Defective iron-based perovskite / nano TiO2 sphere catalyst as well as preparation method and application thereof
By adding urea to the iron-based perovskite catalyst and forming a Fe-O-Ti structure with nanoTiO2 spheres, the problem of coordinated removal of NOx and VOCs at low temperatures is solved, and efficient removal of NO and toluene is achieved, providing new gaseous pollutant removal technology.
Patent Information
- Application Number
- CN202411199571.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to synergistically and efficiently remove NOx and VOCs in industrial flue gas under low temperature conditions. The traditional SCR catalyst activity is insufficient and the temperature removal windows of NOx and VOCs do not match, making it difficult to achieve coordinated control.
The activity of iron-based perovskite catalyst is enhanced by adding urea and formed a rich Fe-O-Ti structure with nanoTiO2 spheres to promote electron transfer, and a defective iron-based perovskite/nanoTiO2 sphere catalyst is prepared to achieve NO and toluene synergistic and efficient removal.
The oxidation performance of the catalyst is significantly improved under low temperature conditions, and the coordinated and efficient removal of NO and toluene is achieved, providing a new research idea for synergistic removal of gaseous pollutants.
Smart Images

Figure CN119076000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gaseous pollutant control, and in particular relates to a defective iron-based perovskite / nano-TiO2 ball catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO x ) and volatile organic compounds (VOCs) are the main pollutants in industrial exhaust gases. 2.5 Therefore, the development of an efficient catalyst and removal technology for the synergistic and efficient denitrification and removal of VOCs from flue gas has become the focus of research.
[0003] Currently, NO x The commonly used control technologies for NO and VOCs are selective catalytic reduction technology (SCR) and catalytic oxidation technology. x and VOCs can be effectively controlled under existing technologies; however, in actual working conditions, especially in non-electric industries, NO x The emission environment temperature of pollutants such as NO and VOCs is relatively low (<300°C), and the activity of traditional SCR catalysts under this temperature condition is not enough to achieve the purpose of removing pollutants. x It does not match the removal temperature window of VOCs, making it difficult to achieve coordinated control.
[0004] Therefore, developing a new technology for synergistic denitrification and VOCs removal with high-performance catalysts at low temperatures is particularly important for controlling multi-pollutant emissions in non-power industries.
[0005] In recent years, advanced oxidation processes (AOPs) have been used to generate reactive oxygen species to catalyze the removal of NO. x The technology of removing VOCs has attracted wide attention from researchers due to its advantages such as low reaction temperature, high removal efficiency and less secondary pollution. Among them, hydrogen peroxide (H2O2) has the advantages of low cost and environmental friendliness, and is often used as a precursor of reactive oxygen species; and iron-based perovskite catalysts have been widely studied in Fenton-like systems because they can improve the utilization rate of H2O2 and the yield of reactive oxygen species. However, conventional iron-based perovskite catalysts have limited activity and it is difficult to achieve NO x The present invention discloses a defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst, which can achieve the synergistic and efficient removal of NO and toluene under low-concentration H2O2 and low-temperature conditions. Summary of the invention
[0006] In view of the above technical problems, the present invention provides a defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst and its preparation method and application. First, the activity of the iron-based perovskite catalyst is enhanced by adding urea, and then a rich Fe-O-Ti structure is formed through the interaction between the metal (U-LFO) and the carrier (nano-TiO2 ball), which promotes the electron transfer between each other, further improves the oxidation performance of the catalyst, and realizes the synergistic and efficient removal of NO and toluene. That is, the prepared U-LFO / TiO2 catalyst can not only achieve low-temperature denitration, but also achieve efficient synergistic conversion of toluene.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] One of the technical solutions of the present invention:
[0009] A method for preparing a defective iron-based perovskite / nano-TiO2 ball catalyst comprises the following steps:
[0010] Dissolving lanthanum nitrate hexahydrate, ferric nitrate nonahydrate, citric acid and urea in water at a molar ratio of La:Fe:citric acid:urea of 1:1:2.2-3:4-6 to obtain a mixed solution;
[0011] The nano-TiO2 balls are added into the mixed solution, and ultrasonic, heating and stirring, drying and calcining are performed in sequence to obtain the defective iron-based perovskite / nano-TiO2 ball catalyst.
[0012] Preferably, the preparation process of the nano TiO2 spheres is:
[0013] The mixed solution containing tetrabutyl titanate and the glucose solution are placed in a hydrothermal synthesis reactor, and then dried, filtered, vacuum dried and calcined to obtain nano-TiO2 balls.
[0014] Furthermore, the mixed solution containing tetrabutyl titanate is prepared by sequentially adding tetrabutyl titanate and water into anhydrous ethanol and stirring the mixture uniformly;
[0015] wherein, after adding the tetrabutyl titanate, stirring was performed at a speed of 300 r / min for 1 h at room temperature;
[0016] After adding the water (preferably deionized water), stirring was carried out at 60° C. and a speed of 700 r / min for 3 h.
[0017] Furthermore, the volume ratio of tetrabutyl titanate, anhydrous ethanol and water is: 0.4-0.5:5:1;
[0018] Preferably, the conditions in the drying process are: drying at 180° C. for 12 h;
[0019] The conditions in the vacuum drying process are: drying in a vacuum drying oven at 80°C for 12h;
[0020] The conditions during the calcination process are: calcination at 500-600° C. for 3-5 hours.
[0021] Preferably, the mass ratio of defective iron-based perovskite to nano-TiO2 balls in the defective iron-based perovskite / nano-TiO2 ball catalyst is 2.43: 1. The mass ratio is calculated as follows: as in Example 1, 0.006 mol of lanthanum nitrate hexahydrate and ferric nitrate nonahydrate are added, and theoretically 0.006 mol of LaFeO3 can be obtained. Then, by calculation, the mass of 0.006 mol of LaFeO3 can be compared with the amount of TiO2 added.
[0022] Preferably, the conditions of the heating and stirring process are: heating and stirring at 80°C and 600 r / min until the solution forms a gel;
[0023] The conditions of the drying process are: drying at 90-110°C overnight;
[0024] The conditions of the calcination process are: calcination at 600-700° C. for 5-7 hours.
[0025] The second technical solution of the present invention:
[0026] A defective iron-based perovskite / nano-TiO2 ball catalyst is prepared by the above preparation method.
[0027] The third technical solution of the present invention:
[0028] The above-mentioned defective iron-based perovskite / nano-TiO2 ball catalyst is used in the synergistic oxidation of NO and toluene in flue gas.
[0029] Preferably, the process of synergistically oxidizing NO and toluene in flue gas is: passing flue gas into a reaction device containing the defective iron-based perovskite / nano-TiO2 ball catalyst to carry out synergistic NO removal and toluene removal reactions at a temperature of 90-210°C; preferably 180°C;
[0030] The oxygen content in the flue gas is 10%, and the hydrogen peroxide concentration is 3%.
[0031] Compared with the prior art, the present invention has the following advantages and technical effects:
[0032] 1. The present invention prepares the nano-TiO2 carrier by a simple one-pot hydrothermal synthesis method, which not only ensures that the TiO2 carrier can form a regular spherical structure, but also avoids a complicated preparation process.
[0033] 2. The present invention uniformly loads defective iron-based perovskite onto nano-TiO2 balls in situ to synthesize a composite oxide catalyst, which forms a rich Fe-O-Ti structure through the interaction between metal oxides, promotes electron transfer between each other, and thus significantly improves the catalytic oxidation performance of defective iron-based perovskite / nano-TiO2 balls.
[0034] 3. The composite oxide U-LFO / TiO2 prepared by the present invention not only presents a regular spherical structure, but also maintains the stability of the perovskite oxide structure; at the same time, it can also achieve synergistic and efficient oxidation removal of NO and toluene in the low temperature zone, providing a new research idea for the synergistic removal of gaseous pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0036] Figure 1 This is a schematic diagram of the preparation process of the U-LFO / TiO2 catalyst of Example 1 of the present invention;
[0037] Figure 2 The X-ray diffraction (XRD) characterization results of the iron-based perovskite (LFO) prepared in Comparative Example 1, the urea-regulated iron-based perovskite (U-LFO) prepared in Comparative Example 2, and the U-LFO / TiO2 catalyst and carrier (nano-TiO2 spheres) prepared in Example 1 of the present invention;
[0038] Figure 3 The scanning electron microscope (SEM) characterization result diagram of the carrier (nano-TiO2 spheres) and U-LFO / TiO2 catalyst prepared in Example 1 of the present invention;
[0039] Among them, the left picture shows nano-TiO2 balls; the right picture shows U-LFO / TiO2 catalyst. DETAILED DESCRIPTION
[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0041] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0045] The present invention provides a novel method for preparing a defective iron-based perovskite / nano-TiO2 spherical catalyst for synergistic removal of NO and toluene from flue gas, which specifically comprises:
[0046] In the first step, a proper amount of tetrabutyl titanate is added dropwise to a certain amount of anhydrous ethanol, and after being stirred evenly, a certain amount of deionized water is added dropwise, and then stirred at a set temperature and time to form a solution A;
[0047] In the second step, solution A and glucose solution are mixed and placed in a hydrothermal reactor, and reacted in a forced air drying oven for a period of time to obtain product B;
[0048] The third step is to filter, wash and dry the product B, and then calcine it in a muffle furnace to obtain nano-TiO2 balls;
[0049] Step 4, weigh a certain amount of lanthanum nitrate hexahydrate, ferric nitrate nonahydrate, citric acid and urea, dissolve them in an appropriate amount of deionized water, and stir them evenly to form a solution C;
[0050] Step 5: Add a certain amount of nano-TiO2 balls into solution C, heat and stir after ultrasonic treatment until the solution forms a gel;
[0051] Step 6, drying the gel product overnight and grinding it to obtain a powder sample;
[0052] In the seventh step, the powdered sample is placed in a muffle furnace and calcined to obtain the final product, a defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst.
[0053] In some preferred embodiments, the first step is to dropwise add a certain amount of tetrabutyl titanate into an appropriate amount of anhydrous ethanol, stir at 300 r / min for 1 hour at room temperature, and then dropwise add a certain amount of deionized water (the volume ratio of deionized water to anhydrous ethanol is 1:5); then stir at 700 r / min for 3 hours at 60°C to form solution A.
[0054] In some preferred embodiments, the second step is to mix solution A and 0.4 mol / L glucose solution and place the mixture in a hydrothermal reactor, and then react in a forced air drying oven at 180° C. for 12 hours to obtain product B.
[0055] In some preferred embodiments, the third step is to filter and wash the product B, place it in a vacuum drying oven at 80°C for 12 hours, and then calcine it in a muffle furnace at 500-600°C for 3-5 hours to obtain nano-TiO2 balls.
[0056] In some preferred embodiments, the fourth step specifically comprises weighing lanthanum nitrate hexahydrate, ferric nitrate nonahydrate, citric acid and urea in an amount satisfying a molar ratio of lanthanum nitrate hexahydrate: ferric nitrate nonahydrate: citric acid: urea of 1:1:2.2-3:4-6, and stirring the mixture in 40 mL of deionized water at a speed of 300 r / min at room temperature for 1 h.
[0057] In some preferred embodiments, the fifth step is specifically to add a certain amount of nano-TiO2 balls into solution B, ultrasonically treat for 30 minutes, and then heat and stir at 80°C and 600r / min until the solution forms a gel.
[0058] In some preferred embodiments, the sixth step is to place the gel in a forced air drying oven immediately after it is formed, dry it at 90-110° C. overnight, and grind the dried product to obtain a brown-yellow powder sample.
[0059] In some preferred embodiments, the seventh step is specifically to place the brown-yellow powder sample obtained in the seventh step in a muffle furnace at 600-700°C for calcining for 5-7h to obtain the final product defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst.
[0060] The defective iron-based perovskite / nano-TiO2 sphere catalyst prepared by the above method is applied to the synergistic oxidation of NO and toluene in flue gas.
[0061] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.
[0062] The raw materials used in the present invention are all purchased from the market.
[0063] The technical solution of the present invention is further illustrated by the following embodiments.
[0064] Example 1
[0065] like Figure 1 As shown, a method for preparing a defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst comprises the following steps:
[0066] A solution A was formed by adding a certain amount of tetrabutyl titanate (9 mL) dropwise into 100 mL of anhydrous ethanol, stirring at 300 r / min for 1 h at room temperature, then adding a certain amount of deionized water (the volume ratio of water to anhydrous ethanol was 1:5), stirring at 700 r / min for 3 h at 60°C, and then forming a solution A.
[0067] 129 mL of solution A and 35 mL of 0.4 mol / L glucose solution were mixed and placed in a hydrothermal synthesis reactor, and then dried in a 180°C forced air drying oven for 12 hours to obtain product B; product B was filtered and washed, and then placed in a vacuum drying oven at 80°C for 12 hours, and after drying, placed in a muffle furnace and calcined at 600°C for 3 hours to obtain nano-TiO2 balls;
[0068] Lanthanum nitrate hexahydrate, ferric nitrate nonahydrate, citric acid and urea were weighed according to the following molar amounts, wherein lanthanum nitrate hexahydrate was 0.006 mol, ferric nitrate nonahydrate was 0.006 mol, citric acid was 0.0132 mol, and urea was 0.03 mol, and placed in 40 mL of deionized water, and stirred at a speed of 300 r / min for 1 h at room temperature to obtain a solution C;
[0069] 0.6 g of nano-TiO2 balls were added into 40 mL of solution C, and after ultrasonic treatment for 30 min, the solution was heated and stirred at 90°C and 700 r / min until the solution formed a gel state; after the gel state was formed, the solution was immediately placed in a forced air drying oven and dried at 110°C overnight, and the dried product was ground to obtain a brown-yellow powder;
[0070] The obtained brown-yellow powder was placed in a muffle furnace and calcined at 700° C. for 5 h to obtain the final product, a defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst.
[0071] Next, the present invention further prepared an iron-based perovskite catalyst (LFO) and a urea-regulated iron-based perovskite catalyst (U-LFO) by changing whether urea and carrier nano-TiO2 balls were added.
[0072] Comparative Example 1 (Catalyst LFO)
[0073] The same preparation method as in Example 1 was adopted, except that urea and carrier nano-TiO2 balls were not added, and the prepared catalyst was LFO.
[0074] Comparative Example 2 (Catalyst U-LFO)
[0075] The same preparation method as in Example 1 was adopted, except that no carrier nano-TiO2 balls were added, and the prepared catalyst was U-LFO.
[0076] The products obtained in Example 1 and Comparative Examples 1-2 were analyzed by X-ray diffraction (XRD) characterization. Figure 2 ;from Figure 2 It can be seen that the modification methods such as urea regulation and carrier nano-TiO2 addition did not change the catalyst crystal shape, and U-LFO / TiO2 still maintained the stable configuration of perovskite-type oxide. The nano-TiO2 balls prepared in Example 1 were analyzed by scanning electron microscopy (SEM). Figure 3 (Left picture); It can be seen from the picture that the synthesized TiO2 presents a spherical structure, indicating that the nano-TiO2 spheres were successfully synthesized; and after the defective iron-based perovskite is loaded onto the nano-TiO2, U-LFO / TiO2 can still maintain a spherical structure, the results are shown in Figure 3 (Right picture).
[0077] Effect verification
[0078] Effect Example 1 Performance test of different types of catalysts for oxidation of NO and toluene
[0079] Weigh 0.2 g of the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2, respectively, and load them into a quartz reaction tube (inner diameter 10 mm), then introduce 200 mL / min of a reaction mixture (comprising N2 carrier gas, 10% O2, 200 ppm NO and 100 ppm toluene), set the reaction temperature to 120°C, add 3% H2O2 during the experiment, record the changes in NO and toluene concentrations before and after the reaction, and calculate the NO removal and toluene removal efficiencies of the LFO, U-LFO and U-LFO / TiO2 catalysts.
[0080] The conversion rate of NO and toluene is calculated as follows:
[0081] Conversion rate (%) = ([C]0-[C] t ) / [C]0*100%
[0082] Among them, [C]0 and [C] t are the concentrations of NO or toluene before and after the reaction, respectively.
[0083] The results of relevant NO removal and toluene removal efficiency are shown in Table 1:
[0084] Table 1
[0085]
[0086] As can be seen from Table 1, under the conditions of 120°C, 10% O2 and 3% H2O2, the U-LFO / TiO2 catalyst can achieve a NO removal efficiency of 99.19% and a toluene removal efficiency of 90.37%, which are much higher than those of LFO and U-LFO. This result shows that the modification method of urea regulation and carrier nano-TiO2 ball addition can significantly improve the NO and toluene oxidation performance of defective iron-based perovskite catalysts, and can achieve the synergistic and efficient removal of NO and toluene in the low temperature zone.
[0087] Effect Example 2 Effect of temperature on the removal of NO and toluene
[0088] The effect of different temperatures on the removal of NO and toluene by this U-LFO / TiO2 catalyst is now investigated. The reaction temperature is controlled at 90°C, 120°C, 150°C, 180°C and 210°C, the reaction conditions are 10% O2 and 3% H2O2, and the defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst is used to oxidize NO and toluene. The relevant results are shown in Table 2.
[0089] Table 2
[0090] Reaction temperature (℃) NO conversion efficiency (%) Toluene conversion efficiency (%) 90 85.78 82.33 120 99.19 90.37 150 99.90 91.76 180 99.95 94.88 210 97.19 91.10
[0091] It can be seen from Table 2 that when the reaction temperature increases from 90°C to 180°C, the NO conversion efficiency increases from 85.78% to 99.95%, and the toluene conversion efficiency increases from 82.33% to 94.88%; when the reaction temperature continues to increase to 210°C, the conversion efficiencies of NO and toluene show a slight downward trend, but both can maintain a conversion efficiency of more than 90%.
[0092] From the results of the above specific embodiments, it can be seen that the defective iron-based perovskite / nano-TiO2 ball (U-LFO / TiO2) catalyst provided by the present invention can achieve synergistic and efficient removal of NO and toluene in the low temperature zone, providing a feasible solution to solve the problem of multiple pollutants in flue gas.
[0093] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a defective iron-based perovskite / nano-TiO2 sphere catalyst, characterized in that: The following steps are involved: Dissolve lanthanum nitrate hexahydrate, ferric nitrate nonahydrate, citric acid and urea in water at a molar ratio of La:Fe:citric acid:urea=1:1:(2.2-3):(4-6) to obtain a mixed solution; The nano-TiO2 balls are added into the mixed solution, and ultrasonic, heating and stirring, drying and calcining are performed in sequence to obtain the defective iron-based perovskite / nano-TiO2 ball catalyst.
2. The method for preparing a defective iron-based perovskite / nano-TiO2 spherical catalyst according to claim 1, characterized in that: The preparation process of the nano TiO2 ball is: The mixed solution containing tetrabutyl titanate and the glucose solution are placed in a hydrothermal synthesis reactor, and then dried, filtered, dried and calcined to obtain nano-TiO2 balls.
3. The method for preparing a defective iron-based perovskite / nano-TiO2 spherical catalyst according to claim 2, characterized in that: The mixed solution containing tetrabutyl titanate is prepared by sequentially adding tetrabutyl titanate and water into anhydrous ethanol and stirring the mixture evenly.
4. The method for preparing a defective iron-based perovskite / nano-TiO2 sphere catalyst according to claim 3, characterized in that: The volume ratio of tetrabutyl titanate, anhydrous ethanol and water is 0.4-0.5:5:
1.
5. The method for preparing a defective iron-based perovskite / nano-TiO2 spherical catalyst according to claim 2, characterized in that: The conditions in the drying process are: drying at 180°C for 12h; The conditions during the calcination process are: calcination at 500-600° C. for 3-5 hours.
6. The method for preparing a defective iron-based perovskite / nano-TiO2 sphere catalyst according to claim 1, characterized in that: The mass ratio of the defective iron-based perovskite to the nano-TiO2 sphere in the defective iron-based perovskite / nano-TiO2 sphere catalyst is 2.43:
1.
7. The method for preparing a defective iron-based perovskite / nano-TiO2 sphere catalyst according to claim 1, characterized in that: The conditions of the heating and stirring process are: heating and stirring at 70-90° C. and 600-800 r / min until the solution forms a gel; The conditions of the drying process are: drying at 90-110°C overnight; The conditions of the calcination process are: calcination at 600-700° C. for 5-7 hours.
8. A defective iron-based perovskite / nano-TiO2 ball catalyst, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of a defective iron-based perovskite / nano-TiO2 ball catalyst as claimed in claim 8 in the synergistic oxidation of NO and toluene in flue gas.
10. The use of a defective iron-based perovskite / nano-TiO2 ball catalyst in the synergistic oxidation of NO and toluene in flue gas according to claim 9, characterized in that: The temperature during the synergistic oxidation of NO and toluene in the flue gas is 90-210°C.
Citation Information
Cited By
Far-infrared functional photobiotin composite material, acupoint patch prepared from same and application of acupoint patch
CN120037377A
A far-infrared functional bioluminescent composite material and acupuncture patch prepared therefrom and its application
CN120037377B