Adsorbing material for organic wastewater treatment and preparation method thereof
By adjusting the biochar raw materials and processes, efficient adsorption materials are prepared, which solves the problems of large consumption and poor regeneration performance in organic wastewater treatment by adsorption, and efficient and economical organic wastewater treatment is achieved, reducing environmental burden.
Patent Information
- Application Number
- CN202411501441.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-25
AI Technical Summary
The existing adsorption method consumes a large amount of consumption and is easy to saturate in organic wastewater treatment, has a long treatment time, is high operating cost, and has poor regeneration performance, which affects the treatment efficiency and economicality.
By adjusting the source and ratio of biochar raw materials, combining high-temperature carbonization and heat treatment processes, efficient adsorption materials are prepared to improve their regeneration performance and treatment efficiency. The specific steps include carbonizing the straw and cyanobacteria powder at high temperature under argon conditions, mixing it with the treatment solution for heat treatment, forming a biochar adsorption material with rich pore structure and surface functional groups.
It significantly improves the regeneration performance of adsorbent materials, shortens processing time, improves processing efficiency, and reduces operating costs. It is suitable for large-scale industrial production, and has good environmental benefits and application prospects.
Smart Images

Figure CN119075956A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic wastewater treatment, and in particular to an adsorption material for organic wastewater treatment and a preparation method thereof. Background Art
[0002] With the rapid development of the industrial economy, a large amount of organic wastewater is inevitably generated in the production process of various industries. These organic wastewaters are rich in various chemical substances. Due to their poor biodegradability and large differences in relative molecular mass, they are very challenging to treat. If these organic wastewaters are discharged directly without treatment, they will seriously harm the ecological environment and the quality of water bodies. In addition, this type of organic wastewater also contains a large amount of toxic substances, and traditional biodegradation treatment methods can no longer meet the requirements of relevant treatment standards.
[0003] There are many methods for treating organic wastewater, mainly including physical treatment, chemical treatment, physicochemical treatment and biological treatment. Physical treatment methods such as screens, sedimentation and regulating tanks are mainly used to remove large particles and suspended solids; chemical treatment methods such as coagulation and oxidation-reduction are used to remove some soluble organic matter; physicochemical treatment methods such as adsorption (using adsorbents such as activated carbon and molecular sieves) and membrane separation technology (such as reverse osmosis, nanofiltration, etc.) are used to remove small molecular organic matter; biological treatment methods include aerobic treatment (activated sludge method, biofilm method) and anaerobic treatment (UASB, anaerobic filter), using microorganisms to degrade organic matter; advanced oxidation processes such as Fenton reagent, ozone oxidation and ultraviolet photocatalysis are used for difficult-to-degrade organic matter; evaporation concentration and pyrolysis / incineration evaporate and concentrate high-concentration wastewater, and the concentrate can be thoroughly treated by pyrolysis or incineration. These methods can be combined according to the specific properties and treatment requirements of the wastewater to achieve the best treatment effect.
[0004] The adsorption method has the advantages of good treatment effect, simple operation, small footprint, and no secondary pollution in the treatment of organic wastewater. However, the adsorption material used in the adsorption method is highly consuming, easily saturated, and requires frequent replacement, which increases the operating cost, takes a long time to process, is difficult to regenerate the adsorbent, and has a complex process and high cost, which affects the economic efficiency.
[0005] Therefore, how to improve the adsorption performance, adsorption efficiency and regeneration performance of adsorption materials is of great significance to improving the efficiency and economy of organic wastewater treatment, reducing environmental burden and promoting sustainable development. Summary of the invention
[0006] In view of this, the present invention provides an adsorption material for treating organic wastewater and a preparation method thereof. The present invention significantly improves the regeneration performance of the adsorption material by adjusting the source and ratio of the biochar raw material and combining the adjustment of the preparation process, and also shortens the treatment time of the adsorption material to a certain extent and improves the treatment efficiency.
[0007] The method for preparing the adsorbent material for treating organic wastewater of the present invention comprises the following steps:
[0008] S1, drying and crushing the straw and blue algae respectively, and passing through a 80-100 mesh sieve to obtain straw powder and blue algae powder;
[0009] S2, mixing straw powder and cyanobacteria powder to obtain a mixed powder, adding sodium hydroxide and carbonizing at high temperature under argon gas to obtain biochar;
[0010] S3, mixing the biochar with the treatment liquid, heat treating it, and cooling it to obtain an adsorption material for organic wastewater treatment.
[0011] Furthermore, the drying temperature is 100° C. to 120° C., and the drying time is 8 to 12 hours.
[0012] Furthermore, the mass ratio of the straw powder to the blue algae powder is (3-5): 1. Preferably, the mass ratio of the straw powder to the blue algae powder is 4:1.
[0013] Further, the mass ratio of the sodium hydroxide to the mixed powder is (1-2): 1. Preferably, the mass ratio of the sodium hydroxide to the mixed powder is 1.5:1.
[0014] Furthermore, the carbonization temperature is 800°C to 900°C, and the carbonization time is 2 to 3 hours. Preferably, the carbonization temperature is 850°C, and the carbonization time is 2.5 hours.
[0015] Furthermore, the treatment solution includes 300-500 mg·L -1 of ferric chloride and 350-600 mg·L -1 Preferably, the treatment solution includes 350 mg·L -1 of ferric chloride and 450mg·L -1 of sodium chloride.
[0016] Furthermore, the solid-liquid ratio of the biochar to the treatment liquid is 5 to 15 g / mL. Preferably, the solid-liquid ratio of the biochar to the treatment liquid is 10 g / mL.
[0017] Furthermore, the heat treatment is carried out in two steps, the first step is low-temperature pre-sintering, the low-temperature pre-sintering temperature is 80-120°C, the holding time is 30-60min, and the heating rate is 5°C / min-10°C / min, and the second step is high-temperature calcining, the high-temperature calcining temperature is 250°C-350°C, the holding time is 60-90min, and the heating rate is 2°C / min-5°C / min. Preferably, the low-temperature pre-sintering temperature is 100°C, the holding time is 45min, and the heating rate is 8°C / min, and the high-temperature calcining temperature is 320°C, the holding time is 60min, and the heating rate is 3°C / min.
[0018] The present invention also provides an adsorption material for treating organic wastewater prepared according to the method.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] The present invention significantly improves the regeneration performance of the adsorption material, shortens the processing time, and improves the processing efficiency by adjusting the source and ratio of the biochar raw materials and optimizing the preparation process.
[0021] The present invention adopts straw and blue algae as raw materials, and combines the biochar prepared under high-temperature carbonization conditions with sodium hydroxide, which has rich pore structure and surface functional groups, and enhances the adsorption capacity of organic pollutants.
[0022] The invention utilizes biomass waste as raw material, reduces waste discharge, and has good environmental benefits.
[0023] The preparation method of the adsorption material provided by the invention is simple and feasible, suitable for large-scale industrial production, and has broad application prospects in the field of organic wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described below in conjunction with the accompanying drawings.
[0025] Figure 1 The present invention is a flow chart of the preparation process of the adsorption material for treating organic wastewater. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing an adsorbent material for treating organic wastewater, comprising the following steps:
[0027] S1, drying and crushing the straw and blue algae respectively, and passing through a 80-100 mesh sieve to obtain straw powder and blue algae powder;
[0028] S2, mixing straw powder and cyanobacteria powder to obtain a mixed powder, adding sodium hydroxide and carbonizing at high temperature under argon gas to obtain biochar;
[0029] S3, mixing the biochar with the treatment liquid, heat treating it, and cooling it to obtain an adsorption material for organic wastewater treatment.
[0030] In one embodiment, the drying temperature is 100° C. to 120° C., and the drying time is 8 to 12 hours.
[0031] In one embodiment, the mass ratio of the straw powder to the blue algae powder is (3-5):1.
[0032] In one embodiment, the mass ratio of the straw powder to the blue algae powder is 4:1.
[0033] Eutrophication of water bodies accelerates the eutrophication of lakes, promotes cyanobacterial blooms and red tides, causes water quality to deteriorate, and reduces dissolved oxygen, thereby affecting the survival of aquatic plants and animals. Therefore, the resource processing of cyanobacteria has a relatively positive impact on solving this problem. To this end, the present invention selects cyanobacteria as a partial raw material source for the preparation of biochar, which can achieve the resource processing of cyanobacteria to a certain extent and reduce the adverse effects of eutrophication of water bodies. In addition, the salvaged cyanobacteria after dehydration contain metal elements, which can be incorporated into biochar through pyrolysis and subsequent biochar modification and activation, enhance its adsorption capacity, and have a certain positive impact on the microstructure of the material, thereby improving the adsorption performance and regeneration performance of the material.
[0034] In addition, the present invention has a relatively strict limit on the ratio of straw powder to the blue algae powder, because this ratio can control costs while ensuring adsorption performance, optimize pore structure and specific surface area, and ensure the stability of biochar during carbonization. Too low a dosage of blue algae powder will result in low metal content and poor pore structure in biochar, while too high a dosage of blue algae powder will result in pore blockage and reduced material adsorption performance.
[0035] In one embodiment, the mass ratio of the sodium hydroxide to the mixed powder is (1-2):1.
[0036] In one embodiment, the mass ratio of the sodium hydroxide to the mixed powder is 1.5:1.
[0037] Sodium hydroxide and potassium hydroxide are commonly used for the activation of biochar, but actual research shows that potassium hydroxide is not suitable for the present invention. Experiments show that compared with potassium hydroxide, biochar activated with sodium hydroxide has more mesopores. More mesopores are beneficial to improving the treatment effect of subsequent treatment liquid.
[0038] In one embodiment, the carbonization temperature is 800° C. to 900° C., and the carbonization time is 2 to 3 hours.
[0039] In one embodiment, the carbonization temperature is 850° C. and the carbonization time is 2.5 h.
[0040] In one embodiment, the treatment solution includes 300-500 mg·L -1 of ferric chloride and 350-600 mg·L -1 of sodium chloride.
[0041] In one embodiment, the treatment solution includes 350 mg·L -1 of ferric chloride and 450mg·L -1 of sodium chloride.
[0042] The treatment liquid can introduce functional groups such as hydroxyl and carboxyl groups on the surface of biochar, which help to improve the adsorption capacity of biochar for organic pollutants. Sodium chloride in the treatment liquid can adjust the ionic strength of the treatment liquid, thereby affecting the interaction between the treatment liquid and biochar. Secondly, sodium chloride can help form more mesoporous structures during the heat treatment process, and these mesopores are conducive to the adsorption of organic pollutants. In addition, sodium chloride promotes the precipitation of organic pollutants through salting out, thereby improving the adsorption efficiency of the material. Finally, the presence of sodium chloride can help the adsorbent material to desorb the adsorbate more easily during the regeneration process, thereby improving the regeneration efficiency, and extending the service life of the adsorbent material, reducing the replacement frequency and cost, making its application in organic wastewater treatment more efficient and economical.
[0043] In one embodiment, the solid-liquid ratio of the biochar to the treatment liquid is 5 to 15 g / mL.
[0044] In one embodiment, the solid-liquid ratio of the biochar to the treatment liquid is 10 g / mL.
[0045] The present invention controls the content of iron oxides in the material by limiting the material-to-liquid ratio of biochar and treatment liquid. The research of the present invention shows that the presence of iron oxides helps to improve the adsorption performance and regeneration performance of the material, but too high an iron oxide content not only fails to further improve the material performance, but also leads to a significant decrease in the specific surface area, thereby causing damage to the performance of the adsorption material. Therefore, the present invention strictly limits the material-to-liquid ratio of biochar and treatment liquid to maximize the specific surface area of the adsorption material and improve the adsorption performance. In addition, an appropriate material-to-liquid ratio can ensure that the biochar is in full contact with the treatment liquid, thereby improving the production efficiency of the adsorption material.
[0046] In one embodiment, the heat treatment is carried out in two steps. The first step is low-temperature pre-burning, the low-temperature pre-burning temperature is 80-120°C, the insulation time is 30-60min, and the heating rate is 5°C / min-10°C / min. The second step is high-temperature calcination, the high-temperature calcination temperature is 250°C-350°C, the insulation time is 60-90min, and the heating rate is 2°C / min-5°C / min.
[0047] In one embodiment, the low-temperature pre-sintering temperature is 100°C, the holding time is 45 minutes, and the heating rate is 8°C / min; the high-temperature calcining temperature is 320°C, the holding time is 60 minutes, and the heating rate is 3°C / min.
[0048] The present invention improves the regeneration performance of the adsorbent material by low-temperature pre-burning, high-temperature calcination, and strictly controlling the heating rate of the step-by-step heat treatment. A faster heating rate is usually used in the low-temperature pre-burning stage. This is because at low temperatures, the volatile substances and moisture in the biochar need to be quickly discharged to avoid excessive gas generation during the subsequent high-temperature calcination process, which causes the sample to expand or rupture. Rapid heating also helps to remove organic impurities and residues in the biochar and reduce interference with subsequent high-temperature treatment. A slower heating rate is used in the high-temperature calcination stage, mainly to control the structure and pore formation of the biochar. Slow heating can ensure that the biochar gradually forms a stable structure at high temperature, avoiding structural damage caused by too rapid temperature changes. Slow heating also helps to uniformly calcine, making the physical and chemical properties of the biochar more uniform, and improving its adsorption performance and stability.
[0049] Finally, the treatment solution is used first and then the heat treatment is performed. The order of the two steps cannot be interchanged. The ferric chloride and sodium chloride in the treatment solution can introduce functional functional groups on the surface of biochar, while promoting the formation and development of pores on the surface and inside of biochar, increasing the specific surface area and porosity. If high-temperature heat treatment is performed first, it will make it difficult for the chemicals in the treatment solution to effectively penetrate and react, reducing the introduction of functional functional groups. In addition, after high-temperature heat treatment, the change in the pore structure of biochar will reduce the diffusion efficiency of the treatment solution in the biochar and affect the adsorption performance. Therefore, using the treatment solution for treatment first and then performing step-by-step heat treatment can ensure the optimization of the surface and internal structure of biochar and maximize its adsorption performance and stability.
[0050] The present invention also provides an adsorption material for treating organic wastewater prepared according to the method.
[0051] The technical solution provided by the present invention is further described below in conjunction with embodiments.
[0052] Example 1 A method for preparing an adsorbent material for treating organic wastewater, the steps are as follows:
[0053] S1, drying the straw at 100°C for 8 hours, crushing it, and passing it through an 80-mesh sieve to obtain straw powder; drying the cyanobacteria at 120°C for 12 hours, crushing it, and passing it through a 100-mesh sieve to obtain cyanobacteria powder;
[0054] S2, the straw powder and the blue algae powder are mixed in a mass ratio of 4:1 to obtain a mixed powder, and the sodium hydroxide is mixed with the mixed powder in a mass ratio of 1.5:1, and carbonized at 850°C for 2.5h under argon to obtain biochar;
[0055] S3, the biochar and the treatment liquid are mixed evenly at a material-liquid ratio of 10 g / mL, the temperature is raised to 100°C at a heating rate of 8°C / min, and the temperature is kept for 45 min, then the temperature is raised to 320°C at a heating rate of 3°C / min, and the temperature is kept for 60 min, and the temperature is cooled to obtain an adsorption material for organic wastewater treatment;
[0056] The treatment solution is a mixture of an aqueous solution of ferric chloride and an aqueous solution of sodium chloride, wherein the concentration of ferric chloride is 350 mg·L -1 , the concentration of sodium chloride is 450 mg·L -1 .
[0057] Example 2 A method for preparing an adsorbent material for treating organic wastewater, the steps are as follows:
[0058] S1, drying the straw at 100°C for 8 hours, crushing it, and passing it through an 80-mesh sieve to obtain straw powder; drying the cyanobacteria at 120°C for 12 hours, crushing it, and passing it through a 100-mesh sieve to obtain cyanobacteria powder;
[0059] S2, the straw powder and the blue algae powder are mixed in a mass ratio of 3:1 to obtain a mixed powder, and the sodium hydroxide is mixed with the mixed powder in a mass ratio of 2:1, and carbonized at 900° C. for 2 h under argon to obtain biochar;
[0060] S3. Evenly mix the biochar and the treatment liquid at a solid-liquid ratio of 15 g / mL, heat the temperature to 120°C at a heating rate of 5°C / min, keep the temperature for 60 min, then heat the temperature to 350°C at a heating rate of 2°C / min, keep the temperature for 90 min, and cool to obtain an adsorption material for organic wastewater treatment.
[0061] The treatment solution is a mixture of an aqueous solution of ferric chloride and an aqueous solution of sodium chloride, wherein the concentration of ferric chloride is 350 mg·L -1 , the concentration of sodium chloride is 450 mg·L -1 .
[0062] Example 3 A method for preparing an adsorbent material for treating organic wastewater, the steps are as follows:
[0063] S1, drying the straw at 100°C for 8 hours, crushing it, and passing it through an 80-mesh sieve to obtain straw powder; drying the cyanobacteria at 120°C for 12 hours, crushing it, and passing it through a 100-mesh sieve to obtain cyanobacteria powder;
[0064] S2, the straw powder and the blue algae powder are mixed in a mass ratio of 5:1 to obtain a mixed powder, and the sodium hydroxide is mixed with the mixed powder in a mass ratio of 1:1, and carbonized at 800° C. for 3 h under argon to obtain biochar;
[0065] S3. Evenly mix the biochar and the treatment liquid at a material-liquid ratio of 5 g / mL, increase the temperature to 80°C at a heating rate of 10°C / min, keep warm for 30 minutes, then increase the temperature to 250°C at a heating rate of 5°C / min, keep warm for 60 minutes, and cool to obtain an adsorption material for organic wastewater treatment.
[0066] The treatment solution is a mixture of an aqueous solution of ferric chloride and an aqueous solution of sodium chloride, wherein the concentration of ferric chloride is 350 mg·L -1 , the concentration of sodium chloride is 450 mg·L -1 .
[0067] Comparative Example 1
[0068] Same as Example 1, except that the straw powder is sieved through a 20-mesh sieve and the blue algae powder is sieved through a 40-mesh sieve.
[0069] Comparative Example 2
[0070] Same as Example 1, except that no blue algae powder was used.
[0071] Comparative Example 3
[0072] Same as Example 1, except that the mass ratio of the straw powder to the blue algae powder is 1:1.
[0073] Comparative Example 4
[0074] Same as Example 1, except that sodium hydroxide is replaced by an equal amount of potassium hydroxide.
[0075] Comparative Example 5
[0076] The same as Example 1, except that: the heat treatment method is: heating to 320° C. at a heating rate of 3° C. / min, keeping the temperature for 60 min, cooling, and obtaining an adsorption material for organic wastewater treatment.
[0077] Comparative Example 6
[0078] The same as Example 1, except that the temperature is raised to 100°C at a heating rate of 3°C / min, kept warm for 45 minutes, then raised to 320°C at a heating rate of 8°C / min, kept warm for 60 minutes, and cooled to obtain an adsorption material for organic wastewater treatment.
[0079] Comparative Example 7
[0080] A method for preparing an adsorbent material for treating organic wastewater, comprising the following steps:
[0081] S1, drying the straw at 100°C for 8 hours, crushing it, and passing it through an 80-mesh sieve to obtain straw powder; drying the cyanobacteria at 120°C for 12 hours, crushing it, and passing it through a 100-mesh sieve to obtain cyanobacteria powder;
[0082] S2, the straw powder and the blue algae powder are mixed in a mass ratio of 4:1 to obtain a mixed powder, and the sodium hydroxide is mixed with the mixed powder in a mass ratio of 1.5:1, and carbonized at 850°C for 2.5h under argon to obtain biochar;
[0083] S3, heating the biochar to 100°C at a heating rate of 8°C / min, keeping the temperature for 45min, then heating the biochar to 320°C at a heating rate of 3°C / min, keeping the temperature for 60min, cooling, mixing the biochar with the treatment liquid at a material-liquid ratio of 10g / mL, stirring for 60min, and drying to obtain an adsorption material for organic wastewater treatment;
[0084] The treatment solution is a mixture of an aqueous solution of ferric chloride and an aqueous solution of sodium chloride, wherein the concentration of ferric chloride is 350 mg·L -1 , the concentration of sodium chloride is 450 mg·L -1 .
[0085] Test Example 1
[0086] The performance of the adsorbent material for organic wastewater treatment obtained in the examples and comparative examples was tested. Unless otherwise specified, all tests were repeated 3 times. SPSS 21.0 was used for variance analysis (ANOVA) and Duncan multiple comparison analysis, and the results were expressed as mean ± standard deviation. The test method is as follows:
[0087] Weigh 0.2 g of adsorption material for organic wastewater treatment and add it to 100 mL of methylene blue solution with a concentration of 100 mg / L. The reaction is carried out in a 250 mL conical flask. The sample is placed on a magnetic stirrer and stirred at an appropriate rate. After the reaction reaches the equilibrium time, centrifuge it. The supernatant is filtered with a 0.22 μm filter head and the absorbance is measured. The concentration of methylene blue after adsorption is converted using a standard curve to calculate the adsorption rate.
[0088] The adsorbent material for organic wastewater treatment adsorbed with methylene blue was regenerated with 3% H2O2, the regeneration temperature was 30°C, and the regeneration time was 4h. After regeneration, the adsorbent material was separated and washed with distilled water for 3 times and then dried for the second adsorption experiment, which was repeated 5 times to calculate the regeneration rate.
[0089] The test results are as follows:
[0090] Adsorption rate, % Equilibration time, min Regeneration rate, % Example 1 97.38±2.0ab 54.42±1.73g 74.55±1.59a Example 2 96.95±1.6b 52.73±1.82g 74.18±1.23a Example 3 97.87±1.3ab 52.11±2.18g 74.90±1.72a Comparative Example 1 70.11±2.1g 73.47±1.46a 61.99±2.31e Comparative Example 2 77.90±1.4f 68.03±1.01b 63.17±1.66d Comparative Example 3 80.83±1.9e 63.67±1.25d 62.91±2.28d Comparative Example 4 98.55±2.0a 65.30±2.04c 64.43±2.05c Comparative Example 5 89.59±1.7d 58.77±1.50e 65.70±1.54b Comparative Example 6 92.51±1.4c 57.14±1.67f 65.06±1.87bc Comparative Example 7 96.93±1.37b 63.21±1.06d 61.25±1.15e
[0091] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing an adsorbent material for treating organic wastewater, characterized in that: The following steps are involved: S1, drying and crushing the straw and blue algae respectively, and passing through a 80-100 mesh sieve to obtain straw powder and blue algae powder; S2, mixing straw powder and cyanobacteria powder to obtain a mixed powder, adding sodium hydroxide and carbonizing at high temperature under argon gas to obtain biochar; S3, mixing the biochar with the treatment liquid, heat treating, and cooling to obtain an adsorption material for organic wastewater treatment; The treatment solution includes 300-500 mg·L -1 of ferric chloride and 350-600 mg·L -1 of sodium chloride; The heat treatment is carried out in two steps. The first step is low-temperature pre-firing, the low-temperature pre-firing temperature is 80-120°C, the insulation time is 30-60min, and the heating rate is 5°C / min-10°C / min. The second step is high-temperature calcination, the high-temperature calcination temperature is 250°C-350°C, the insulation time is 60-90min, and the heating rate is 2°C / min-5°C / min.
2. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that The drying temperature is 100° C. to 120° C., and the drying time is 8 to 12 hours.
3. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The mass ratio of the straw powder to the blue algae powder is (3-5):
1.
4. The method for preparing an adsorbent material for treating organic wastewater according to claim 3, characterized in that: The mass ratio of the straw powder to the blue algae powder is 4:
1.
5. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The mass ratio of the sodium hydroxide to the mixed powder is (1-2):
1.
6. The method for preparing an adsorbent material for treating organic wastewater according to claim 5, characterized in that: The mass ratio of the sodium hydroxide to the mixed powder is 1.5:
1.
7. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The carbonization temperature is 800° C. to 900° C., and the carbonization time is 2 to 3 hours.
8. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The treatment solution includes 350 mg·L -1 of ferric chloride and 450mg·L -1 of sodium chloride.
9. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The solid-liquid ratio of the biochar to the treatment liquid is 5 to 15 g / mL.
10. The method for preparing an adsorbent material for treating organic wastewater according to claim 1, characterized in that: The low-temperature pre-sintering temperature is 100°C, the holding time is 45 minutes, and the heating rate is 8°C / min. The high-temperature calcining temperature is 320°C, the holding time is 60 minutes, and the heating rate is 3°C / min.
Citation Information
Patent Citations
Oily sludge-based biochar as well as preparation method and application thereof
CN114517104A
Molecular sieve-like biochar adsorbent and preparation method thereof
CN116459796A
Modified charcoal-based CO2 efficient selective adsorption material and preparation method thereof
CN116532083A
Method for preparing charcoal metal adsorbent based on zizania aquatica straw and blue-green algae
CN117960124A