapatite (HAP), as a natural biomaterial, has excellent biocompatibility, ion exchange capacity, non-toxicity, high stability and high adsorption potential. Moreover, HAP is rich in reactive functional groups (Ca-OH and PO4 3- ), which helps to form more stable crystalline products with radionuclides and heavy metal ions in complex water environments. However, due to its small specific surface area, HAP is prone to agglomeration, resulting in many active sites on HAP being hidden, which seriously reduces the adsorption capacity of HAP for uranium and heavy metal ions in wastewater. It has great limitations in practical application.

[0004] Research has found that evenly loading HAP on a suitable carrier material to form a composite material can effectively prevent its agglomeration behavior, thereby increasing the adsorption capacity of the HAP material and effectively removing uranium and heavy metal ions from wastewater. For example, the composite material of graphene and hydroxyapatite disclosed in the prior art has an adsorption capacity of 510 mg / g for uranium in wastewater; the composite material of hydroxyapatite and graphene oxide disclosed in the prior art has an adsorption capacity of 510 mg / g for heavy metal ions Pb. 2+ The adsorption capacity of Cr 2+ The adsorption capacity can reach 106.7 mg / g. However, the adsorption capacity of the composite material provided in the above prior art still cannot meet the needs of practical applications. Summary of the invention

[0005] The purpose of the present invention is to provide a hydroxyapatite nanorod modified carbon nanosphere composite material and its preparation method and application. The composite material provided by the present invention has a high adsorption capacity and can effectively enrich and separate uranium and heavy metal ions in wastewater.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres;

[0008] The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is (23-68):(32-73).

[0009] Preferably, the particle size of the carbon nanospheres is 1.91 to 5.57 μm; the length of the hydroxyapatite nanorods is 0.18 to 1.01 μm, and the diameter is 0.03 to 0.08 μm.

[0010] The present invention also provides a method for preparing the hydroxyapatite nanorod-modified carbon nanosphere composite material described in the above technical solution, comprising the following steps:

[0011] (1) mixing a phosphorus source, a calcium source, glucose and water to obtain a mixed solution; the molar ratio of P in the phosphorus source, C in the glucose and Ca in the calcium source is 1:(0.46-1.83):1.67;

[0012] (2) subjecting the mixed solution obtained in step (1) to a hydrothermal reaction to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material.

[0013] Preferably, the phosphorus source in step (1) is one or more of diammonium hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate.

[0014] Preferably, the calcium source in step (1) is one or more of calcium chloride dihydrate, calcium nitrate tetrahydrate and calcium chloride.

[0015] Preferably, in step (1), the mass ratio of the phosphorus source to the volume of water is 1 g: (156.25-218.75) mL;

[0016] Preferably, the mixing in step (1) is carried out under stirring conditions; the stirring speed is 400 to 800 rpm / min, and the stirring time is 15 to 30 min.

[0017] Preferably, the temperature of the hydrothermal reaction in step (2) is 120 to 200° C., and the time of the hydrothermal reaction is 12 to 48 hours.

[0018] The present invention also provides the use of the hydroxyapatite nanorod modified carbon nanosphere composite material described in the above technical solution or the hydroxyapatite nanorod modified carbon nanosphere composite material prepared by the preparation method described in the above technical solution in adsorbing uranium and heavy metal ions in wastewater.

[0019] Preferably, the addition amount of the hydroxyapatite nanorod modified carbon nanosphere composite material is 0.1-0.6 g / L.

[0020] The present invention provides a hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres; the mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is (23-68): (32-73). The present invention significantly improves the specific surface area of ​​the composite material and increases the adsorption sites by loading hydroxyapatite nanorods on the carbon nanospheres, thereby promoting ion exchange and dissolution precipitation between the composite material and uranium and heavy metal ions; the surface of the composite material has abundant hydrophilic oxygen-containing functional groups, which can synergistically promote the fixation of uranium and heavy metal ions through complexation reactions, thereby significantly improving the adsorption of uranium and heavy metal ions; at the same time, the mass ratio of hydroxyapatite nanorods to carbon nanospheres in the composite material is controlled to achieve uniform loading of hydroxyapatite nanorods, avoid agglomeration between hydroxyapatites, further improve the adsorption of uranium and heavy metal ions by the composite material, thereby achieving the enrichment and separation of uranium and heavy metal ions in wastewater. The data of the embodiment show that the adsorption capacity of the composite material provided by the present invention for uranium can reach 2660.3 mg / g, and the adsorption capacity for heavy metal ions Cd 2+ , Pb 2+ and Cr 2+ The adsorption capacities can reach 1062.3 mg / g, 1430.9 mg / g and 1553.7 mg / g respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of the hydroxyapatite nanorod-modified carbon nanosphere composite material of Example 1 of the present invention;

[0022] Figure 2 This is a transmission electron microscopy image of the hydroxyapatite nanorod-modified carbon nanosphere composite material of Example 1 of the present invention;

[0023] Figure 3 This is a scanning electron microscope image of the hydroxyapatite nanorod material of Comparative Example 1 of the present invention;

[0024] Figure 4 This is a scanning electron microscope image of the carbon nanosphere material of Comparative Example 2 of the present invention;

[0025] Figure 5 XRD diagrams of materials of Examples 1 to 3 and Comparative Examples 1 to 2 of the present invention;

[0026] Figure 6 This is an X-ray photoelectron spectrum of the hydroxyapatite nanorod-modified carbon nanosphere composite material before and after uranium adsorption in Example 1 of the present invention;

[0027] Figure 7 The uranium and heavy metal ions (Cd 2+ , Pb 2+ Cr 2+ )’s adsorption performance. DETAILED DESCRIPTION

[0028] The present invention provides a hydroxyapatite nanorod-modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres;

[0029] The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is (23-68):(32-73).

[0030] The hydroxyapatite nanorod-modified carbon nanosphere composite material provided by the present invention comprises carbon nanospheres. In the present invention, the carbon nanospheres are used as the matrix of the hydroxyapatite nanorods, which can effectively avoid the agglomeration of the hydroxyapatite nanorods, increase the specific surface area and the number of adsorption sites of the composite material, thereby increasing the adsorption capacity of the composite material, and effectively improving the enrichment and separation and removal of uranium and heavy metal ions in wastewater of the composite material.

[0031] In the present invention, the particle size of the carbon nanospheres is preferably 1.91 to 5.57 μm, more preferably 2 to 5 μm, and most preferably 3 to 4 μm.

[0032] The hydroxyapatite nanorod-modified carbon nanosphere composite material provided by the present invention also includes hydroxyapatite nanorods. In the present invention, the hydroxyapatite nanorods are used as adsorption entities, and their surfaces have abundant hydrophilic oxygen-containing functional groups, which can synergistically promote the fixation of uranium and heavy metal ions through complexation reactions, and can significantly improve the adsorption of uranium and heavy metal ions.

[0033] In the present invention, the length of the hydroxyapatite nanorods is preferably 0.18-1.01 μm, more preferably 0.2-1 μm, and most preferably 0.4-0.6 μm; the diameter of the hydroxyapatite nanorods is preferably 0.03-0.08 μm, more preferably 0.04-0.07 μm, and most preferably 0.05-0.06 μm.

[0034] In the present invention, the mass ratio of the hydroxyapatite nanorods and the carbon nanospheres is (23-68): (32-73), preferably (25-60): (35-65), more preferably (30-50): (40-60), and most preferably (35-40): (45-50). In the present invention, by controlling the mass ratio of the hydroxyapatite nanorods and the carbon nanospheres in the composite material, the uniform loading of the hydroxyapatite nanorods is achieved, the agglomeration of the hydroxyapatite nanorods is avoided, and the adsorption of uranium and heavy metal ions by the composite material is further improved.

[0035] The hydroxyapatite nanorod-modified carbon nanosphere composite material provided by the present invention significantly improves the specific surface area of ​​the composite material and increases the adsorption sites by loading hydroxyapatite nanorods on carbon nanospheres, thereby promoting ion exchange and dissolution precipitation between the composite material and uranium and heavy metal ions; at the same time, the mass ratio of hydroxyapatite nanorods to carbon nanospheres in the composite material is controlled to achieve uniform loading of hydroxyapatite nanorods, avoid agglomeration between hydroxyapatites, and further improve the adsorption of uranium and heavy metal ions by the composite material.

[0036] The present invention also provides a method for preparing the hydroxyapatite nanorod-modified carbon nanosphere composite material described in the above technical solution, comprising the following steps:

[0037] (1) mixing a phosphorus source, a calcium source, glucose and water to obtain a mixed solution; the molar ratio of P in the phosphorus source, C in the glucose and Ca in the calcium source is 1:(0.46-1.83):1.67;

[0038] (2) subjecting the mixed solution obtained in step (1) to a hydrothermal reaction to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material.

[0039] The invention mixes a phosphorus source, a calcium source, glucose and water to obtain a mixed solution.

[0040] In the present invention, the phosphorus source is preferably one or more of diammonium hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate; more preferably diammonium hydrogen phosphate. In the present invention, the phosphorus source provides P element as a raw material for synthesizing hydroxyapatite nanorods.

[0041] In the present invention, the calcium source is one or more of calcium chloride dihydrate, calcium nitrate tetrahydrate and calcium chloride, and more preferably calcium chloride dihydrate. In the present invention, the calcium source provides Ca element for synthesizing hydroxyapatite nanorods.

[0042] In the present invention, the glucose provides C element as a raw material for synthesizing carbon nanospheres; the carbon nanospheres prepared by using glucose have uniform particle size and controllable size, and at the same time, the obtained carbon nanospheres have a large number of active functional groups on the surface and good surface activity, which can well realize the loading of hydroxyapatite nanorods, help to exert the performance of the composite material, and further improve the adsorption performance of the composite material.

[0043] In the present invention, the molar ratio of P in the phosphorus source, C in the glucose and Ca in the calcium source is 1:(0.46-1.83):1.67, preferably 1:(0.69-1.39):1.67, and more preferably 1:(0.93-1.16):1.67. In the present invention, by limiting the ratio of the reaction raw materials, the ratio of hydroxyapatite nanorods and carbon nanospheres in the composite material is controlled, the uniformity of the hydroxyapatite nanorod loading is further improved, and the agglomeration of the hydroxyapatite nanorods is further avoided, thereby improving the adsorption performance of the composite material.

[0044] In the present invention, the ratio of the mass of the phosphorus source to the volume of water is preferably 1g: (156.25-218.75) mL, more preferably 1g: (170-200) mL, and most preferably 1g: (180-190) mL. In the present invention, by limiting the ratio of the mass of the phosphorus source to the volume of water, the contact opportunity of the phosphorus source, glucose and calcium source in the mixed solution is increased, ensuring that the three can fully react, and a composite material can be obtained; at the same time, by controlling the concentration of the reaction raw materials, the crystallization process of the hydroxyapatite nanorods can be controlled, which is helpful to obtain a product with high crystallinity and regular crystal structure, and improve the porosity of the hydroxyapatite nanorods, expose surface active sites, and further improve the adsorption performance of the composite material; by controlling the concentration of the reaction raw materials, it is also beneficial to form carbon nanospheres with smooth surface and uniform structure, avoid the generation of internal structural defects, help load the hydroxyapatite nanorods and further improve the adsorption performance.

[0045] In the present invention, the phosphorus source, calcium source, glucose and water are preferably mixed as follows: the calcium source is mixed with part of the water to obtain solution A, the phosphorus source and the carbon source are mixed with the remaining water to obtain solution B, and then solution A is mixed with solution B to obtain a mixed solution. In the present invention, there is no particular limitation on the amount ratio of the water in solution A to the water in solution B, as long as the amount ratio of P to Ca in the mixed solution is 1:1.67. In the present invention, by adopting the above-mentioned step-by-step mixing method, the mixing uniformity of the mixed solution is further improved, and the performance of the composite material is further improved.

[0046] In the present invention, the mixing is preferably carried out under stirring conditions; the stirring speed is preferably 400-800 rpm / min, more preferably 500-700 rpm / min, most preferably 550-600 rpm / min; the stirring time is preferably 15-30 min, more preferably 18-28 min, most preferably 20-25 min.

[0047] After obtaining the mixed solution, the present invention performs a hydrothermal reaction on the mixed solution to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material.

[0048] In the present invention, the temperature of the hydrothermal reaction is preferably 120-200°C, more preferably 140-180°C, and most preferably 150-160°C; the time of the hydrothermal reaction is preferably 12-48h, more preferably 16-36h, and most preferably 20-30h. In the present invention, the process parameters of the hydrothermal reaction are limited to ensure the smooth progress of the hydrothermal reaction; at the same time, a chemical reaction occurs between the calcium source and the phosphorus source to obtain hydroxyapatite nanorods, and glucose is thermally decomposed and aggregated to obtain carbon nanospheres; by controlling the conditions of the hydrothermal reaction, the growth rate of hydroxyapatite and carbon nanospheres is controlled to make the product morphology complete and regular; controlling the reaction conditions can also avoid the formation of surface and internal defects during the formation of hydroxyapatite nanorods and carbon nanospheres, further improving the performance of the composite material.

[0049] After the hydrothermal reaction is completed, the present invention preferably cools the product of the hydrothermal reaction naturally to room temperature, and then centrifuges, washes and dries it in sequence to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material.

[0050] The present invention has no special limitation on the centrifugation, washing and drying operations, and the centrifugation, washing and drying operations commonly used in the art can be used. In the present invention, surface impurities can be effectively removed by post-treatment, further improving the adsorption performance of the composite material, and preventing impurities from occupying adsorption sites and affecting the adsorption performance.

[0051] The preparation method of the composite material provided by the present invention can promote the loading and loading uniformity of hydroxyapatite nanorods on carbon nanospheres, and further improve the adsorption performance of the composite material.

[0052] The present invention also provides the use of the hydroxyapatite nanorod-modified carbon nanosphere composite material described in the above technical solution in adsorbing uranium and heavy metal ions in wastewater.

[0053] In the present invention, the heavy metal ion is preferably Cu 2+ , Mn 2+ 、Cd 2+ , Pb 2+ and Cr 2+One or more of; the concentration of uranium is preferably 10-1500 mg / L, more preferably 100-1300 mg / L, most preferably 400-800 mg / L; the concentration of heavy metal ions is preferably 10-400 mg / L, more preferably 100-350 mg / L, most preferably 150-250 mg / L; the pH value of the wastewater is preferably 2-9, more preferably 4-7, most preferably 5-6. In the present invention, by limiting the concentration of uranium in the wastewater, the type and concentration of heavy metal ions, and the pH value of the wastewater, it is beneficial to the performance of the adsorption material and ensure the effective removal of harmful substances in the wastewater.

[0054] In the present invention, the amount of the hydroxyapatite nanorod-modified carbon nanosphere composite material is preferably 0.1-0.6 g / L, more preferably 0.2-0.5 g / L, and most preferably 0.3-0.4 g / L; the hydroxyapatite nanorod-modified carbon nanosphere composite material is preferably used in a stirring state, and the stirring rate is preferably 100-300 rpm / min, more preferably 150-250 rpm / min, and most preferably 160-180 rpm / min; the stirring temperature is preferably room temperature; the stirring time is preferably 60-180 min, more preferably 80-150 min, and most preferably 85-90 min. In the present invention, by limiting the amount and state of use of the composite material, it is ensured that the composite material can effectively remove uranium and heavy metal ions in wastewater.

[0055] The present invention helps the composite material to fully contact with uranium and heavy metal ions in waste water by controlling the parameters of the composite material application process, thereby improving the enrichment and separation effect of the composite material.

[0056] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] Example 1

[0058] A hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres;

[0059] The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is 44:56; the particle size of the carbon nanospheres is 2.51 μm; the length of the hydroxyapatite nanorods is 0.34 μm; and the diameter of the hydroxyapatite nanorods is 0.05 μm.

[0060] The preparation method of the hydroxyapatite nanorod modified carbon nanosphere composite material comprises the following steps:

[0061] (1) 0.59 g of calcium source CaCl2·2H2O was mixed with 30 mL of deionized water to obtain solution A, 0.32 g of phosphorus source (NH4)2HPO4 and 0.4 g of carbon source glucose were mixed with 30 mL of deionized water to obtain solution B, and solution A and solution B were mixed at 600 rpm / min for 20 min to obtain a mixed solution; wherein the molar ratio of Ca, P and C in CaCl2·2H2O, (NH4)2HPO4 and glucose was 1.67:1:0.93; and the ratio of the mass of (NH4)2HPO4 to the volume of water in the mixed solution was 1 g:187.5 mL;

[0062] (2) The mixed solution obtained in step (1) was transferred into a Teflon-lined stainless steel autoclave, and a hydrothermal reaction was carried out at 180° C. for 24 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and a black precipitate was collected by centrifugation at 7000 rpm / min for 10 min. The black precipitate was washed three times with deionized water, and then dried in an oven at 60° C. for 10 h to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-2.

[0063] The hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-2 obtained in Example 1 was detected using GeminiSEM 300, and the obtained scanning electron microscope image is as follows: Figure 1 As shown, (a) is a scanning electron microscope image of HAP / CNS-2 at a magnification of 1 μm, and (b) is a scanning electron microscope image of HAP / CNS-2 at a magnification of 500 nm. Figure 1 In (a), it can be seen that the structure of hydroxyapatite nanorods decorated on the surface of nanocarbon spheres has successfully appeared in the composite material; Figure 1 As can be seen in (b), there are small pores on the surface of carbon nanospheres, which can provide more adsorption sites for uranium and heavy metal ions.

[0064] The hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-2 obtained in Example 1 was detected using JEM-2100F, and the obtained transmission electron microscopy image is as follows: Figure 2 As shown, (c) is a transmission electron micrograph of HAP / CNS-2 at a magnification of 200 nm, and (d) is a transmission electron micrograph of HAP / CNS-2 at a magnification of 5 nm. Figure 2 As can be seen in (c), it is further confirmed that the composite material has a unique porous microsphere structure, and the surface is decorated with many short nanorods with regular shapes; Figure 2As can be seen in (d), the nanorods have clear lattice fringes with a spacing of about 0.272 nm, which is related to the (300) crystal plane of hydroxyapatite, indicating that it has a high degree of crystallinity.

[0065] Example 2

[0066] A hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres;

[0067] The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is 66:34; the particle size of the carbon nanospheres is 5.57 μm; the length of the hydroxyapatite nanorods is 0.87 μm; and the diameter of the hydroxyapatite nanorods is 0.07 μm.

[0068] The preparation method of the hydroxyapatite nanorod modified carbon nanosphere composite material comprises the following steps:

[0069] (1) 0.59 g of calcium source CaCl2·2H2O was mixed with 30 mL of deionized water to obtain solution A, 0.32 g of phosphorus source (NH4)2HPO4 and 0.2 g of carbon source glucose were mixed with 30 mL of deionized water to obtain solution B, and solution A and solution B were mixed at 600 rpm / min for 20 min to obtain a mixed solution; wherein the molar ratio of Ca, P and C in CaCl2·2H2O, (NH4)2HPO4 and glucose was 1.67:1:0.46; and the ratio of the mass of (NH4)2HPO4 to the volume of water in the mixed solution was 1 g:187.5 mL;

[0070] (2) The mixed solution obtained in step (1) was transferred into a Teflon-lined stainless steel autoclave, and a hydrothermal reaction was carried out at 180° C. for 24 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and a black precipitate was collected by centrifugation at 7000 rpm / min for 10 min. The black precipitate was washed three times with deionized water, and then dried in an oven at 60° C. for 10 h to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-1.

[0071] Example 3

[0072] A hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres;

[0073] The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is 37:63; the particle size of the carbon nanospheres is 2.13 μm; the length of the hydroxyapatite nanorods is 0.20 μm; and the diameter of the hydroxyapatite nanorods is 0.03 μm.

[0074] The preparation method of the hydroxyapatite nanorod modified carbon nanosphere composite material comprises the following steps:

[0075] (1) 0.59 g of calcium source CaCl2·2H2O was mixed with 30 mL of deionized water to obtain solution A, 0.32 g of phosphorus source (NH4)2HPO4 and 0.8 g of carbon source glucose were mixed with 30 mL of deionized water to obtain solution B, and solution A and solution B were mixed at 600 rpm / min for 20 min to obtain a mixed solution; wherein the molar ratio of Ca, P and C in CaCl2·2H2O, (NH4)2HPO4 and glucose was 1.67:1:1.83; and the ratio of the mass of (NH4)2HPO4 to the volume of water in the mixed solution was 1 g:187.5 mL;

[0076] (2) The mixed solution obtained in step (1) was transferred into a Teflon-lined stainless steel autoclave, and a hydrothermal reaction was carried out at 180° C. for 24 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and a black precipitate was collected by centrifugation at 7000 rpm / min for 10 min. The black precipitate was washed three times with deionized water, and then dried in an oven at 60° C. for 10 h to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-4.

[0077] Comparative Example 1

[0078] The difference between Comparative Example 1 and Example 1 is that the addition of carbon source is omitted to obtain hydroxyapatite nanorod material, and the rest is the same as Example 1.

[0079] The hydroxyapatite nanorod material obtained in Comparative Example 1 was tested using GeminiSEM 300, and the obtained scanning electron microscope image is as follows: Figure 3 As shown. Figure 3 It can be seen that hydroxyapatite is composed of many irregularly stacked nanorods in a disordered structure.

[0080] Comparative Example 2

[0081] The difference between Comparative Example 2 and Example 1 is that the addition of calcium source and phosphorus source is omitted, and the mass of the carbon source is 1 g, and a carbon nanosphere material is obtained. The rest is the same as Example 1.

[0082] The carbon nanosphere material obtained in Comparative Example 2 was tested using GeminiSEM 300, and the obtained scanning electron microscope image is as follows: Figure 4 As shown. Figure 4 It can be seen that the surface of the carbon nanospheres is smooth.

[0083] The materials of Examples 1 to 3 and Comparative Examples 1 to 2 were tested using an X-ray diffractometer, and the results obtained are as follows: Figure 5 As shown. Figure 5 It can be seen that in the XRD spectrum of the carbon nanosphere material of Comparative Example 2, a typical amorphous carbon diffraction peak appears at 20-30°; the XRD spectrum of the composite materials of Examples 1 to 3 shows that the main component of the generated product is hydroxyapatite, and the generated hydroxyapatite has a high degree of crystallinity; in the XRD spectrum of Example 1 HAP / CNS-2, in addition to the characteristic peaks of hydroxyapatite, peaks corresponding to the (001) and (002) crystal planes of graphite carbon are observed at 13.17° and 26.44°, respectively; and with the increase of the amount of glucose used, the diffraction peak intensities at 13.17°, 26.44° and 39.819° are significantly enhanced, indicating that the presence of glucose promotes the crystallization of the composite material.

[0084] Application Example 1

[0085] 4 mg of the hydroxyapatite nanorod modified carbon nanosphere composite material of Examples 1 to 3, the hydroxyapatite nanorod material of Comparative Example 1, and the carbon nanosphere material of Comparative Example 2 were respectively put into 20 mL of wastewater containing 600 mg / L uranium, and ultrasonicated for 10 s to fully disperse the above materials in the wastewater, maintaining the pH of the wastewater at 4, and stirring and adsorbing for 180 min at a temperature of 25°C and a stirring rate of 500 rpm / min, and sampling was taken at different time points to detect the concentration of radioactive uranium.

[0086] The results show that the adsorption capacity of uranium by the hydroxyapatite nanorod material of comparative example 1 is 1042.3 mg / g, the adsorption capacity of uranium by the carbon nanosphere material of comparative example 2 is 77.4 mg / g, the adsorption capacity of uranium by the hydroxyapatite nanorod modified carbon nanosphere composite material of example 1 is 2660.3 mg / g, the adsorption capacity of uranium by the hydroxyapatite nanorod modified carbon nanosphere composite material of example 2 is 1493.6 mg / g, and the adsorption capacity of uranium by the hydroxyapatite nanorod modified carbon nanosphere composite material of example 3 is 1624.7 mg / g.

[0087] The hydroxyapatite nanorod-modified carbon nanosphere composite material HAP / CNS-2 of Example 1 was detected by X-ray photoelectron spectroscopy. The X-ray photoelectron spectra of the material before and after uranium adsorption are as follows: Figure 6 As shown. Figure 6 It can be seen that before the adsorption of uranium, the peaks of C1s, O 1s, Ca 2p, and P 2p appeared in the XPS spectrum of HAP / CNS-2, proving that the HAP / CNS-2 composite material was successfully prepared, while a new peak appeared after the adsorption of uranium, which was related to U 4f, indicating that uranium was successfully fixed by the HAP / CNS-2 material.

[0088] Application Example 2

[0089] 4 mg of the hydroxyapatite nanorod-modified carbon nanosphere composite material of Example 1, the hydroxyapatite nanorod material of Comparative Example 1, and the carbon nanosphere material of Comparative Example 2 were respectively put into 20 mL of each heavy metal ion (Cd 2+ , Pb 2 + Cr 2+ ) in wastewater with a concentration of 400 mg / L, and ultrasonication was performed for 10 seconds to fully disperse the above materials in the wastewater, and the pH value of the wastewater was maintained at 4. The adsorption was stirred for 180 minutes at a temperature of 25°C and a stirring rate of 500 rpm / min, and samples were taken at different time points to detect the concentrations of the above three heavy metal ions.

[0090] The results show that the hydroxyapatite nanorod material of comparative example 1 has a strong affinity for heavy metal ions Cd 2+ , Pb 2+ and Cr 2+ The adsorption capacities of the carbon nanospheres in Comparative Example 2 for heavy metal ions Cd 2 + , Pb 2+ and Cr 2+ The adsorption capacities of the hydroxyapatite nanorods modified carbon nanospheres composite material in Example 1 were 23.3 mg / g, 25.1 mg / g and 33.5 mg / g, respectively. 2+ , Pb 2+ and Cr 2+ The adsorption capacities are 1062.3 mg / g, 1430.9 mg / g and 1553.7 mg / g respectively.

[0091] The hydroxyapatite nanorods modified carbon nanospheres composite material HAP / CNS-2 in Example 1 was effective in treating 600 mg / L uranium and 400 mg / L heavy metal ions (Cd 2+ , Pb 2+ Cr 2+ )'s adsorption properties such as Figure 7 As shown. Figure 7 It can be seen that in the first 90 minutes of adsorption, the adsorption rate of HAP / CNS-2 for uranium and heavy metal ions was faster. In the last 90 minutes, the adsorption rate of HAP / CNS-2 for uranium and heavy metal ions slowly tended to equilibrium. The adsorption effect of HAP / CNS-2 material on radioactive uranium was significantly higher than that on heavy metal ions. Among them, its adsorption performance for uranium reached 2660.3 mg / g, and for heavy metal ions Cd 2+ , Pb 2+ and Cr 2+The adsorption capacities are 1062.3 mg / g, 1430.9 mg / g and 1553.7 mg / g respectively.

[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A hydroxyapatite nanorod modified carbon nanosphere composite material, comprising carbon nanospheres and hydroxyapatite nanorods loaded on the surface of the carbon nanospheres; The mass ratio of the hydroxyapatite nanorods to the carbon nanospheres is (23-68):(32-73).

2. The hydroxyapatite nanorod-modified carbon nanosphere composite material according to claim 1, characterized in that: The particle size of the carbon nanosphere is 1.91-5.57 μm; the length of the hydroxyapatite nanorod is 0.18-1.01 μm, and the diameter is 0.03-0.08 μm.

3. The method for preparing the hydroxyapatite nanorod-modified carbon nanosphere composite material according to claim 1, comprising the following steps: (1) mixing a phosphorus source, a calcium source, glucose and water to obtain a mixed solution; the molar ratio of P in the phosphorus source, C in the glucose and Ca in the calcium source is 1:(0.46-1.83):1.67; (2) subjecting the mixed solution obtained in step (1) to a hydrothermal reaction to obtain a hydroxyapatite nanorod-modified carbon nanosphere composite material.

4. The preparation method according to claim 3, characterized in that: In the step (1), the phosphorus source is one or more of diammonium hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate and potassium dihydrogen phosphate.

5. The preparation method according to claim 3, characterized in that: The calcium source in step (1) is one or more of calcium chloride dihydrate, calcium nitrate tetrahydrate and calcium chloride.

6. The preparation method according to any one of claims 3 to 4, characterized in that: In the step (1), the mass ratio of the phosphorus source to the volume of water is 1 g: (156.25-218.75) mL.

7. The preparation method according to claim 3, characterized in that: The mixing in step (1) is carried out under stirring conditions; the stirring speed is 400 to 800 rpm / min, and the stirring time is 15 to 30 min.

8. The preparation method according to claim 3, characterized in that: The temperature of the hydrothermal reaction in step (2) is 120 to 200° C., and the time of the hydrothermal reaction is 12 to 48 hours.

9. Use of the hydroxyapatite nanorod-modified carbon nanosphere composite material according to claim 1 or 2 or the hydroxyapatite nanorod-modified carbon nanosphere composite material prepared by the preparation method according to claims 3 to 8 in adsorbing uranium and heavy metal ions in wastewater.

10. The use according to claim 9, characterized in that: The addition amount of the hydroxyapatite nanorod modified carbon nanosphere composite material is 0.1-0.6 g / L.