Preparation method and application of acid-resistant polyacrylic acid hydrogel adsorbent

By preparing acid-resistant polyacrylic acid hydrogel adsorbent, using TA and Na-MMT as crosslinking agents, the problem of unstable hydrogel under acidic conditions is solved, and efficient uranium ion adsorption and regeneration performance is achieved, suitable for containing Purification of uranium wastewater.

CN119075943APending Publication Date: 2024-12-06EAST CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411376211.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing hydrogels have low mechanical properties when treating uranium-containing wastewater and are unstable under acidic conditions, which limits their application.

Method used

The mass ratio of N,N'-methylenebisacrylamide, tannic acid, sodium montmorillonite, acrylic acid and ammonium persulfate is 1: (0.8-8.3): (0.8-8.3): (250-750 ): (30-35) ratio, acid-resistant polyacrylic acid hydrogel adsorbent is prepared by simple radical polymerization, using TA and Na-MMT as a combined crosslinking agent to significantly enhance the stability of the hydrogel, and Maintain good adsorption performance in acidic environments.

Benefits of technology

The prepared acid-resistant polyacrylic acid hydrogel adsorbent exhibits excellent uranium ion adsorption performance under pH=6, with a maximum adsorption capacity of 1218.03 mg·g-1, and remains stable under acidic conditions, significantly improving the traditional adsorbent regeneration performance and adsorption capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075943A_ABST
    Figure CN119075943A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an acid-resistant polyacrylic acid hydrogel adsorbent, and relates to a preparation method and application of hydrogel. The invention aims to solve the technical problems that the existing hydrogel is low in mechanical property and unstable under an acidic condition when being applied to treatment of uranium-containing wastewater. The preparation method of the acid-resistant polyacrylic acid hydrogel adsorbent comprises the following steps: adding N, N '-methylene bisacrylamide, tannic acid and Na-montmorillonite into an acrylic acid aqueous solution, and stirring to obtain a mixed solution; then adding ammonium persulfate into the mixed solution, and carrying out stirring reaction in an ice-water bath to obtain a precursor solution; standing the precursor solution to obtain hydrogel, and finally freeze-drying to obtain the acid-resistant polyacrylic acid hydrogel adsorbent. When the adsorbent is used for purifying uranium-containing wastewater with the pH value of 6, the maximum adsorption capacity reaches 1218.03 mg.g <-1 >, and the adsorbent is good in regeneration performance, stable under the acidic condition and capable of being used in the field of uranium-containing wastewater purification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a hydrogel. Background Art

[0002] With the development of nuclear industry, it is very important to remove wastewater containing radioactive metal ions (mainly uranium). Uranium is usually oxidized in the form of uranyl ions (UO2 2+ ) form, so the treatment of uranium-containing wastewater is actually the treatment of UO2 2+ treatment. In recent years, there are many uranium treatment technologies, such as chemical precipitation, solvent extraction, membrane treatment, etc. Among these technologies, adsorption is considered to be a technology with good development prospects due to its simplicity, economy and high efficiency. Among them, polymers are considered to be very promising uranium adsorption materials because of their rich adsorption sites. Hydrogels are formed by cross-linking of hydrophilic polymer chains. Their unique three-dimensional network structure enables metal ions in the solution to quickly penetrate the network through water and form stable complexes with functional groups. However, most hydrogels have low ductility and are brittle, with low mechanical properties. At the same time, hydrogels are also unstable under acidic conditions, which severely limits the application of hydrogels in the treatment of uranium-containing wastewater. Summary of the invention

[0003] The present invention aims to solve the problems that the existing hydrogel has low mechanical properties and is unstable under acidic conditions when used to treat uranium-containing wastewater, and provides a preparation method and application of an acid-resistant polyacrylic acid hydrogel adsorbent.

[0004] The preparation method of the acid-resistant polyacrylic acid hydrogel adsorbent of the present invention is carried out according to the following steps:

[0005] 1. Weigh N,N'-methylenebisacrylamide (MBA), tannic acid (TA), sodium montmorillonite (Na-MMT), acrylic acid (AA), and ammonium persulfate (APS) according to the mass ratio of N,N'-methylenebisacrylamide (MBA), tannic acid (TA), sodium montmorillonite (Na-MMT), acrylic acid (AA), and ammonium persulfate (APS) of 1: (0.8-8.3): (0.8-8.3): (250-750): (30-35);

[0006] 2. First, acrylic acid is mixed with water to prepare an acrylic acid aqueous solution with a mass percentage concentration of 15% to 45%; then, the N,N'-methylenebisacrylamide, tannic acid and sodium montmorillonite weighed in step 1 are added to the acrylic acid aqueous solution, and stirred at room temperature for 20 to 60 minutes to obtain a mixed solution; then, the ammonium persulfate weighed in step 1 is added to the mixed solution, and stirred in an ice water bath for 5 to 15 minutes to obtain a precursor solution;

[0007] 3. Pour the precursor solution into a container and place it in an oven at a temperature of 35-75°C for 20-40 minutes to obtain PAA-TA@MMT hydrogel;

[0008] 4. Freeze-dry the PAA-TA@MMT hydrogel to obtain an acid-resistant polyacrylic acid hydrogel adsorbent, which is recorded as PAA-TA@MMT adsorbent.

[0009] Furthermore, the mass ratio of N,N'-methylenebisacrylamide, tannic acid, sodium montmorillonite, acrylic acid and ammonium persulfate described in step 1 is 1:(2-5):(2-5):(400-600):(32-34).

[0010] Furthermore, the freeze-drying temperature in step 4 is -30 to -50°C, and the freeze-drying time is 20 to 28 hours.

[0011] The application of the acid-resistant polyacrylic acid hydrogel adsorbent prepared by the method is to use the acid-resistant polyacrylic acid hydrogel adsorbent for purifying uranium-containing wastewater.

[0012] The method for purifying uranium-containing wastewater using acid-resistant polyacrylic acid hydrogel adsorbent is as follows: adding the acid-resistant polyacrylic acid hydrogel adsorbent to the uranium-containing wastewater, adjusting the pH to 5-7, stirring and adsorbing at a speed of 150-200 rpm for 600-1200 minutes at a temperature of 5-45°C, taking out the acid-resistant polyacrylic acid hydrogel adsorbent, and completing the treatment of the uranium-containing wastewater.

[0013] The present invention uses a simple free radical polymerization method and TA and Na-MMT as a joint crosslinking agent to significantly enhance the stability of the hydrogel, so that the PAA-TA@MMT hydrogel exhibits good acid resistance and reliable regeneration performance during application. The acid-resistant polyacrylic acid hydrogel of the present invention exhibits excellent performance in adsorbing uranium ions, especially under the condition of pH = 6, with a maximum adsorption capacity of 1218.03 mg·g -1 .

[0014] The adsorbent prepared by the present invention can effectively solve the problems of low adsorption capacity, poor regeneration performance and instability under acidic conditions of traditional adsorbents, and can be used in the field of purification of uranium-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 PAA-TA prepared in Example 1 15 @MMT 15 photos;

[0016] Figure 2 PAA-TA in Example 1 15 @MMT15 Microscopic topography of the plane;

[0017] Figure 3 PAA-TA in Example 1 15 @MMT 15 Microscopic morphology of the cross section;

[0018] Figure 4 PAA-TA in Example 1 15 @MMT 15 Fourier transform infrared spectrum of

[0019] Figure 5 PAA-TA in Example 1 15 @MMT 15 Photo of contact angle with water;

[0020] Figure 6 PAA-TA in Example 1 15 @MMT 15 Contact angle photograph with U standard solution (pH=6);

[0021] Figure 7 PAA-TA in Example 1 15 @MMT 15 Contact angle photograph with U standard solution (pH=5);

[0022] Figure 8 PAA-TA in Example 1 15 @MMT 15 Contact angle photograph with U standard solution (pH = 4);

[0023] Fig. 9 PAA-TA in Example 1 15 @MMT 15 Morphological photographs after treatment with acidic solution (pH = 1);

[0024] Fig.10 PAA-TA in Example 1 15 @MMT 15 Microscopic morphology after treatment with acidic solution (pH = 1);

[0025] Fig.11 PAA-TA in Example 1 15 @MMT 15 Adsorption performance diagram of uranium-containing wastewater at different pH;

[0026] Fig.12 PAA-TA in Example 1 15 @MMT 15 Adsorption performance diagram of uranium-containing wastewater at different temperatures;

[0027] Fig.13 PAA-TA in Example 1 15 @MMT 15 Adsorption performance diagram of uranium-containing wastewater at different times;

[0028] Fig.14 PAA-TA in Example 1 15 @MMT 15 Adsorption performance diagram of uranium-containing wastewater at different initial concentrations;

[0029] Fig.15 PAA-TA in Example 1 15 @MMT 15 Reuse performance diagram;

[0030] Fig.16 PAA-TA in Example 1 15 @MMT 15 Adsorption performance diagram of uranium-containing wastewater in the presence of competing ions;

[0031] Fig.17 PAA-TA in Example 1 15 @MMT 15 Microscopic morphology after adsorption of uranium ions. DETAILED DESCRIPTION

[0032] Use the following examples to verify the beneficial effects of the present invention:

[0033] Example 1: The preparation method of the acid-resistant polyacrylic acid hydrogel for purifying uranium-containing wastewater in Example 1 is carried out according to the following steps:

[0034] 1. Weigh 6 mg N,N'-methylenebisacrylamide (MBA), 15 mg tannic acid (TA), 15 mg sodium montmorillonite (Na-MMT), 3 g acrylic acid (AA), and 200 mg ammonium persulfate (APS);

[0035] 2. First, acrylic acid is mixed with water to prepare an acrylic acid aqueous solution with a mass percentage concentration of 30%; then, N,N'-methylenebisacrylamide (MBA), tannic acid (TA), and sodium montmorillonite (Na-MMT) weighed in step 1 are added to the acrylic acid aqueous solution, and stirred at room temperature for 40 minutes to obtain a mixed solution; then, the ammonium persulfate weighed in step 1 is added to the mixed solution, and stirred in an ice water bath for 10 minutes to obtain a precursor solution;

[0036] 3. Pour the precursor solution into a culture dish and place it in an oven at 55°C for 30 minutes to obtain PAA-TA@MMT hydrogel;

[0037] Fourth, the PAA-TA@MMT hydrogel was freeze-dried in a freeze drying oven at -40 °C for 24 h to obtain an acid-resistant polyacrylic acid hydrogel adsorbent, denoted as PAA-TA 15 @MMT 15 Adsorbent.

[0038] Example 1 PAA-TA prepared by step 4 15 @MMT 15 Photos of adsorbents Figure 1 As shown, PAA-TA 15 @MMT 15 The adsorbent was tested by scanning electron microscopy, and the microscopic morphology of the plane was obtained. Figure 2 The microscopic morphology of the cross section is shown in Figure 3 As shown by Figure 1 , Figure 2 and Figure 3 It can be seen that PAA-TA 15 @MMT 15 The surface is flat and the cross section is relatively uniform, indicating that the adsorbent has good uniformity.

[0039] PAA-TA prepared in step 4 of Example 1 15 @MMT 15 The adsorbent was tested by Fourier infrared spectroscopy, and the infrared spectrum obtained was as follows Figure 4 As shown by Figure 4 It is known that PAA-TA 15 @MMT 15 Strong hydroxyl and carboxyl peaks appeared on the surface. Compared with the PAA powder purchased directly, PAA-TA 15 @MMT 15 The hydroxyl peak of the hydroxyl group is stronger, indicating that it has better stability.

[0040] PAA-TA prepared in step 4 of Example 1 15 @MMT 15 The contact angle of the adsorbent was measured with water and uranium solution (pH = 4, 5, 6). 15 @MMT 15 The contact angle with water is Figure 5 As shown by Figure 5 It is known that PAA-TA 15 @MMT 15 The contact angle with water as the medium is 78.5°. 15 @MMT 15 The contact angle with U standard solution (pH = 6) is as follows Figure 6 As shown, PAA-TA 15 @MMT 15 The contact angle with U standard solution (pH = 5) is as follows Figure 7 Shown; PAA-TA 15 @MMT 15 The contact angle with U standard solution (pH = 4) is as follows Figure 8 As shown. Figure 6 , 7 As can be seen from Figure 8, the contact angles when uranium liquid is used as the medium are 82° (pH = 4), 84° (pH = 5), and 84° (pH = 6), respectively. Although the contact angles increase, they are still < 90°, indicating that PAA-TA 15 @MMT 15 The surface is hydrophilic, which is conducive to the entry of uranium ions in water into the material and improves the adsorption efficiency.

[0041] PAA-TA prepared in step 4 of Example 1 15 @MMT 15 The adsorbent was placed in a 0.1M HNO3 solution and its morphology in the solution was observed after different periods of time. Fig. 9 As shown, after 1440 min, PAA-TA 15 @MMT 15 The adsorbent swelled and absorbed water until equilibrium was reached, and then there was no significant change in its morphology until it was treated with 0.1M HNO3 for 48 hours. After drying, it was tested by scanning electron microscopy to obtain the microscopic morphology after strong acid treatment, as shown in 10. Fig.10 It is known that PAA-TA 15 @MMT 15 There is no significant change. When it is applied to uranium wastewater treatment, the adsorption capacity is not significantly reduced compared with direct application. 15 @MMT 15 Has good acid resistance.

[0042] Application Example 1: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a series of conical flasks, in which uranyl ions (UO2 2+ ) concentration was 20 ppm, and after adjusting the pH to 3, 4, 5, 6, and 7, 5 mg PAA-TA 15 @MMT 15 The adsorbent was added to the uranium-containing solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was carried out for 1440 min at a temperature of 25 °C. The uranium ion concentration in the supernatant was measured and the adsorption capacity was calculated. 15 @MMT 15 The adsorption of uranium-containing wastewater at different pH values ​​is shown in Figure 2. Fig.11As shown, from Fig.11 It can be seen that under strong acidic conditions of pH = 3, PAA-TA 15 @MMT 15 The adsorption capacity of is the lowest, but with the increase of pH value, the adsorption performance gradually increases, and reaches the best performance at pH = 6 (adsorption capacity is 567.55 mg·g-1), and then shows a downward trend with the increase of pH.

[0043] Application Example 2: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a series of conical flasks, in which uranyl ions (UO2 2+ ) concentration was 20ppm, and after adjusting the values ​​to 6, 5mgPAA-TA 15 @MMT 15 The adsorbent was added to the uranium-containing solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was carried out for 1440 min at temperatures of 5, 15, 25, 35, and 45 °C, respectively. The uranium ion concentration in the supernatant was measured and the adsorption capacity was calculated. 15 @MMT 15 The adsorption amount of Fig.12 shown; from Fig.12 It can be seen that when the temperature is between 5 and 25°C, the adsorption performance gradually increases with the increase in temperature; when the temperature is between 25 and 45°C, the increase in temperature will lead to a decrease in the adsorption amount, and the best temperature is 25°C.

[0044] Application Example 3: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a series of conical flasks, in which uranyl ions (UO2 2+ ) concentration was 20ppm, and after adjusting the pH value to 6, 5mgPAA-TA 15 @MMT 15 The adsorbent was added to the uranium-containing solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was performed at 25°C for 30, 60, 120, 240, 360, 480, 720, 960, 1200, and 1440 min. The uranium ion concentration in the supernatant was measured and the adsorption capacity was calculated. 15 @MMT 15 The variation of adsorption amount with adsorption time is shown in Fig.13 shown; from Fig.13 It can be seen that the adsorption rate increased rapidly in the first 480 min after the adsorption, and then began to increase slowly, reaching equilibrium after 1200 min.

[0045] Application Example 4: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a series of conical flasks, in which uranyl ions (UO2 2+ ) concentrations of 5, 10, 20, 30, 40, 50, 60, 80, and 100 ppm, and after adjusting the pH value to 6, 5 mg PAA-TA 15 @MMT 15 The adsorbent was added to the uranium-containing solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was carried out for 1200 min at a temperature of 25 °C. The uranium ion concentration in the supernatant was measured and the adsorption capacity was calculated. 15 @MMT 15 The variation of adsorption amount with initial concentration is shown in Fig.14 shown; from Fig.14 It can be seen that as the initial oil concentration increases, the adsorption capacity also increases. When the initial oil concentration is 100 ppm, the maximum adsorption capacity reaches 1218.03 mg g -1 .

[0046] Application Example 5: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a conical flask, wherein uranyl ions (UO2 2+ ) concentration was 20ppm, and after adjusting the pH value to 6, 5mgPAA-TA 15 @MMT 15 The adsorbent was added to the uranium solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was carried out for 1440 min at a temperature of 25 ° C. The uranium ion concentration in the supernatant was measured; the adsorbed sample was then placed in 10 ml of 0.01 M HNO3, and desorbed for 2 h in a constant temperature shaker (25 ° C, 180 rpm), and the concentration of the supernatant was measured; the desorbed adsorbent was then directly used again in the batch adsorption experiment, and the cycle was repeated 3 times to calculate the adsorption and desorption amounts each time. PAA-TA 15 @MMT 15 The reuse performance of Fig.15 shown; from Fig.15It can be seen that after each elution, PAA-TA 15 @MMT 15 The desorption rates were all higher than 95%. During the third adsorption, the adsorption capacity still had 85% of the initial adsorption capacity.

[0047] Application Example 6: Acid-resistant polyacrylic acid hydrogel adsorbent PAA-TA prepared using Example 1 15 @MMT 15 The specific method for purifying uranium-containing wastewater is as follows: add 200 mL of uranium-containing solution into a series of conical flasks, in which uranyl ions (UO2 2+ ) concentration was 20ppm, and then competing ions were added, and the competing ions were Cu 2+ 、Al 3+ 、Zn 2+ 、Co 2+ , Mn 2+ 、Ni 2+ , Fe 2+ , Fe 3+ , all the above competitive ions, make the competitive ion concentration reach 20ppm, and then adjust the pH value to 6, then add 5mgPAA-TA 15 @MMT 15 The adsorbent was added to the uranium-containing solution; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption was carried out for 1200 min at a temperature of 25 ° C. The uranium ion concentration in the supernatant was measured by sampling; PAA-TA 15 @MMT 15 The adsorption performance of uranium-containing wastewater in the presence of competing ions is as follows Fig.16 shown; from Fig.16 It can be seen that even if all eight common metal competing ions were added at the same concentration, the adsorption of uranium still exceeded 50% of the blank group; the experimental results show that PAA-TA 15 @MMT 15 In the competing ion (Cu 2+ 、Al 3+ 、Zn 2+ 、Co 2+ , Mn 2+ 、Ni 2+ , Fe 2+ , Fe 3+ ) can still purify UO2 2+ ion.

[0048] PAA-TA in Application Example 1 15 @MMT 15 After adsorbing uranium at pH 6, the samples were air-dried and then tested by scanning electron microscopy. The microstructures were as follows: Fig.16 As shown by Fig.17 It can be seen that the adsorbed uranium ions are distributed in PAA-TA 15 @MMT 15 The surface of the adsorbent shows that the complexation of exposed hydroxyl and carboxyl groups with uranium plays a major role in the adsorption process.

[0049] The large number of carboxyl groups and hydroxyl groups on the surface of the acid-resistant polyacrylic acid hydrogel adsorbent prepared in Example 1 have a high adsorption capacity for uranium ions. The cross-linked structure formed by tannic acid and sodium montmorillonite enhances the stability of the adsorbent and effectively improves the regeneration performance and acid resistance.

Claims

1. A method for preparing an acid-resistant polyacrylic acid hydrogel adsorbent, characterized in that The method proceeds as follows:

1. Weigh N,N'-methylenebisacrylamide, tannic acid, sodium montmorillonite, acrylic acid and ammonium persulfate in a mass ratio of 1:(0.8-8.3):(0.8-8.3):(250-750):(30-35); 2. First, the acrylic acid weighed in step 1 is mixed with water to prepare an acrylic acid aqueous solution with a mass percentage concentration of 15% to 45%; then, the N,N'-methylenebisacrylamide, tannic acid and sodium montmorillonite weighed in step 1 are added to the acrylic acid aqueous solution, and stirred at room temperature for 20 to 60 minutes to obtain a mixed solution; then, the ammonium persulfate weighed in step 1 is added to the mixed solution, and stirred in an ice water bath for 5 to 15 minutes to obtain a precursor solution; 3. Pour the precursor solution into a container and place it in an oven at a temperature of 35-75°C for 20-40 minutes to obtain PAA-TA@MMT hydrogel; 4. Freeze-dry the PAA-TA@MMT hydrogel to obtain an acid-resistant polyacrylic acid hydrogel adsorbent, which is recorded as PAA-TA@MMT adsorbent.

2. The method for preparing an acid-resistant polyacrylic acid hydrogel adsorbent according to claim 1, characterized in that: The mass ratio of N,N'-methylenebisacrylamide, tannic acid, sodium montmorillonite, acrylic acid and ammonium persulfate described in step 1 is 1:(2-5):(2-5):(400-600):(32-34).

3. The method for preparing an acid-resistant polyacrylic acid hydrogel adsorbent according to claim 1 or 2, characterized in that: The freeze-drying temperature in step 4 is -30 to -50°C, and the freeze-drying time is 20 to 28 hours.

4. Application of an acid-resistant polyacrylic acid hydrogel adsorbent prepared by the method of claim 1, characterized in that The application is to use acid-resistant polyacrylic acid hydrogel adsorbent for the purification of uranium-containing wastewater.

5. The use of an acid-resistant polyacrylic acid hydrogel adsorbent according to claim 4, characterized in that The method for purifying uranium-containing wastewater using an acid-resistant polyacrylic acid hydrogel adsorbent is as follows: adding the acid-resistant polyacrylic acid hydrogel adsorbent to the uranium-containing wastewater, adjusting the pH to 5-7, stirring and adsorbing at a speed of 150-200 rpm for 600-1200 minutes at a temperature of 5-45°C, taking out the acid-resistant polyacrylic acid hydrogel adsorbent, and completing the purification of the uranium-containing wastewater.