Fiber type microbial platinum adsorbent and preparation method thereof
Through the preparation of fiber-type microbial platinum adsorbents, the combination of glycidyl methacrylate-acrylonitrile multipolymer and composite porous microspheres has been solved by solving the problems of high energy consumption and poor microbial adsorbent stability of the existing platinum recovery methods. It achieves efficient and stable adsorption and recovery of platinum ion.
Patent Information
- Application Number
- CN202411494144.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-24
AI Technical Summary
The existing platinum recovery methods have problems such as large reagent consumption, high energy consumption, easy to cause secondary contamination, incomplete reactions, and poor performance when dealing with low concentrations of platinum group metals, and the stability of microbial adsorbents is poor.
Using fiber-type microbial platinum adsorbent, fiber blanks are prepared by wet spinning with glycidyl methacrylate-acrylonitrile polycopolymer and composite porous microspheres, and the fiber blanks are prepared in polyethyleneimine, hydroxylamine hydrochloride and E. coli solutions. Insert impregnation, a fiber-type microbial platinum adsorbent with high mechanical properties and excellent adsorption effect is formed.
It improves the adsorption effect of platinum ions and the stability of the material, reduces recovery costs, reduces environmental pollution, and enhances the service life of fiber-type microbial platinum adsorbents.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal adsorbents, in particular to a fiber-type microbial platinum adsorbent and a preparation method thereof. Background Art
[0003] At present, the methods for recovering platinum mainly include traditional methods such as chemical precipitation, electrolysis, ion exchange and solvent extraction. However, these methods generally have problems such as large reagent consumption, high energy consumption, easy to cause secondary pollution, incomplete reaction and high operating cost, especially when dealing with low-concentration platinum group metals.
[0004] In recent years, polymer adsorption fibers or non-woven fabrics have shown great potential in the field of platinum ion enrichment and recovery due to their high adsorption capacity, simple operation process and excellent mechanical properties. This type of adsorbent is a new type of functional polymer material developed on the basis of ion exchange resin. Its preparation usually involves chemical modification of substrates such as natural fibers or synthetic fibers to introduce specific functional groups. Due to the good chemical stability and mechanical properties of the substrate, the adsorption fiber not only has high strength and corrosion resistance, but can also be reused many times. In addition, the fibers or related fabrics are easy to arrange and recycle in water bodies, which simplifies the adsorption and desorption steps in practical applications.
[0005] In addition, microbial adsorption materials, as a green, environmentally friendly and low-cost option, have also attracted the attention of researchers. Such adsorbents can be prepared from living or dead microorganisms and their metabolites, including but not limited to yeast, mold, bacteria and algae. They can effectively convert metal ions in water into accumulative forms through physical adsorption, ion exchange, complexation reaction and even redox reaction. Nevertheless, the effect of microbial adsorbents is easily affected by environmental factors such as solution pH and temperature, and their stability is relatively poor, which is also an area that needs further improvement.
[0006] In summary, exploring a new adsorbent that can effectively adsorb platinum ions and has good stability is of significant value in improving the recovery rate of platinum resources, reducing environmental pollution, and reducing recycling costs. Summary of the invention
[0007] The object of the present invention is to provide a fibrous microbial platinum adsorbent and a preparation method thereof, so as to solve the problems existing in the prior art.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a fibrous microbial platinum adsorbent, wherein the fibrous microbial platinum adsorbent is prepared by firstly compounding glycidyl methacrylate-acrylonitrile multipolymer and composite porous microspheres and then wet-spinning them to obtain a fiber blank, and then successively immersing the fiber blank in a polyethyleneimine solution, a hydroxylamine hydrochloride solution, and an Escherichia coli solution.
[0009] Furthermore, the glycidyl methacrylate-acrylonitrile multi-polymer is obtained by copolymerizing acrylonitrile, glycidyl methacrylate and triallylamine.
[0010] Furthermore, the composite porous microspheres are composited from nano-hydroxy calcium phosphate, collagen and oxidized bacterial cellulose.
[0011] Furthermore, the E. coli solution is prepared at a concentration of 10 8 ~10 10 CFU / L E. coli solution.
[0012] A method for preparing the aforementioned fibrous microbial platinum adsorbent comprises the following preparation steps: (1) A glycidyl acrylate-acrylonitrile multipolymer solution and a composite porous microsphere dispersion were mixed at a mass ratio of 1:0.9-1.1 to obtain a mixed spinning solution, and then the mixed spinning solution was extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a microinjection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and washed and dried with anhydrous ethanol and deionized water to obtain a fiber blank; (2) placing 40-42 parts by weight of the fiber blank in 200 parts by weight of polyethyleneimine solution, reacting for 3.8-4.2 hours under nitrogen protection and 75-85°C, then repeatedly washing the non-woven fabric with ethanol and deionized water to remove residual reagents on the surface, and then drying it in a vacuum oven at 60°C to constant weight to obtain a primary impregnated fiber; (3) placing the primary impregnated fiber obtained in step (2) in 190-210 parts by weight of hydroxylamine hydrochloride solution, reacting at 75-85° C. for 23.8-24.2 hours, washing in deionized water after the reaction and drying in a vacuum oven at 60° C. to constant weight to obtain a secondary impregnated fiber; (4) Place the secondary impregnated fiber obtained in step (3) at 10 8 ~10 10 The CFU / L Escherichia coli solution was shaken at 37°C and 120 r / min for 2-4 hours, removed, and centrifuged and dehydrated at 37°C for 10-20 minutes to obtain a fibrous microbial platinum adsorbent.
[0013] Furthermore, the preparation method of the glycidyl acrylate-acrylonitrile multi-polymer solution is as follows: under nitrogen protection conditions, 53-55 parts by mass of triallylamine, 23-24 parts by mass of acrylonitrile, and 4-6 parts by mass of glycidyl methacrylate are mixed and stirred at 300-500 rpm for 1-3 hours, and then 10-11 parts by mass of azobisisobutyronitrile and 10-11 parts by mass of tert-dodecyl mercaptan are added, and stirring is continued for 1-3 hours, and then added to a mixed solution of 512.5-544.5 parts by mass of dimethylformamide and 57-61 parts by mass of tetrahydrofuran at 59-61° C., stirred for reaction for 5.5-6.5 hours, and the temperature is raised to 84-86° C. and the reaction is continued for 25-35 minutes to obtain a glycidyl acrylate-acrylonitrile multi-polymer solution.
[0014] Furthermore, the preparation method of the composite porous microsphere dispersion is as follows: 24 to 26 parts by mass of composite porous microspheres are added to 100 parts by mass of dimethylformamide and ultrasonically dispersed for 30 to 50 minutes to obtain a composite porous microsphere dispersion.
[0015] Furthermore, the preparation method of the composite porous microspheres is as follows: collagen and oxidized bacterial cellulose are dissolved in deionized water in equal weight proportions, mixed, filtered, and freeze-dried to prepare a collagen-oxidized bacterial cellulose composite; 4 to 6 parts by weight of 1-allyl-3-methylimidazole chloride from which water has been removed, 0.18 to 0.22 parts by weight of the collagen-oxidized bacterial cellulose composite, 0.7 to 0.8 parts by weight of polystyrene, 0.7 to 0.8 parts by weight of nano-hydroxy calcium phosphate, and 2.4 to 2.6 parts by weight of Tween-8 0 is mixed evenly to obtain a dispersed phase; n-hexadecane and Span-80 are mixed evenly in a mass ratio of 1:2-4 to obtain a n-hexadecane continuous phase; 0.8-1.2 parts by mass of the dispersed phase and 10-12 parts by mass of the n-hexadecane continuous phase are stirred to form a W / O type emulsion, 90-110 parts by mass of n-butanol as a precipitant are added to the W / O type emulsion, stirred, and then allowed to stand to precipitate, and the microsphere precipitate is collected by suction filtration, washed with ethanol to remove the template agent styrene, and then washed with n-butanol, acetone, distilled water, repeatedly washed, filtered, and freeze-dried to obtain composite porous microspheres.
[0016] Furthermore, the preparation method of the polyethyleneimine solution is as follows: polyethyleneimine and 1,4-dioxane are mixed and stirred to dissolve in a mass ratio of 1:2-4 to obtain a polyethyleneimine solution.
[0017] Furthermore, the concentration of the hydroxylamine hydrochloride solution is 4-6%, and the solvent is water and dimethyl sulfoxide in a volume ratio of 1:0.8-1.2.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are: The fiber-type microbial platinum adsorbent of the present invention comprises the following steps: firstly, compounding a glycidyl methacrylate-acrylonitrile multi-copolymer and a composite porous microsphere, and then wet spinning the composite microsphere to obtain a fiber blank; then, the fiber blank is sequentially immersed in a polyethyleneimine solution, a hydroxylamine hydrochloride solution, and an Escherichia coli solution; the glycidyl methacrylate-acrylonitrile multi-copolymer is obtained by copolymerizing acrylonitrile, glycidyl methacrylate, and triallylamine; the composite porous microsphere is obtained by compounding nano-calcium hydroxyphosphate, collagen, and bacterial cellulose; and the polyethyleneimine solution is obtained by dissolving polyethyleneimine in dioxane.
[0019] Firstly, acrylonitrile, glycidyl methacrylate and triallylamine are copolymerized to obtain a glycidyl methacrylate-acrylonitrile copolymer with a hyperbranched structure. While a large number of cavities are formed in the glycidyl methacrylate-acrylonitrile copolymer, the crosslinking density of the glycidyl methacrylate-acrylonitrile copolymer is increased, thereby enhancing the mechanical properties of the glycidyl methacrylate-acrylonitrile copolymer.
[0020] Secondly, the glycidyl methacrylate-acrylonitrile multipolymer and the composite porous microspheres are compounded and wet-spun to obtain a fiber blank; the composite porous microspheres are compounded by nano-hydroxy calcium phosphate, collagen and bacterial cellulose; the composite porous microspheres are quickly dispersed in the glycidyl methacrylate-acrylonitrile multipolymer by nano-hydroxy calcium phosphate, thereby avoiding the problem of a large amount of agglomeration of the composite porous microspheres causing a decrease in the mechanical properties of the fiber blank, and increasing the service life of the fiber-type microbial platinum adsorbent.
[0021] Finally, the fiber blank is immersed in polyethyleneimine solution, hydroxylamine hydrochloride solution and Escherichia coli solution in turn to obtain a fiber-type microbial platinum adsorbent; the polyethyleneimine solution reacts with the epoxy group on the glycidyl methacrylate-acrylonitrile copolymer through part of the amino group to graft the polyethyleneimine molecular chain onto the fiber blank, introduce amino groups into the fiber blank, and then immersed in hydroxylamine hydrochloride solution to amine oxime the nitrile group in the fiber blank, further introduce amino groups into the fiber blank, which has good reaction activity and excellent metal ion adsorption effect, thereby enhancing the adsorption effect of the fiber-type microbial platinum adsorbent on platinum metal; further, the fiber blank The composite porous microspheres contain channels and cavities, which can adsorb E. coli solution, make E. coli attached to the secondary impregnated fibers, and combine the microbial adsorption material E. coli and the polymer adsorption fiber with each other, thereby enhancing the platinum adsorption effect of the fiber-type microbial platinum adsorbent. At the same time, the collagen and bacterial cellulose in the secondary impregnated fibers can be used as nutrients to feed E. coli and make E. coli reproduce, which can break the technical barrier of limited E. coli content in the microbial adsorption material polymer adsorption fiber after the microbial adsorption material E. coli and the polymer adsorption fiber are combined with each other, thereby further enhancing the platinum adsorption effect of the fiber-type microbial platinum adsorbent. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the fiber-type microbial platinum adsorbent prepared in the following examples are as follows: Platinum adsorption effect: 50 parts by mass of the fibrous microbial platinum adsorbent prepared in the embodiments and comparative examples were added to 500 parts by mass of a 100 mg / L chloroplatinic acid solution, the pH was adjusted to 7, constant temperature oscillation was performed at 25°C for 6 hours, the solution was filtered, and the concentration of platinum metal ions in the filtrate was determined by an atomic absorption spectrophotometer. Platinum adsorption rate = (100-concentration of platinum metal ions in the filtrate) * 100% / 100.
[0024] Mechanical properties: The tensile properties of the fiber-type microbial platinum adsorbents prepared in the examples and comparative examples were tested using a universal material tensile testing machine; a 50N mechanical sensor, a tensile speed of 1mm / min, a clamping distance of 3cm, each sample was tested 10 times, and the results were averaged.
[0025] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows: The preparation method of the Escherichia coli solution is as follows: Escherichia coli with a strain number of CICC 23917 and a Latin name of Escherichia coli provided by the China Industrial Microbiological Culture Collection Center is inoculated into LB medium, and cultured under shaking conditions of 37° C. and 120 r / min for 6 hours, during which the bacterial concentration is measured using an ultraviolet spectrophotometer, and the sample is centrifuged and freeze-dried overnight, and then dissolved in PBS buffer to obtain 10 8 ~10 10 CFU / L Escherichia coli solution; wherein the LB medium includes 10g of peptone, 5g of yeast extract, and 10g of sodium chloride, and is diluted to 1L with deionized water.
[0026] The preparation method of the collagen is as follows: take fresh pig skin, wash it thoroughly with water, dehair it, remove the fat layer, and cut it into 5mm×5mm leather pieces; weigh 5 parts by weight of the leather pieces and mix them with 10 parts by weight of degreasing agent acetone, stir and soak them at 4°C for 6 hours for degreasing treatment, change the degreasing agent every 2 hours during the degreasing period, wash them with deionized water 3 to 4 times after the treatment, dry them naturally, and store them at 4°C for standby use to obtain defatted leather pieces; weigh 5 parts by weight of the defatted leather pieces, wash them with 50 to 100 parts by weight of deionized water 4 times, then add 75 parts by weight of hydrochloric acid solution with a pH of 2.3, soak them at 4°C for 14 hours, stir them every 2 hours during the soaking period, wait until the leather pieces expand evenly, take out the leather pieces, add appropriate amount of deionized water to pulp them, obtain leather pulp, then add 4.0wt% pepsin to the leather pulp, and adjust the pH to 2 with the hydrochloric acid solution .3, enzymatic hydrolysis at 4℃ for 24h, centrifuge at 9000r / min for 20min, take the supernatant and slowly add 1mol / L sodium hydroxide solution to adjust the pH to about 7, slowly add solid sodium chloride while stirring to a sodium chloride concentration of 1.0mol / L, let it stand for 24h and centrifuge again, take the precipitate and add 0.1mol / L acetic acid solution to dissolve it, put it into a dialysis bag with a treated molecular weight cutoff of 11000kDa, and dialyze it in 0.05mol / L acetic acid solution for 3d, and replace the dialysate every 4h during the dialysis; then dialyze with distilled water, and replace the dialysate every 4h during the dialysis, until no white precipitate is produced in the dialysate detected by 10% silver nitrate solution, stop dialysis, freeze-dry the dialyzed solution to obtain collagen, and store it at 4℃ for later use.
[0027] The preparation method of the oxidized bacterial cellulose is as follows: 0.2 parts by mass of bacterial cellulose is weighed and placed in 50 parts by mass of deionized water for homogenization, the slurry is transferred to a 100 mL round-bottom flask, the round-bottom flask is wrapped with tin foil to avoid light, 0.1 parts by mass of an oxidant sodium metaperiodate is added, and an oil bath reaction is carried out at 40° C. and pH 6 for 14 hours. After the reaction is completed, the precipitate is collected and added with 0.1 mol / L ethylene glycol solution to continue the reaction for 0.8 hours to remove unreacted sodium metaperiodate. After the reaction is completed, the precipitate is collected and added with 0.1 mol / L ethylene glycol solution to continue the reaction for 0.8 hours to remove unreacted sodium metaperiodate. After the reaction is completed, the precipitate is collected and washed with deionized water for 5 times, the filter residue is collected, and freeze-dried to obtain the oxidized bacterial cellulose.
[0028] The weight average molecular weight of the polyethyleneimine is 600.
[0029] Example 1 A method for preparing a fibrous microbial platinum adsorbent comprises the following preparation steps: (1) A glycidyl acrylate-acrylonitrile multipolymer solution and a composite porous microsphere dispersion are mixed in a mass ratio of 1:0.9 to obtain a mixed spinning solution, and then the mixed spinning solution is extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a microinjection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and washed and dried with anhydrous ethanol and deionized water to obtain a fiber blank; (2) 40 parts by weight of the fiber blank was placed in 200 parts by weight of polyethyleneimine solution and nitrogen was introduced for 15 minutes, then sealed and reacted at 75°C for 3.8 hours, then the non-woven fabric was repeatedly washed with ethanol and deionized water to remove residual reagents on the surface, and then placed in a vacuum oven at 60°C to dry to constant weight to obtain a once impregnated fiber; (3) placing the primary impregnated fiber obtained in step (2) in 190 parts by weight of hydroxylamine hydrochloride solution and reacting at 75° C. for 23.8 hours, washing in deionized water after the reaction and drying in a vacuum oven at 60° C. to constant weight to obtain a secondary impregnated fiber; (4) Place the secondary impregnated fiber obtained in step (3) at 10 8 ~10 10 The CFU / L Escherichia coli solution was shaken at 37°C and 120r / min for 2h, removed, and centrifuged and dehydrated at 37°C for 10min to obtain a fibrous microbial platinum adsorbent.
[0030] The preparation method of the glycidyl acrylate-acrylonitrile multi-polymer solution is as follows: under nitrogen protection, 53 parts by mass of triallylamine, 23 parts by mass of acrylonitrile, and 4 parts by mass of glycidyl methacrylate are mixed and stirred at 300 rpm for 1 hour, and then 10 parts by mass of azobisisobutyronitrile and 10 parts by mass of tert-dodecyl mercaptan are added, and stirring is continued for 1 hour, and then the mixture is added to a mixed solution of 512.5 parts by mass of dimethylformamide and 57 parts by mass of tetrahydrofuran at 59° C., and stirred for reaction for 5.5 hours, and the temperature is raised to 84° C. and the reaction is continued for 25 minutes to obtain the glycidyl acrylate-acrylonitrile multi-polymer solution.
[0031] The preparation method of the composite porous microsphere dispersion is as follows: 24 parts by mass of composite porous microspheres are added to 100 parts by mass of dimethylformamide and ultrasonically dispersed for 30 minutes to obtain the composite porous microsphere dispersion.
[0032] The preparation method of the composite porous microspheres is as follows: weigh 0.2 parts by mass of collagen, add 30 parts by mass of deionized water, and stir at 30 rpm in a water bath at 40°C until the collagen is uniformly swollen, and keep stirring for 1 hour to obtain solution A; weigh 0.2 parts by mass of oxidized bacterial cellulose and 30 parts by mass of deionized water, mix them in a high-speed homogenizer for homogenization, and bathe them in a water bath at 40°C for 1 hour to obtain solution B; mix solution A and solution B, stir at 30 r / min for 20 minutes, then filter at room temperature, and then rinse with 40°C hot water to remove the remaining collagen, collect the filter residue, and freeze-dry to obtain a collagen-oxidized bacterial cellulose complex; weigh 4 parts by mass of 1-allyl-3-methylimidazole chloride, place it in a blast drying oven, dry it at 105°C for 3 hours to remove moisture, add 0.18 parts by mass of collagen-oxidized bacterial cellulose complex, and bathe it in an oil bath at 90°C until the collagen-oxidized bacterial cellulose complex is completely dissolved, and at the same time add 0.7 parts by mass of polystyrene olefins and 0.7 parts by mass of nano-calcium hydroxyphosphate were uniformly dispersed, and then 2.4 parts by mass of Tween-80 were added and mixed to obtain a dispersed phase; n-hexadecane and Span-80 were mixed in a mass ratio of 1:2 to obtain a n-hexadecane continuous phase; 0.8 parts by mass of the dispersed phase was slowly added to 10 parts by mass of the n-hexadecane continuous phase under magnetic stirring, and stirring was continued for 2 hours to form a W / O type emulsion, 90 parts by mass of precipitant n-butanol were added to the W / O type emulsion, and magnetic stirring was continued for 3 hours and then allowed to stand for 2 hours. After precipitation was complete, the microsphere precipitate was collected by suction filtration, 50 parts by mass of acetone were added to wash the microsphere precipitate to remove the template agent polystyrene, and 50 parts by mass of n-butanol, 50 parts by mass of acetone and 50 parts by mass of distilled water were used to wash in sequence under suction filtration. During washing, care should be taken not to drain the solvent, and the microsphere precipitate should be kept in a solvent-containing state to avoid collapse or damage of the microspheres caused by suction filtration. After washing, the obtained microspheres were transferred to a drying dish covered with tin foil and freeze-dried to obtain composite porous microspheres.
[0033] The preparation method of the polyethyleneimine solution is as follows: polyethyleneimine and 1,4-dioxane are mixed and stirred to dissolve in a mass ratio of 1:2-4 to obtain the polyethyleneimine solution.
[0034] The concentration of the hydroxylamine hydrochloride solution is 5%, and the solvent is a mixture of water and dimethyl sulfoxide in a volume ratio of 1:1.
[0035] Example 2 A method for preparing a fibrous microbial platinum adsorbent comprises the following preparation steps: (1) A glycidyl acrylate-acrylonitrile multi-polymer solution and a composite porous microsphere dispersion are mixed in a mass ratio of 1:1 to obtain a mixed spinning solution, and then the mixed spinning solution is extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a micro-injection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and washed and dried with anhydrous ethanol and deionized water to obtain a fiber blank; (2) 41 parts by weight of the fiber blank was placed in 200 parts by weight of polyethyleneimine solution and nitrogen was introduced for 15 minutes, then sealed and reacted at 80°C for 4 hours, then the non-woven fabric was repeatedly washed with ethanol and deionized water to remove residual reagents on the surface, and then placed in a vacuum oven at 60°C to dry to constant weight to obtain a primary impregnated fiber; (3) placing the primary impregnated fiber obtained in step (2) in 200 parts by weight of hydroxylamine hydrochloride solution and reacting at 80° C. for 24 hours, washing in deionized water after the reaction and drying in a vacuum oven at 60° C. to constant weight to obtain a secondary impregnated fiber; (4) Place the secondary impregnated fiber obtained in step (3) at 10 8 ~10 10 The CFU / L Escherichia coli solution was shaken at 37°C and 120r / min for 3h, removed, and centrifuged and dehydrated at 37°C for 15min to obtain a fibrous microbial platinum adsorbent.
[0036] The preparation method of the glycidyl acrylate-acrylonitrile multi-polymer solution is as follows: under nitrogen protection, 54 parts by mass of triallylamine, 23.5 parts by mass of acrylonitrile, and 5 parts by mass of glycidyl methacrylate are mixed and stirred at 400 rpm for 2 hours, then 10.5 parts by mass of azobisisobutyronitrile and 10.5 parts by mass of tert-dodecyl mercaptan are added, and stirring is continued for 2 hours, and then the mixture is added to a mixed solution of 529.5 parts by mass of dimethylformamide and 59 parts by mass of tetrahydrofuran at 60° C., stirred for reaction for 6 hours, and the temperature is raised to 85° C. and the reaction is continued for 30 minutes to obtain the glycidyl acrylate-acrylonitrile multi-polymer solution.
[0037] The preparation method of the composite porous microsphere dispersion is as follows: 25 parts by mass of composite porous microspheres are added to 100 parts by mass of dimethylformamide and ultrasonically dispersed for 40 minutes to obtain the composite porous microsphere dispersion.
[0038] The preparation method of the composite porous microspheres is as follows: weigh 0.2 parts by mass of collagen, add 30 parts by mass of deionized water, place in a water bath at 40°C and stir at 40 rpm until the collagen is uniformly swollen, and keep stirring for 1 hour to obtain solution A; weigh 0.2 parts by mass of oxidized bacterial cellulose and 30 parts by mass of deionized water, mix them in a high-speed homogenizer for homogenization, and place them in a water bath at 40°C for 1 hour to obtain solution B; mix solution A and solution B, stir at 40 r / min for 20 minutes, then filter at room temperature, and then rinse with 40°C hot water to remove the remaining collagen, collect the filter residue, and freeze-dry to obtain a collagen-oxidized bacterial cellulose complex; weigh 5 parts by mass of 1-allyl-3-methylimidazole chloride, place it in a blast drying oven, dry it at 105°C for 3 hours to remove moisture, add 0.2 parts by mass of collagen-oxidized bacterial cellulose complex, and place it in an oil bath at 90°C until the collagen-oxidized bacterial cellulose complex is completely dissolved, and at the same time add 0.75 parts by mass of polystyrene olefins, 0.75 parts by mass of nano-calcium hydroxyphosphate were uniformly dispersed, and then 2.5 parts by mass of Tween-80 were added and mixed to obtain a dispersed phase; n-hexadecane and Span-80 were mixed in a mass ratio of 1:3 to obtain a n-hexadecane continuous phase; 1 part by mass of the dispersed phase was slowly added to 11 parts by mass of the n-hexadecane continuous phase under magnetic stirring, and stirring was continued for 2 hours to form a W / O type emulsion, 100 parts by mass of precipitant n-butanol were added to the W / O type emulsion, and magnetic stirring was performed for 3 hours and then allowed to stand for 2 hours. After precipitation was complete, the microsphere precipitate was collected by suction filtration, 50 parts by mass of acetone were added to wash the microsphere precipitate to remove the template agent polystyrene, and 50 parts by mass of n-butanol, 50 parts by mass of acetone and 50 parts by mass of distilled water were used to wash in sequence under suction filtration. During washing, care should be taken not to drain the solvent, and the microsphere precipitate should be kept in a solvent-containing state to avoid collapse or damage of the microspheres caused by suction filtration. After washing, the obtained microspheres were transferred to a drying dish covered with tin foil and freeze-dried to obtain composite porous microspheres.
[0039] The preparation method of the polyethyleneimine solution is as follows: polyethyleneimine and 1,4-dioxane are mixed and stirred to dissolve in a mass ratio of 1:3 to obtain the polyethyleneimine solution.
[0040] The concentration of the hydroxylamine hydrochloride solution is 5%, and the solvent is water and dimethyl sulfoxide in a volume ratio of 1:1.
[0041] Example 3 A method for preparing a fibrous microbial platinum adsorbent comprises the following preparation steps: (1) A glycidyl acrylate-acrylonitrile multipolymer solution and a composite porous microsphere dispersion are mixed in a mass ratio of 1:1.1 to obtain a mixed spinning solution, and then the mixed spinning solution is extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a micro-injection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and washed and dried with anhydrous ethanol and deionized water to obtain a fiber blank; (2) 42 parts by weight of the fiber blank was placed in 200 parts by weight of polyethyleneimine solution and nitrogen was introduced for 15 minutes, then sealed and reacted at 85°C for 4.2 hours, then the non-woven fabric was repeatedly washed with ethanol and deionized water to remove residual reagents on the surface, and then placed in a vacuum oven at 60°C to dry to constant weight to obtain a once impregnated fiber; (3) placing the primary impregnated fiber obtained in step (2) in 210 parts by weight of hydroxylamine hydrochloride solution, reacting at 85° C. for 24.2 hours, washing in deionized water after the reaction, and drying in a vacuum oven at 60° C. to constant weight to obtain a secondary impregnated fiber; (4) Place the secondary impregnated fiber obtained in step (3) at 10 8 ~10 10 The CFU / L Escherichia coli solution was shaken at 37°C and 120r / min for 4h, removed, and centrifuged and dehydrated at 37°C for 20min to obtain a fibrous microbial platinum adsorbent.
[0042] The preparation method of the glycidyl acrylate-acrylonitrile multi-polymer solution is as follows: under nitrogen protection, 55 parts by mass of triallylamine, 24 parts by mass of acrylonitrile, and 6 parts by mass of glycidyl methacrylate are mixed and stirred at 500 rpm for 3 hours, then 11 parts by mass of azobisisobutyronitrile and 11 parts by mass of tert-dodecyl mercaptan are added, and stirring is continued for 3 hours, and then the mixture is added to a mixed solution of 544.5 parts by mass of dimethylformamide and 61 parts by mass of tetrahydrofuran at 61° C., stirred for reaction for 6.5 hours, and the temperature is raised to 86° C. and the reaction is continued for 35 minutes to obtain the glycidyl acrylate-acrylonitrile multi-polymer solution.
[0043] The preparation method of the composite porous microsphere dispersion is as follows: 26 parts by mass of composite porous microspheres are added to 100 parts by mass of dimethylformamide and ultrasonically dispersed for 50 minutes to obtain the composite porous microsphere dispersion.
[0044] The preparation method of the composite porous microspheres is as follows: weigh 0.2 parts by mass of collagen, add 30 parts by mass of deionized water, bath in a water bath at 40°C and stir at 50 rpm until the collagen is uniformly swollen, and keep stirring for 1 hour to obtain solution A; weigh 0.2 parts by mass of oxidized bacterial cellulose and 30 parts by mass of deionized water, mix them in a high-speed homogenizer for homogenization, bath in a water bath at 40°C for 1 hour to obtain solution B; mix solution A and solution B, stir at 50 r / min for 20 minutes, then filter at room temperature, then rinse with 40°C hot water to remove the remaining collagen, collect the filter residue, and freeze-dry to obtain a collagen-oxidized bacterial cellulose complex; weigh 6 parts by mass of 1-allyl-3-methylimidazole chloride, place it in a blast drying oven, dry it at 105°C for 3 hours to remove moisture, add 0.22 parts by mass of collagen-oxidized bacterial cellulose complex, bath in an oil bath at 90°C until the collagen-oxidized bacterial cellulose complex is completely dissolved, and at the same time add 0.8 parts by mass of polystyrene , 0.8 parts by mass of nano-calcium hydroxyphosphate to make it evenly dispersed, then 2.6 parts by mass of Tween-80 were added and mixed evenly to obtain a dispersed phase; n-hexadecane and Span-80 were mixed evenly in a mass ratio of 1:4 to obtain a n-hexadecane continuous phase; 1.2 parts by mass of the dispersed phase was slowly added to 12 parts by mass of the n-hexadecane continuous phase under magnetic stirring, and stirring was continued for 2 hours to form a W / O type emulsion, 110 parts by mass of precipitant n-butanol was added to the W / O type emulsion, and magnetic stirring was performed for 3 hours and then allowed to stand for 2 hours. After precipitation was complete, the microsphere precipitate was collected by suction filtration, 50 parts by mass of acetone was added to wash the microsphere precipitate to remove the template agent polystyrene, and 50 parts by mass of n-butanol, 50 parts by mass of acetone, and 50 parts by mass of distilled water were used to wash in sequence under suction filtration. During washing, care should be taken not to drain the solvent, and the microsphere precipitate should be kept in a solvent-containing state to avoid collapse or damage of the microspheres caused by suction filtration. After washing, the obtained microspheres were transferred to a drying dish covered with tin foil and freeze-dried to obtain composite porous microspheres.
[0045] The preparation method of the polyethyleneimine solution is as follows: polyethyleneimine and 1,4-dioxane are mixed and stirred to dissolve in a mass ratio of 1:4 to obtain the polyethyleneimine solution.
[0046] The concentration of the hydroxylamine hydrochloride solution is 6%, and the solvent is water and dimethyl sulfoxide in a volume ratio of 1:1.2.
[0047] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is only the preparation method of the glycidyl acrylate-acrylonitrile multi-copolymer solution. The preparation method of the glycidyl acrylate-acrylonitrile multi-copolymer solution of Comparative Example 1 is as follows: Under nitrogen protection, 54 parts by mass of butadiene, 23.5 parts by mass of acrylonitrile, and 5 parts by mass of glycidyl methacrylate are mixed and stirred at 400 rpm for 2 hours, and then 10.5 parts by mass of azobisisobutyronitrile and 10.5 parts by mass of tert-dodecyl mercaptan are added, and stirring is continued for 2 hours, and then added to a mixed solution of 529.5 parts by mass of dimethylformamide and 59 parts by mass of tetrahydrofuran at 60° C., stirred for reaction for 6 hours, and heated to 85° C. and continued to react for 30 minutes to obtain a glycidyl acrylate-acrylonitrile multi-copolymer solution; the remaining components, proportions and processes are the same as those in Example 2.
[0048] Comparative Example 2 The difference between Comparative Example 2 and Example 2 lies only in the preparation of the composite porous microspheres. The preparation method of the composite porous microspheres in Comparative Example 2 is as follows: weigh 0.2 parts by mass of collagen, add 30 parts by mass of deionized water, place in a water bath at 40°C and stir at 40 rpm until the collagen is evenly swollen, and keep stirring for 1 hour to obtain solution A; weigh 0.2 parts by mass of oxidized bacterial cellulose and 30 parts by mass of deionized water, place in a high-speed homogenizer for homogenization, and place in a water bath at 40°C for 1 hour to obtain solution B; mix solution A with solution B, stir at 40 r / min for 20 minutes, then filter at room temperature, and then rinse with 40°C hot water to remove the remaining collagen, collect the filter residue, and freeze-dry to obtain a collagen-oxidized bacterial cellulose complex; weigh 5 parts by mass of 1-allyl-3-methylimidazole chloride, place in a blast drying oven, dry at 105°C for 3 hours to remove moisture, add 0.2 parts by mass of collagen-oxidized bacterial cellulose complex, and place in a 90°C oil bath until the collagen-oxidized bacterial cellulose complex is completely dissolved, and add 0.75 parts by mass of polystyrene was added to make it dispersed evenly, and then 2.5 parts by mass of Tween-80 was added and mixed evenly to obtain a dispersed phase; n-hexadecane and Span-80 were mixed evenly in a mass ratio of 1:3 to obtain a n-hexadecane continuous phase; 1 part by mass of the dispersed phase was slowly added to 11 parts by mass of the n-hexadecane continuous phase under magnetic stirring, and stirring was continued for 2 hours to form a W / O type emulsion, and 100 parts by mass of a precipitant n-butanol was added to the W / O type emulsion, and magnetic stirring was performed for 3 hours and then allowed to stand for 2 hours until precipitation was complete. The microsphere precipitate was collected by suction filtration, 50 parts by mass of acetone was added to wash the microsphere precipitate to remove the template polystyrene, and then 50 parts by mass of n-butanol, 50 parts by mass of acetone, and 50 parts by mass of distilled water were used for washing in sequence under suction filtration. During washing, care should be taken not to drain out the solvent, and to keep the microsphere precipitate in a solvent-containing state to avoid collapse or damage of the microspheres caused by suction filtration. After washing, the obtained microspheres were transferred to a drying dish covered with tin foil and freeze-dried to obtain composite porous microspheres. The remaining components, proportions, and processes were the same as those in Example 2.
[0049] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is only the preparation method of the fiber blank: the glycidyl acrylate-acrylonitrile copolymer solution is extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a microinjection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and the fiber blank is obtained after washing and drying with anhydrous ethanol and deionized water; the remaining components, proportions and processes are the same as those in Example 2.
[0050] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is only the preparation steps of the fiber-type microbial platinum adsorbent: (1) A glycidyl acrylate-acrylonitrile multi-polymer solution and a composite porous microsphere dispersion are mixed in a mass ratio of 1:1 to obtain a mixed spinning solution, and then the mixed spinning solution is extruded into an ethyl acetate coagulation bath at a uniform speed of 8 mL / h through a micro-injection pump equipped with a 22G spinning needle with a diameter of 0.4 mm, and formed in the coagulation bath, and then wound and collected, and washed and dried with anhydrous ethanol and deionized water to obtain a fiber blank; (2) Place 41 parts by mass of the fiber blank in 200 parts by mass of hydroxylamine hydrochloride solution and react at 80°C for 24 hours. After the reaction, wash it in deionized water and use a vacuum oven at 60°C to dry it to constant weight to obtain a fiber-type microbial platinum adsorbent; the remaining components, proportions and processes are the same as in Example 2.
[0051] Comparative Example 5 The difference between Comparative Example 5 and Example 2 is that only the fiber blank is immersed in the polyethyleneimine solution to obtain the fiber-type microbial platinum adsorbent; the other components, proportions and processes are the same as those in Example 2.
[0052] Comparative Example 6 The only difference between Comparative Example 6 and Example 2 is that the fiber blank is immersed in polyethyleneimine solution and hydroxylamine hydrochloride solution in sequence to obtain a fiber-type microbial platinum adsorbent; the remaining components, proportions and processes are the same as those in Example 2.
[0053] Comparative Example 7 Comparative Example 7 uses Escherichia coli solution as the platinum adsorbent.
[0054] Effect example Table 1 below shows the performance analysis results of the fiber-type microbial platinum adsorbents of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.
[0055] Table 1 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 6 in Table 1, it can be found that the fibrous microbial platinum adsorbent prepared in the examples has better platinum adsorption effect and better mechanical properties; from the comparison of the experimental data of Examples 1 to 3 and Comparative Example 1, it can be found that the fibrous microbial platinum adsorbent prepared by copolymerizing acrylonitrile, glycidyl methacrylate and triallylamine to obtain a glycidyl methacrylate-acrylonitrile multipolymer has better platinum adsorption effect and better mechanical properties, and acrylonitrile, glycidyl methacrylate and triallylamine are copolymerized to obtain a glycidyl methacrylate-acrylonitrile multipolymer with a hyperbranched structure, while a large number of cavities are formed in the glycidyl methacrylate-acrylonitrile multipolymer, while the glycidyl methacrylate-acrylonitrile is increased. The cross-linking density of the multi-copolymer is increased, thereby enhancing the mechanical properties of the glycidyl methacrylate-acrylonitrile multi-copolymer. When the fiber blank prepared from the glycidyl methacrylate-acrylonitrile multi-copolymer is subsequently immersed in a polyethyleneimine solution, a hydroxylamine hydrochloride solution, and an Escherichia coli solution, the polyethyleneimine solution reacts with the epoxy groups on the glycidyl methacrylate-acrylonitrile multi-copolymer through part of the amino groups, grafts the polyethyleneimine molecular chains onto the fiber blank, introduces amino groups into the fiber blank, and then immerses the fiber blank in a hydroxylamine hydrochloride solution to amine oxime the nitrile groups in the fiber blank, further introducing amino groups into the fiber blank, having good reaction activity and excellent metal ion adsorption effect, thereby enhancing the adsorption effect of the fiber-type microbial platinum adsorbent on platinum metal; Comparison of the experimental data of Examples 1 to 3 and Comparative Examples 2 to 3 shows that the fiber blank is prepared by using composite porous microspheres obtained by compounding nano-calcium hydroxyphosphate, collagen, and bacterial cellulose, and the obtained fiber-type microbial platinum adsorbent has good platinum adsorption effect and good mechanical properties. It can be seen that the addition of nano-calcium hydroxyphosphate can improve the platinum adsorption effect of the fiber-type microbial platinum adsorbent; By comparing the experimental data of Examples 1 to 3 and Comparative Examples 4 to 6, it can be found that the fiber blank is immersed in a polyethyleneimine solution, a hydroxylamine hydrochloride solution, and an Escherichia coli solution in sequence, and the obtained fiber-type microbial platinum adsorbent has a good platinum adsorption effect; wherein the polyethyleneimine solution reacts with the epoxy group on the glycidyl methacrylate-acrylonitrile multipolymer in the fiber blank through part of the amino group, grafts the polyethyleneimine molecular chain to the fiber blank, introduces the amino group into the fiber blank, and then immerses it in a hydroxylamine hydrochloride solution, and the nitrile group in the fiber blank is subjected to amine oxime, and further introduces the amino group into the fiber blank, which has good reaction activity and excellent metal ion adsorption effect, and enhances the adsorption effect of the fiber-type microbial platinum adsorbent on platinum metal; Compared with Example 7, the fibrous microbial platinum adsorbent prepared in Examples 1 to 3 has a better platinum adsorption effect than the traditional platinum adsorption using Escherichia coli.
[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A fiber-type microbial platinum adsorbent, It is characterized in that The fiber-type microbial platinum adsorbent is obtained by firstly compounding glycidyl methacrylate-acrylonitrile multi-polymer and composite porous microspheres and then wet spinning to obtain a fiber blank, and then successively immersing the fiber blank in polyethyleneimine solution, hydroxylamine hydrochloride solution and Escherichia coli solution.
2. The fiber-type microbial platinum adsorbent according to claim 1, It is characterized in that The glycidyl methacrylate-acrylonitrile multi-polymer is obtained by copolymerizing acrylonitrile, glycidyl methacrylate and triallylamine.
3. The fiber-type microbial platinum adsorbent according to claim 1, It is characterized in that The composite porous microspheres are obtained by compounding nanometer hydroxy calcium phosphate, collagen and oxidized bacterial cellulose.
4. The fiber-type microbial platinum adsorbent according to claim 1, It is characterized in that The E. coli solution has a concentration of 10 8 ~10 10 CFU / L of E. coli solution.
5. A method for preparing the fibrous microbial platinum adsorbent according to any one of claims 1 to 4, It is characterized in that The method comprises the following preparation steps: (1) mixing a glycidyl acrylate-acrylonitrile multi-polymer solution with a composite porous microsphere dispersion at a mass ratio of 1:0.9-1.1 to obtain a mixed spinning solution, then extruding the mixed spinning solution into an ethyl acetate coagulation bath at a uniform speed, and forming the mixed spinning solution in the coagulation bath, and then winding and collecting the mixed spinning solution, and washing and drying the mixed spinning solution with anhydrous ethanol and deionized water to obtain a fiber blank; (2) placing 40-42 parts by weight of the fiber blank in 200 parts by weight of polyethyleneimine solution, reacting for 3.8-4.2 hours under nitrogen protection and 75-85°C, then repeatedly washing the non-woven fabric with ethanol and deionized water to remove residual reagents on the surface, and drying to constant weight to obtain a primary impregnated fiber; (3) placing the primary impregnated fiber obtained in step (2) in 190-210 parts by weight of hydroxylamine hydrochloride solution, reacting at 75-85° C. for 23.8-24.2 hours, and washing in deionized water and drying to constant weight after the reaction to obtain a secondary impregnated fiber; (4) Place the secondary impregnated fiber obtained in step (3) at 10 8 ~10 10 coli solution with a concentration of 0.1447 W / L, shaken, fished out, and centrifuged for dehydration to obtain a fibrous microbial platinum adsorbent.
6. The method for preparing the fiber-type microbial platinum adsorbent according to claim 5, It is characterized in that The preparation method of the glycidyl acrylate-acrylonitrile multi-polymer solution is as follows: under nitrogen protection, 53-55 parts by mass of triallylamine, 23-24 parts by mass of acrylonitrile, and 4-6 parts by mass of glycidyl methacrylate are mixed and stirred at 300-500 rpm for 1-3 hours, then 10-11 parts by mass of azobisisobutyronitrile and 10-11 parts by mass of tert-dodecyl mercaptan are added, stirring is continued for 1-3 hours, and then the mixture is added to a mixed solution of 512.5-544.5 parts by mass of dimethylformamide and 57-61 parts by mass of tetrahydrofuran at 59-61° C., stirred for reaction for 5.5-6.5 hours, and heated to 84-86° C. to continue reaction for 25-35 minutes to obtain the glycidyl acrylate-acrylonitrile multi-polymer solution.
7. The method for preparing the fiber-type microbial platinum adsorbent according to claim 5, It is characterized in that The preparation method of the composite porous microsphere dispersion is as follows: 24 to 26 parts by mass of composite porous microspheres are added to 100 parts by mass of dimethylformamide and ultrasonically dispersed for 30 to 50 minutes to obtain the composite porous microsphere dispersion.
8. The method for preparing the fiber-type microbial platinum adsorbent according to claim 7, It is characterized in that The preparation method of the composite porous microspheres is as follows: collagen and oxidized bacterial cellulose are dissolved in deionized water in equal weight proportions, mixed, filtered, and freeze-dried to prepare a collagen-oxidized bacterial cellulose composite; 4 to 6 weight parts of 1-allyl-3-methylimidazole chloride from which water has been removed, 0.18 to 0.22 weight parts of the collagen-oxidized bacterial cellulose composite, 0.7 to 0.8 weight parts of polystyrene, 0.7 to 0.8 weight parts of nano-hydroxy calcium phosphate, and 2.4 to 2.6 weight parts of Tween-80 are mixed. The mixture was mixed evenly to obtain a dispersed phase; n-hexadecane and Span-80 were mixed evenly at a mass ratio of 1:2-4 to obtain a n-hexadecane continuous phase; 0.8-1.2 parts by mass of the dispersed phase and 10-12 parts by mass of the n-hexadecane continuous phase were stirred to form a W / O type emulsion; 90-110 parts by mass of a precipitant n-butanol were added to the W / O type emulsion, stirred, and then allowed to stand to precipitate; the microsphere precipitate was collected by suction filtration; after washing with ethanol to remove the template agent styrene, n-butanol, acetone, distilled water, repeated washing, suction filtration, and freeze-drying were used in sequence to obtain composite porous microspheres.
9. The method for preparing the fiber-type microbial platinum adsorbent according to claim 5, It is characterized in that The preparation method of the polyethyleneimine solution is as follows: polyethyleneimine and 1,4-dioxane are mixed and stirred to dissolve in a mass ratio of 1:2-4 to obtain the polyethyleneimine solution.
10. The method for preparing the fiber-type microbial platinum adsorbent according to claim 5, It is characterized in that The concentration of the hydroxylamine hydrochloride solution is 4-6%, and the solvent is water and dimethyl sulfoxide in a volume ratio of 1:0.8-1.2.
Citation Information
Patent Citations
Method for preparing polystyrene microsphere-type cellulose-based heavy metal adsorbent
AU2020101319A4
Preparation method of noble metal platinum-doped fluorescent bacterial cellulose
CN110066423A
Double metal oxide-hyperbranched polymer adsorbent and preparation method thereof
CN110756178A
Endotoxin adsorbent as well as preparation method and application thereof
CN114669282A
Preparation method of magnetic cellulose-based polyamine chelating heavy metal adsorbent