Ultra-light metal honeycomb monolithic catalyst as well as preparation method and application thereof
By preparing high-active catalysts and catalytic slurries on ultra-thin metal foils, an ultra-light metal honeycomb integral catalyst is solved, and the existing catalyst preparation process is complex and poor activity is achieved, efficient CO removal and hydrogen purification are achieved. At low temperature operation, the system complexity is reduced.
Patent Information
- Application Number
- CN202411192744.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing metal integral catalyst preparation process is complex, the catalyst is easy to crush, the coating is uneven, the activity is poor, and it is difficult to be suitable for high-flow hydrogen purification, especially when it is easily damaged under high temperature shock, and needs to be replaced frequently.
Using ultra-thin metal foil as the matrix, high-active catalyst raw powder and high-active catalytic slurry are prepared by impregnation method to ensure the firm combination of the coating and the metal matrix, and to form ultra-light metal honeycombs with small mass, high porosity and good activity. Integral catalyst, suitable for low temperature CO removal.
The catalyst is high activity and mechanical strength, suitable for high flow hydrogen purification, CO is basically completely removed at 80°C, and is filled in a methanol reformer to supply hydrogen, reducing system complexity.
Smart Images

Figure CN119076013A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic material preparation, and in particular to an ultra-light metal honeycomb monolithic catalyst and a preparation method and application thereof. Background Art
[0002] Methanol fuel cell technology is a technology that combines methanol reforming to produce hydrogen and hydrogen fuel cells as automobile generators. This technology can achieve instant on-board hydrogen production and power generation. Electric vehicles powered by methanol fuel cells have the same convenience as gasoline internal combustion engine vehicles. Methanol can be made from renewable resources and meets carbon neutrality requirements. The development of methanol reforming hydrogen production technology in the transportation field will make a huge contribution to global carbon dioxide emission reduction and air pollution control.
[0003] The product of hydrogen production from methanol reforming generally contains about 1% CO. CO is strongly adsorbed on the surface of the Pt electrode of the fuel cell, which will cause a sharp decline in the performance of the battery. Only by reducing the CO content in the system to below 10ppm can the poisoning problem of the Pt electrode of the fuel cell be solved. Currently, the only catalyst available on the market for CO removal in a hydrogen-rich atmosphere is the TSSA-5 spherical catalyst from Tanaka, Japan. Although the spherical catalyst has good activity, the pressure drop of the catalytic bed after filling is large, which is not suitable for large-flow hydrogen purification. In addition, the spherical catalyst is easy to crush under high-intensity vibration and needs to be replaced frequently.
[0004] Therefore, the prior art proposes a metal-based monolithic catalyst to avoid the technical problems of easy crushing and frequent replacement. However, the metal monolithic catalyst in the prior art is to coat the catalyst particles on a porous metal carrier by multiple coating, drying and calcination. The process is complicated and time-consuming, which not only increases the mass of the monolithic catalyst, but also easily leads to problems such as uneven coating, easy cracking of the coating, low surface area and poor activity in the prepared monolithic catalyst. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides an ultra-light metal honeycomb monolithic catalyst and its preparation method and application. The present invention selects ultra-thin metal foil as the substrate, and prepares high-activity catalyst raw powder and high-activity catalytic slurry with good coating properties to ensure the firm bonding between the coating and the metal substrate, and prepares a metal honeycomb monolithic catalyst with small mass, high porosity, good activity and high mechanical strength. When the catalyst is applied to the removal of CO in a hydrogen-rich atmosphere containing a small amount of CO and a large amount of H2O and CO2, CO can be basically completely removed at a low temperature of 80°C, and can be filled in a methanol reformer to complete the purification of hydrogen, thereby supplying hydrogen for fuel cells.
[0006] The ultra-light metal honeycomb monolithic catalyst and its preparation method and application of the present invention are realized by the following technical solutions:
[0007] The first object of the present invention is to provide a method for preparing an ultralight metal honeycomb monolithic catalyst, comprising the following steps:
[0008] Step 1: Preparation of high-activity catalyst powder:
[0009] 1) Using an oxide as a carrier and a noble metal salt solution as an impregnation solution, an impregnation method is adopted to load the noble metal in the noble metal salt solution on the surface of the oxide to obtain a catalyst raw powder precursor.
[0010] 2) Using the catalyst raw powder precursor as a carrier and a 3d transition metal salt solution as an impregnation solution, an impregnation method is adopted to load the 3d transition metal component in the 3d transition metal salt solution on the surface of the catalyst raw powder precursor to obtain a high-activity catalyst raw powder.
[0011] It should be noted that the present invention uses an oxide with a large specific surface area as a carrier to load the precious metal, which increases the dispersion of the precious metal and reduces the amount of the precious metal. On the basis of reducing the preparation cost, the carrier also achieves the anchoring effect on the active metal and prevents the aggregation of metal particles during service. In order to ensure that the above effects can be achieved, in some preferred embodiments of the present invention, the mass ratio of the precious metal salt in the precious metal salt solution to the oxide is 0.1% to 5%:1.
[0012] In order to ensure that the oxide used can achieve the above effects, in some preferred embodiments of the present invention, the oxide is one or more of aluminum oxide, silicon oxide, MCM molecular sieve, SBA molecular sieve and ZSM molecular sieve.
[0013] In some preferred embodiments of the present invention, the noble metal salt in the noble metal salt solution is one or more of Au salt, Pt salt, Pd salt, Ru and Rh salt. Wherein, when the noble metal salt used includes Au salt, in some preferred embodiments of the present invention, the Au salt used can be selected from one or both of chloroauric acid and gold nitrate. When the noble metal salt used includes Pt salt, in some preferred embodiments of the present invention, the Pt salt used can be selected from one or both of chloroplatinic acid, platinum nitrate and platinum sulfate. When the noble metal salt used includes Pd salt, in some preferred embodiments of the present invention, the Pd salt used can be selected from one or both of palladium nitrate, palladium chloride, palladium acetate, potassium palladate and ammonium palladate. When the noble metal salt used includes Ru salt, in some preferred embodiments of the present invention, the Ru salt used can be selected from one or both of ruthenium chloride, ruthenium nitrate and ruthenium acetate. When the noble metal salt used includes Rh salt, in some preferred embodiments of the present invention, the Rh salt used can be selected from one or both of rhodium chloride and rhodium nitrate.
[0014] The use of impregnation method to prepare catalysts is a commonly used method in this field, so those skilled in the art should know which preparation steps are specifically included. In order to ensure that the precious metal in the precious metal salt solution can be loaded on the surface of the oxide by impregnation method to obtain a catalyst powder precursor, in some preferred embodiments of the present invention, the catalyst powder precursor is prepared by the following steps: under stirring conditions, the oxide is added to the precious metal salt solution and mixed, so that the precious metal component is attached to the oxide carrier in the form of ions, and then aging, drying and roasting are performed in sequence to convert the precious metal component into a precious metal oxide and load it on the surface of the oxide carrier, that is, to obtain a catalyst powder precursor. Among them, in some preferred embodiments of the present invention, the concentration of the precious metal salt in the precious metal salt solution is 0.1g / L~100g / L. In some preferred embodiments of the present invention, the aging temperature is room temperature~90℃, and the aging time is 1h~12h. In some preferred embodiments of the present invention, the drying temperature is room temperature~120℃, and the drying time is 1h~24h. In some preferred embodiments of the present invention, the calcination temperature is 300° C. to 800° C., and the drying time is 1 h to 24 h. The present invention does not limit the specific particle size after grinding, as long as the calcined product can be ground into powder for subsequent further impregnation of 3d transition metals.
[0015] The present invention further introduces a 3d transition metal component on the basis of the catalyst powder precursor, so that a confinement effect is formed between the noble metal and the 3d transition metal. This confinement effect makes the 3d transition metal in a metastable state, which is more conducive to the activation of O2, thereby promoting the oxidation reaction of CO. In order to ensure that the above effects can be achieved in the future, in some preferred embodiments of the present invention, the mass ratio of the 3d transition metal salt in the 3d transition metal salt solution to the catalyst powder precursor is 0.01% to 1%:1.
[0016] In order to further promote the formation of a confined domain effect between the noble metal and the 3d transition metal, in some preferred embodiments of the present invention, the 3d transition metal salt in the 3d transition metal salt solution is one or more of an Fe salt, a Co salt and a Ni salt. Wherein, when the 3d transition metal salt used includes an Fe salt, in some preferred embodiments of the present invention, the Fe salt used can be selected from one or more of ferric nitrate, ferric chloride and ferric sulfate. When the 3d transition metal salt used includes a Co salt, in some preferred embodiments of the present invention, the Co salt used can be selected from one or more of cobalt nitrate, cobalt chloride and cobalt sulfate. When the 3d transition metal salt used includes a Ni salt, in some preferred embodiments of the present invention, the Ni salt used is selected from one or more of nickel nitrate, nickel chloride and nickel sulfate.
[0017] The preparation of catalysts by impregnation is a commonly used method in the art, so those skilled in the art should know the specific preparation steps involved. In order to ensure that the 3d transition metal salt in the 3d transition metal salt solution can be loaded on the surface of the catalyst raw powder precursor by the impregnation method to obtain a high-activity catalyst raw powder, in some preferred embodiments of the present invention, the high-activity catalyst raw powder is prepared by the following steps: under stirring conditions, the catalyst raw powder precursor is added to the 3d transition metal salt solution and mixed, so that the 3d transition metal component is attached to the catalyst raw powder precursor carrier in the form of ions, and then, aging, drying and calcining are performed in sequence to convert the 3d transition metal component into an unsaturated oxide form and load it on the surface of the catalyst raw powder precursor carrier, that is, to obtain a high-activity catalyst raw powder. Among them, in some preferred embodiments of the present invention, the concentration of the 3d transition metal salt in the 3d transition metal salt solution is 1g / L~20g / L. In some preferred embodiments of the present invention, the aging temperature is room temperature~90°C, and the aging time is 1h~12h. In some preferred embodiments of the present invention, the drying temperature is room temperature to 120°C, and the drying time is 1h to 24h. In some preferred embodiments of the present invention, in order to facilitate the subsequent formation of a high-activity catalytic slurry with uniform components, the calcined product is also ground, and the calcination temperature is 300°C to 800°C, and the drying time is 1h to 24h. The present invention does not limit the specific particle size after grinding, as long as the powdered high-activity catalyst raw powder can be obtained by grinding, so that the catalyst can be better dispersed in the slurry during the subsequent slurrying process.
[0018] Step 2: Preparation of high-activity catalytic slurry:
[0019] The high-activity catalyst raw powder and water are mixed evenly and then subjected to ball milling treatment to obtain a high-activity catalyst slurry.
[0020] It should be noted that, in order to ensure the catalytic performance of the high-activity catalytic slurry, in some preferred embodiments of the present invention, the high-activity catalyst raw powder accounts for 1% to 50% of the total mass of the high-activity catalytic slurry.
[0021] In order to improve the coating uniformity of the high-activity catalytic slurry and the bonding force with the substrate, in some preferred embodiments of the present invention, the high-activity catalytic slurry also includes other slurry components; and the other slurries include binders, dispersants, leveling agents and defoamers. Among them, in some preferred embodiments of the present invention, the binder accounts for 1% to 20% of the total mass of the high-activity catalytic slurry. In some preferred embodiments of the present invention, the dispersant accounts for 1% to 10% of the total mass of the high-activity catalytic slurry. In some preferred embodiments of the present invention, the leveling agent accounts for 1% to 10% of the total mass of the high-activity catalytic slurry. In some preferred embodiments of the present invention, the defoamer accounts for 0.1% to 10% of the total mass of the high-activity catalytic slurry.
[0022] In some preferred embodiments of the present invention, the binder is one or more of silica sol, aluminum sol, zirconium sol, polyethylene glycol and methyl cellulose. Among them, when the binder used includes silica sol or aluminum sol or zirconium sol, silica sol, aluminum sol and zirconium sol are all inorganic binders. After high-temperature calcination, inorganic substances remain around the catalyst, which can prevent the catalyst from sintering. At the same time, it can withstand high temperatures and fix the catalyst on the surface of the metal carrier. When the binder used includes polyethylene glycol or methyl cellulose, polyethylene glycol and methyl cellulose are organic binders. There is no residue after high-temperature calcination, but it is beneficial to the dispersion of the catalyst during the pulping process and to the film formation of the coating during the coating process.
[0023] In some preferred embodiments of the present invention, the dispersant is one or more of sodium tripolyphosphate, sodium hexametaphosphate, polyacrylamide and polyvinyl alcohol, so that the dispersant helps the catalyst powder to be dispersed in the sol containing the additive without sedimentation.
[0024] In some preferred embodiments of the present invention, the leveling agent is an organic silicon leveling agent, so as to reduce the surface energy between the coating and the metal substrate, increase the fluidity of the slurry, and facilitate coating and film formation. In some preferred embodiments of the present invention, the organic silicon leveling agent includes but is not limited to one or both of German BYK-333 and BYK-346.
[0025] In some preferred embodiments of the present invention, the defoaming agent is one or more of a silicone defoaming agent and an alcohol defoaming agent, so that the defoaming agent can eliminate bubbles generated by stirring the slurry, and the coating of the slurry will be smoother after the bubbles are eliminated.
[0026] In some preferred embodiments of the present invention, the ball milling treatment is a combination of forward and reverse milling, wherein forward rotation is 5min to 30min, stop for 1min to 10min, reverse for 5min to 30min, and the cycle is repeated multiple times. The rotation speed is 500rpm to 10000rpm, and the total ball milling time is 1h to 24h.
[0027] Step 3: Coating of high-activity catalytic slurry:
[0028] A metal foil is used as a substrate, and its surface is pretreated by roasting to obtain a metal substrate; the high-activity catalytic slurry is coated on the surface of the metal substrate, and a high-activity catalyst coating is formed on the surface of the metal substrate after curing to obtain a flat modified metal substrate, referred to as a flat plate. In some preferred embodiments of the present invention, the curing is carried out by drying first and then rolling. The drying can be carried out by oven drying or microwave drying. When drying is carried out by oven drying, it can be dried in an oven at 50°C to 100°C for 0.5h to 6h. When drying is carried out by microwave drying, the drying temperature and time are not specifically limited, and the liquid water can be evaporated.
[0029] It should be noted that the present invention does not specifically limit the type of metal foil, and the type can be selected according to the time requirement, for example, any one of iron-based foil, titanium-based foil, aluminum-based foil and nickel-based foil can be selected. In some preferred embodiments of the present invention, the iron-based foil can be selected from any one of stainless steel and iron-chromium-aluminum. In some preferred embodiments of the present invention, the titanium-based foil can be selected from any one of TC4 and TA2.
[0030] In some preferred embodiments of the present invention, the present invention takes into account that the thinner the metal foil is, the larger the open porosity of the honeycomb after being rolled into a honeycomb, the larger the surface area, the greater the loading amount of the catalyst, and the higher the catalytic efficiency; however, the thinner the metal foil is, the more difficult it is to prepare, and the thinner the foil is, the easier it is to wrinkle and cannot maintain a flat state. In order to achieve high catalytic efficiency of flat metal foil, the present invention uses a metal foil with a thickness of 20μm to 100μm.
[0031] The present invention has been found in the process of exploration that when the high-activity catalytic slurry is directly applied to the surface of the metal foil, the metal foil surface is smooth, and the material of the metal foil is very different from the properties of the active components in the high-activity catalytic slurry, resulting in poor bonding between the metal foil and the high-activity catalytic slurry. The formed coating is prone to peeling at the interface, resulting in gaps, causing the coating to fall off. Therefore, in order to further improve the bonding force between the metal foil and the high-activity catalytic slurry, in some preferred embodiments of the present invention, before applying the high-activity catalytic slurry, the metal foil is first calcined to convert the metal on the surface of the metal foil into metal oxide particles through the calcination process, so that the main components of the metal foil surface and the high-activity catalytic slurry are both oxides, and the properties of the two are similar or close, which helps to firmly bond the high-activity catalytic slurry to the substrate. For example, in some preferred embodiments of the present invention, when stainless steel with components of Fe, Cr and Ni is used as the metal foil material, mixed oxide particles of Fe2O3, Cr2O3 and NiO will be formed on the surface of the stainless steel during the calcination process, which are consistent with the properties of the catalyst which is also an oxide, so it helps to firmly bond the catalyst to the substrate.
[0032] During the research process, the present invention found that the calcination temperature of the calcination treatment will affect the surface properties of the metal foil. When the calcination temperature is lower than 500°C, it is difficult to completely oxidize the metal on the surface of the metal foil, that is, the oxide formed on the surface of the metal foil is not obvious, and it is difficult to effectively improve the bonding force between the catalyst coating and the substrate. When the calcination temperature is too high, the size of the oxide particles formed will be too large, which will affect the uniform coating effect of the high-activity catalytic slurry, and further affect the overall performance of the final catalyst. Therefore, in some preferred embodiments of the present invention, the calcination temperature is 500°C to 1000°C, so that the particle size of the oxide formed on the surface of the metal foil at this temperature is close to the size of the high-activity catalytic slurry, which is conducive to improving the bonding effect between the two. In another preferred embodiment of the present invention, the calcination time is 1h to 24h.
[0033] In order to further improve the bonding strength between the substrate and the high-activity catalytic slurry, in some preferred embodiments of the present invention, the metal foil is cleaned before being calcined, and the cleaning solvent is one or both of ethanol and acetone to remove impurities on the surface of the metal foil.
[0034] In order to avoid cracking and falling off during the coating drying process, in some preferred embodiments of the present invention, the coating thickness of the high-activity catalytic slurry is 1μm to 100μm, so as to ensure that the high-activity catalytic slurry can be evenly coated on the surface of the metal substrate, thereby achieving a high-strength bond with the metal substrate, effectively preventing cracking and falling off during the subsequent coating drying process.
[0035] The present invention does not limit the specific coating method, as long as the high-activity catalytic slurry can be evenly coated on the surface of the metal substrate, for example, any one of blade coating, ultrasonic spray coating and immersion coating can be selected.
[0036] Step 4: Forming of the monolithic catalyst:
[0037] 1) A piece of the modified metal substrate is pressed into a corrugated shape, and is placed on top of another piece of the modified metal substrate which remains in a flat shape for stacking, and then rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0038] 2) The honeycomb monolithic catalyst precursor is subjected to calcination treatment and reduction treatment in sequence to obtain an ultra-light metal honeycomb monolithic catalyst.
[0039] It should be noted that the present invention takes into account that the traditional granular catalyst has a large filling pressure drop and is not suitable for large-flow gas-phase reactions. In addition, although the traditional ceramic honeycomb catalyst has large pores, the thinnest honeycomb wall thickness is 1 mm, and the opening rate is not high. Therefore, the present invention presses a modified metal substrate with a high-activity catalyst coating on the surface of a flat plate into a corrugated shape, that is, presses a flat plate into a corrugated shape to obtain a corrugated plate, and then places the obtained corrugated plate on top of another flat plate that has not been pressed, and then fills it into a rolling welding machine and rolls it into a honeycomb shape. The preparation principle is as follows: Figure 1 As shown, a honeycomb monolithic catalyst precursor is obtained.
[0040] In some preferred embodiments of the present invention, when the honeycomb monolithic catalyst precursor is calcined, the calcination temperature is 300° C. to 800° C. In some other preferred embodiments of the present invention, the calcination time is 1 hour to 24 hours.
[0041] The present invention takes into account that in the honeycomb monolithic catalyst precursor after the calcination treatment, the precious metal component and the 3d transition metal component mainly exist in the form of precious metal oxides and 3d transition metal oxides, while the completely oxidized precious metals and 3d transition metals are inactive. Therefore, the present invention also performs a reduction treatment on the honeycomb monolithic catalyst precursor after the calcination treatment, so as to reduce the precious metal oxides to precious metals through the reduction treatment, and at the same time ensure that the 3d transition metal oxides are in a non-completely oxidized state, thereby ensuring that the metallic precious metals and the non-completely oxidized 3d transition metals are the active sites of the catalyst, the former adsorbs and activates CO, and the latter adsorbs and activates O2, and the activated CO combines with the activated O2 to form CO2 to complete the reaction. In order to ensure that the above-mentioned effect can be achieved through the reduction treatment, in some preferred embodiments of the present invention, the reducing atmosphere of the reduction treatment is hydrogen or a mixture of hydrogen and inert gas, and the reduction temperature is 300°C to 600°C.
[0042] The second object of the present invention is to provide an ultralight metal honeycomb monolithic catalyst prepared by the above preparation method. Figure 2 shown.
[0043] The second object of the present invention is to provide an application of the above-mentioned ultra-light metal honeycomb monolithic catalyst in purifying the hydrogen production product of methanol reforming.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The present invention uses oxide as a carrier, noble metal salt solution as an impregnation liquid, and adopts an impregnation method to load the noble metal component in the noble metal salt solution on the oxide surface in the form of noble metal oxide to obtain a catalyst original powder precursor. Among them, the oxide has an ultra-large specific surface area that can increase the dispersion of the noble metal and reduce the amount of the noble metal, so as to reduce the preparation cost and also realize the anchoring effect of the carrier on the active metal, thereby preventing the aggregation of metal particles during the service process. Then, the catalyst original powder precursor is used as a carrier, and the 3d transition metal salt solution is used as an impregnation liquid. The impregnation method is adopted to make the 3d transition metal component in the 3d transition metal salt solution finally loaded on the catalyst original powder precursor surface in the form of an unsaturated oxide, so as to further introduce the 3d transition metal component on the basis of the noble metal component, so as to form a confined effect between the noble metal and the 3d transition metal, and this confined effect makes the 3d transition metal in a metastable state, which is more conducive to the activation of O2, thereby promoting the oxidation reaction of CO, and improving the catalytic activity of the catalyst original powder on the basis of improving the stability of the catalyst original powder component. The obtained high-activity catalyst raw powder and water are then ball-milled to fully and evenly disperse the high-activity catalyst raw powder to form a high-activity catalytic slurry with uniform components, so as to improve the subsequent uniform coating on the substrate material, thereby avoiding to a certain extent the occurrence of coating cracking and low catalytic activity caused by uneven coating of the high-activity catalyst slurry.
[0046] The present invention uses an ultra-thin metal foil as a substrate to reduce the overall mass of the catalyst, and then coats the ultra-thin metal foil with a high-activity catalytic slurry after calcining, so that the metal on the surface of the metal foil is converted into metal oxide particles through the calcining treatment, so that the main components of the metal foil surface and the high-activity catalytic slurry are both oxides, that is, the properties of the metal foil surface material and the main components of the high-activity catalytic slurry are similar or close, and the metal foil surface and the main components of the high-activity catalytic slurry are easily combined, thereby achieving a firm combination between the substrate and the high-activity catalytic slurry, so as to avoid the formed coating from being easily peeled off at the interface, resulting in gaps and causing the coating to fall off.
[0047] The present invention takes a piece of modified metal substrate and presses it into a corrugated shape, and places it on top of another piece of modified metal substrate that remains in a flat plate shape for superposition, and then rolls it into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor, so as to increase the opening rate of the monolithic catalyst, increase the effective contact surface area of the monolithic catalyst, and thus increase the catalytic activity of the monolithic catalyst, which is suitable for large-flow gas-phase reactions. Then, by sequentially performing calcination treatment and reduction treatment, the catalyst forms a monolithic structure, and the active sites in the monolithic catalyst are metallic noble metals and non-completely oxidized 3d transition metals, the former adsorbs and activates CO, and the latter adsorbs and activates O2, and the activated CO combines with the activated O2 to form CO2, completing the reaction.
[0048] The preparation method of the present invention is simple to operate, and the coating and the metal substrate are firmly bonded in the prepared ultralight metal honeycomb monolithic catalyst, which has small mass, high open porosity, good activity and high mechanical strength. When the ultralight metal honeycomb monolithic catalyst prepared by the present invention is applied to the removal of CO in a hydrogen-rich atmosphere containing a small amount of CO and a large amount of H2O and CO2, CO can be basically completely removed at a low temperature of 80°C, and can be filled in a methanol reformer to complete the purification of hydrogen, thereby supplying hydrogen to a fuel cell.
[0049] The high-activity catalytic slurry of the present invention also includes other slurry components to further increase the uniformity of slurry coating. The uniform coating of the high-activity catalytic slurry and its high-strength bonding with the substrate effectively prevent cracking and shedding during the subsequent coating drying process.
[0050] The present invention uses ultra-thin metal foil as a matrix to prepare an integral catalyst. The obtained honeycomb catalyst has a wall thickness of ≤100μm, a high porosity, operates at high air velocity, and has a small pressure drop. The catalyst is applied to the removal reaction of trace amounts of CO in a hydrogen-rich atmosphere. The catalyst has a CO removal temperature as low as 80°C and has excellent water resistance and CO2 resistance. As is known to all, the operating temperature of a hydrogen fuel cell is 80°C. If high-temperature hydrogen obtained by reforming is used, the hydrogen needs to be cooled because the purification temperature is generally lower than the reforming temperature. If the purification temperature is higher than 80°C, the purified hydrogen needs to be cooled again. In the present invention, the catalyst purifies hydrogen at a temperature as low as 80°C, so the purified hydrogen can be directly introduced into the fuel cell without any heat exchange, which can greatly reduce the complexity of the methanol reforming hydrogen production and fuel cell system. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a schematic diagram of the principle of forming a honeycomb monolithic catalyst precursor according to the present invention.
[0052] Figure 2 This is a schematic structural diagram of the ultralight metal honeycomb monolithic catalyst prepared by the present invention.
[0053] Figure 3 This is a SEM image of the coating on the surface of the ultra-light metal honeycomb monolithic catalyst of Example 1 at a scale of 50 μm.
[0054] Figure 4 This is a SEM image of the coating on the surface of the ultra-light metal honeycomb monolithic catalyst of Example 1 at a scale of 500 nm.
[0055] Figure 5 This is a SEM image of the cross section of the ultra-light metal honeycomb monolithic catalyst surface coating of Example 1.
[0056] Figure 6 The reaction performance test results of the ultralight metal honeycomb monolithic catalyst of Example 1 are shown. DETAILED DESCRIPTION
[0057] The technical solutions in the embodiments of the present invention will be described clearly and completely below. It should be noted that in the following embodiments of the present invention, the seam welding machine used is a special straight seam seam welding machine, which is manufactured by PANASONIC Panasonic, model GH-0018, and the relevant working parameters are: the current is direct current, the driving mode is automatic, the welding mode is continuous welding, and the welding pressure is 4MPa.
[0058] Example 1
[0059] This embodiment provides an ultra-light metal honeycomb monolithic catalyst, which is prepared by the following steps:
[0060] Step 1: Preparation of high-activity catalyst powder:
[0061] 1) Dissolve 26 g of chloroplatinic acid in 5 L of ultrapure water to obtain a noble metal salt solution. Add 1 kg of alumina powder to the obtained noble metal salt solution under stirring and mix well, then age at room temperature for 12 h, filter to obtain a solid component, dry the obtained solid component at 100° C. for 8 h, and then calcine in a muffle furnace at 500° C. for 5 h to obtain a catalyst raw powder precursor.
[0062] 2) Dissolve 72g of ferric nitrate in 5L of ultrapure water to obtain a 3d transition metal salt solution. Add the above catalyst powder precursor to the 3d transition metal salt solution under stirring, mix well, age for 12h under stirring at room temperature, filter to obtain a solid component, dry the obtained solid component at 100°C for 8h, and then calcine in a muffle furnace at 500°C for 5h to obtain a high-activity catalyst powder.
[0063] Step 2: Preparation of high-activity catalytic slurry:
[0064] The high-activity catalyst powder, silica sol, sodium tripolyphosphate, BYK-333, n-hexanol and ultrapure water obtained above were added into a ball mill in a mass ratio of 3:2:1:1:1:2. The ball mill was set to rotate forward and reverse for 30 minutes, reverse for 30 minutes, stop for 5 minutes, and the speed was 1000 rpm for 5 hours to obtain a high-activity catalytic slurry.
[0065] Step 3: Coating of high-activity catalytic slurry:
[0066] 1) A stainless steel foil with a length of 100 cm, a width of 10 cm, and a thickness of 30 μm was used as a substrate, which was immersed in ethanol for cleaning, placed in a muffle furnace, and calcined at 1000° C. for 2 h to obtain a metal substrate.
[0067] 2) Using a scraper coater, the high-activity catalytic slurry obtained in the above step 2 is coated on a metal substrate with a coating thickness of 10 μm. After the coating is dried, it is compacted with a roller press to obtain a flat modified metal substrate.
[0068] Step 4: Forming of the monolithic catalyst:
[0069] 1) Please refer to Figure 1 The modified metal substrate obtained above is cut into two plates of the same size according to actual needs, one of which is pressed into a corrugated shape, and the other remains in its original flat shape. The corrugated sheet and the flat sheet are stacked up and filled into a rolling welding machine and rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0070] 2) The honeycomb monolithic catalyst precursor obtained above was calcined at 500°C for 5 hours, and then reduced at 300°C for 5 hours in a pure hydrogen atmosphere to obtain an ultra-light metal honeycomb monolithic catalyst having a structure as shown in Figure 2 shown.
[0071] Example 2
[0072] This embodiment provides an ultra-light metal honeycomb monolithic catalyst, which is prepared by the following steps:
[0073] Step 1: Preparation of high-activity catalyst powder:
[0074] 1) Dissolve 40 g of chloroauric acid in 5 L of ultrapure water to obtain a noble metal salt solution. Under stirring conditions, add 1 kg of MCM-41 molecular sieve powder to the obtained noble metal salt solution and mix well, then age at 80° C. for 12 h, filter to obtain a solid component, dry the obtained solid component at 100° C. for 8 h, and then calcine at 500° C. in a muffle furnace for 5 h to obtain a catalyst raw powder precursor.
[0075] 2) Dissolve 50g of cobalt nitrate in 5L of ultrapure water to obtain a 3d transition metal salt solution. Add the above catalyst powder precursor to the 3d transition metal salt solution under stirring, age at 80°C for 12h, filter to obtain a solid component, dry the obtained solid component at 100°C for 8h, and then calcine at 500°C in a muffle furnace for 5h to obtain a high-activity catalyst powder.
[0076] Step 2: Preparation of high-activity catalytic slurry:
[0077] The high-activity catalyst powder, silica sol, sodium tripolyphosphate, BYK-333, n-hexanol and ultrapure water obtained above were added into a ball mill in a mass ratio of 3:2:1:1:1:2. The ball mill was set to rotate forward and reverse for 30 minutes, reverse for 30 minutes, stop for 5 minutes, and the speed was 1000 rpm for 5 hours to obtain a high-activity catalytic slurry.
[0078] Step 3: Coating of high-activity catalytic slurry:
[0079] 1) A stainless steel foil with a length of 100 cm, a width of 10 cm, and a thickness of 30 μm was used as a substrate, which was immersed in ethanol for cleaning, placed in a muffle furnace, and calcined at 1000° C. for 2 h to obtain a metal substrate.
[0080] 2) Using a scraper coater, the high-activity catalytic slurry obtained in the above step 2 is coated on a metal substrate with a coating thickness of 10 μm. After the coating is dried, it is compacted with a roller press to obtain a flat modified metal substrate.
[0081] Step 4: Forming of the monolithic catalyst:
[0082] 1) The modified metal substrate obtained above is cut into two plates of the same size according to actual needs, one of which is pressed into a corrugated shape, and the other is kept in its original flat shape, and the corrugated sheet and the flat sheet are stacked up and down and filled into a roll welding machine and rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0083] 2) The honeycomb monolithic catalyst precursor obtained above was calcined at 500° C. for 5 h, and then reduced at 300° C. for 5 h in a pure hydrogen atmosphere to obtain an ultra-light metal honeycomb monolithic catalyst.
[0084] Example 3
[0085] This embodiment provides an ultra-light metal honeycomb monolithic catalyst, which is prepared by the following steps:
[0086] Step 1: Preparation of high-activity catalyst powder:
[0087] 1) Dissolve 26 g of chloroplatinic acid in 5 L of ultrapure water to obtain a noble metal salt solution. Add 1 kg of alumina powder to the obtained noble metal salt solution under stirring and mix well, then age at 50° C. for 12 h, filter to obtain a solid component, dry the obtained solid component at 100° C. for 8 h, and then calcine at 500° C. for 5 h in a muffle furnace to obtain a catalyst raw powder precursor.
[0088] 2) Dissolve 72g of ferric nitrate in 5L of ultrapure water to obtain a 3d transition metal salt solution. Add the above catalyst powder precursor to the 3d transition metal salt solution under stirring, age at 50°C for 12h, filter to obtain a solid component, dry the obtained solid component at 100°C for 8h, and then calcine at 500°C in a muffle furnace for 5h to obtain a high-activity catalyst powder.
[0089] Step 2: Preparation of high-activity catalytic slurry:
[0090] The high-activity catalyst powder, polyethylene glycol, polyvinyl alcohol, BYK-346, n-hexanol and ultrapure water obtained above were added into a ball mill in a mass ratio of 4:1:1:1:1:2. The ball mill was set to rotate forward and reverse for 30 minutes, reverse for 30 minutes, stop for 5 minutes, and the speed was 1000 rpm for 5 hours to obtain a high-activity catalytic slurry.
[0091] Step 3: Coating of high-activity catalytic slurry:
[0092] 1) A stainless steel foil with a length of 100 cm, a width of 10 cm, and a thickness of 30 μm was used as a substrate, which was immersed in ethanol for cleaning, placed in a muffle furnace, and calcined at 1000° C. for 2 h to obtain a metal substrate.
[0093] 2) Using a scraper coater, the high-activity catalytic slurry obtained in the above step 2 is coated on a metal substrate with a coating thickness of 10 μm. After the coating is dried, it is compacted with a roller press to obtain a flat modified metal substrate.
[0094] Step 4: Forming of the monolithic catalyst:
[0095] 1) The modified metal substrate obtained above is cut into two plates of the same size according to actual needs, one of which is pressed into a corrugated shape, and the other is kept in its original flat shape, and the corrugated sheet and the flat sheet are stacked up and down and filled into a roll welding machine and rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0096] 2) The honeycomb monolithic catalyst precursor obtained above was calcined at 500° C. for 5 h, and then reduced at 300° C. for 5 h in a pure hydrogen atmosphere to obtain an ultra-light metal honeycomb monolithic catalyst.
[0097] Example 4
[0098] This embodiment provides an ultra-light metal honeycomb monolithic catalyst, which is prepared by the following steps:
[0099] Step 1: Preparation of high-activity catalyst powder:
[0100] 1) Dissolve 26 g of chloroplatinic acid in 5 L of ultrapure water to obtain a noble metal salt solution. Add 1 kg of alumina powder to the obtained noble metal salt solution under stirring and mix well, then age at room temperature for 12 h, filter to obtain a solid component, dry the obtained solid component at 100° C. for 8 h, and then calcine in a muffle furnace at 500° C. for 5 h to obtain a catalyst raw powder precursor.
[0101] 2) Dissolve 72g of ferric nitrate in 5L of ultrapure water to obtain a 3d transition metal salt solution. Add the above catalyst powder precursor to the 3d transition metal salt solution under stirring, mix well, age for 12h under stirring at room temperature, filter to obtain a solid component, dry the obtained solid component at 100°C for 8h, and then calcine in a muffle furnace at 500°C for 5h to obtain a high-activity catalyst powder.
[0102] Step 2: Preparation of high-activity catalytic slurry:
[0103] The high-activity catalyst powder, silica sol, sodium tripolyphosphate, BYK-333, n-hexanol and ultrapure water obtained above were added into a ball mill in a mass ratio of 3:2:1:1:1:2. The ball mill was set to rotate forward and reverse for 30 minutes, reverse for 30 minutes, stop for 5 minutes, and the speed was 1000 rpm for 5 hours to obtain a high-activity catalytic slurry.
[0104] Step 3: Coating of high-activity catalytic slurry:
[0105] 1) A stainless steel foil with a length of 200 cm, a width of 10 cm, and a thickness of 50 μm was used as a substrate, which was immersed in ethanol for cleaning, placed in a muffle furnace, and calcined at 1000° C. for 2 h to obtain a metal substrate.
[0106] 2) Using a scraper coater, the high-activity catalytic slurry obtained in the above step 2 is coated on a metal substrate with a coating thickness of 20 μm. After the coating is dried, it is compacted with a roller press to obtain a flat modified metal substrate.
[0107] Step 4: Forming of the monolithic catalyst:
[0108] 1) The modified metal substrate obtained above is cut into two plates of the same size according to actual needs, one of which is pressed into a corrugated shape, and the other is kept in its original flat shape, and the corrugated sheet and the flat sheet are stacked up and down and filled into a roll welding machine and rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0109] 2) The honeycomb monolithic catalyst precursor obtained above was calcined at 500° C. for 5 h, and then reduced at 300° C. for 5 h in a pure hydrogen atmosphere to obtain an ultra-light metal honeycomb monolithic catalyst.
[0110] Example 5
[0111] This embodiment provides an ultra-light metal honeycomb monolithic catalyst, which is prepared by the following steps:
[0112] Step 1: Preparation of high-activity catalyst powder:
[0113] 1) Dissolve 150 g of palladium nitrate in 2 L of ultrapure water to obtain a noble metal salt solution. Add 1 kg of silicon oxide powder to the obtained noble metal salt solution under stirring, and then age at room temperature for 10 h, filter to obtain a solid component, dry the obtained solid component at 80° C. for 12 h, and then calcine at 500° C. in a muffle furnace for 5 h to obtain a catalyst raw powder precursor.
[0114] 2) Dissolve 15g of nickel nitrate in 2L of ultrapure water to obtain a 3d transition metal salt solution. Add the above catalyst powder precursor to the 3d transition metal salt solution under stirring, mix well, age at room temperature for 12h, filter to obtain a solid component, dry the obtained solid component at 80°C for 8h, and then calcine at 600°C in a muffle furnace for 5h to obtain a high-activity catalyst powder.
[0115] Step 2: Preparation of high-activity catalytic slurry:
[0116] The high-activity catalyst powder, methyl cellulose, polyacrylamide, BYK-346, n-hexanol and ultrapure water obtained above were added into a ball mill in a mass ratio of 5:1:1:1:1:1. The ball mill was set to rotate forward and reverse for 10 min, reverse for 10 min, stop for 1 min, and the speed was 500 rpm for 3 h to obtain a high-activity catalytic slurry.
[0117] Step 3: Coating of high-activity catalytic slurry:
[0118] 1) A stainless steel foil with a length of 200 cm, a width of 10 cm, and a thickness of 50 μm was used as a substrate, which was immersed in ethanol for cleaning, placed in a muffle furnace, and calcined at 1000° C. for 2 h to obtain a metal substrate.
[0119] 2) Using a scraper coater, the high-activity catalytic slurry obtained in the above step 2 is coated on a metal substrate with a coating thickness of 10 μm. After the coating is dried, it is compacted with a roller press to obtain a flat modified metal substrate.
[0120] Step 4: Forming of the monolithic catalyst:
[0121] 1) The modified metal substrate obtained above is cut into two plates of the same size according to actual needs, one of which is pressed into a corrugated shape, and the other is kept in its original flat shape, and the corrugated sheet and the flat sheet are stacked up and down and filled into a roll welding machine and rolled into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor.
[0122] 2) The honeycomb monolithic catalyst precursor obtained above was calcined at 500° C. for 5 h, and then reduced at 500° C. for 5 h in a pure hydrogen atmosphere to obtain an ultra-light metal honeycomb monolithic catalyst.
[0123] Experimental Section
[0124] (I) Scanning electron microscope test
[0125] The present invention takes the ultra-light metal honeycomb monolithic catalyst of Example 1 as an example, and performs an electron scanning electron microscope test on the coating on its surface, and the test results are as follows: Figure 3-Figure 5 shown.
[0126] Figure 3 This is a SEM image of the coating on the surface of the ultralight metal honeycomb monolithic catalyst of Example 1 at a scale of 50 μm. It can be seen that the surface coating of the ultralight metal honeycomb monolithic catalyst of Example 1 is uniform without any cracks.
[0127] Figure 4 This is an SEM image of the coating on the surface of the ultra-light metal honeycomb monolithic catalyst of Example 1 at a scale of 500nm. It can be seen that there are nano-scale catalyst particles in the coating on the surface of the ultra-light metal honeycomb monolithic catalyst, indicating that in the ultra-light metal honeycomb monolithic catalyst prepared by the present invention, the catalyst particles in the coating are well dispersed, no agglomeration occurs, the coating has good uniformity, and the prepared monolithic catalyst has high activity.
[0128] Figure 5 This is a cross section of the ultralight metal honeycomb monolithic catalyst coating in Example 1. It can be seen that the coating thickness on the surface of the ultralight metal honeycomb monolithic catalyst in Example 1 is about 3 μm, and the coating is firmly bonded to the metal substrate without cracks.
[0129] (II) Catalyst reaction performance test
[0130] The present invention takes the ultra-light metal honeycomb monolithic catalyst of Example 1 as an example, and conducts an electronic catalyst reaction performance test on it, and the test results are as follows: Figure 6 shown.
[0131] Test method:
[0132] The reaction performance of the ultralight metal honeycomb monolithic catalyst was evaluated in a large flow fixed bed reactor. The catalyst was filled in a quartz reaction tube, and a hydrogen-rich raw gas containing CO, CO2, and H2O was introduced. The composition of the raw gas was 60vol.%H2 / 20vol.%H2O / 15vol.%CO2 / 0.7vol.%CO / 1.4vol.%O2 / N2, the flow rate was 20L / min, the pressure was atmospheric pressure, the test temperature was 70℃~200℃, and the volume space velocity was 60000h -1 .
[0133] Depend on Figure 6 It can be seen from the test results that after being treated with the ultralight metal honeycomb monolithic catalyst of Example 1, the concentration of CO can be removed to below 10ppm between 80℃ and 150℃. It shows that the coating on the surface of the ultralight metal honeycomb monolithic catalyst prepared by the present invention is evenly coated, there is no cracking phenomenon in the coating, and the activity is high. It can be applied to a variety of catalytic reactions, especially to the preferential oxidation reaction of CO in a hydrogen-rich atmosphere. Under harsh conditions containing CO2 and H2O, even if the operating temperature is as low as 80℃, the catalyst can still basically completely remove CO. The catalyst is filled in a methanol reformer to achieve deep purification of hydrogen, thereby supplying hydrogen for hydrogen fuel cells.
[0134] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing an ultra-light metal honeycomb monolithic catalyst, It is characterized in that The following steps are involved: Using an oxide as a carrier and a noble metal salt solution as an impregnation liquid, an impregnation method is used to load the noble metal in the noble metal salt solution on the surface of the oxide to obtain a catalyst raw powder precursor; using the catalyst raw powder precursor as a carrier and a 3d transition metal salt solution as an impregnation liquid, an impregnation method is used to load the 3d transition metal component in the 3d transition metal salt solution on the surface of the catalyst raw powder precursor to obtain a high-activity catalyst raw powder; The high-activity catalyst raw powder and water are mixed and then subjected to ball milling to obtain a high-activity catalyst slurry; Using a metal foil as a substrate, pre-treating its surface by calcining to obtain a metal substrate; The highly active catalytic slurry is applied to the surface of the metal substrate, and after curing, a highly active catalyst coating is formed on the surface of the metal substrate to obtain a flat modified metal substrate; Taking a piece of the modified metal substrate and pressing it into a corrugated shape, placing it on top of another piece of the modified metal substrate that remains in a flat shape to overlap, and then rolling it into a honeycomb shape to obtain a honeycomb monolithic catalyst precursor; The honeycomb monolithic catalyst precursor is subjected to calcination treatment and reduction treatment in sequence to obtain an ultra-light metal honeycomb monolithic catalyst.
2. The preparation method according to claim 1, It is characterized in that The mass ratio of the noble metal salt in the noble metal salt solution to the oxide is 0.1% to 5%:1; The oxide is one or more of aluminum oxide, silicon oxide, MCM molecular sieve, SBA molecular sieve and ZSM molecular sieve.
3. The preparation method according to claim 1, It is characterized in that The 3d transition metal salt in the 3d transition metal salt solution is one or more of Fe salt, Co salt and Ni salt; The mass ratio of the 3d transition metal salt in the 3d transition metal salt solution to the catalyst raw powder precursor is 0.01% to 1%:
1.
4. The preparation method according to claim 1, It is characterized in that When the metal foil is calcined, the calcination temperature is 500° C. to 1000° C.; When the honeycomb monolithic catalyst precursor is subjected to calcination treatment, the calcination temperature is 300°C to 800°C.
5. The preparation method according to claim 1, It is characterized in that The reducing atmosphere of the reduction treatment is hydrogen or a mixture of hydrogen and inert gas, and the reducing temperature is 300°C-600°C.
6. The preparation method according to claim 1, It is characterized in that The high-activity catalyst raw powder accounts for 1% to 50% of the total mass of the high-activity catalytic slurry; The coating thickness of the high-activity catalytic slurry is 1 μm to 100 μm.
7. The preparation method according to claim 1, It is characterized in that The metal foil is any one of an iron-based foil, a titanium-based foil, an aluminum-based foil and a nickel-based foil; The thickness of the metal foil is 20 μm to 100 μm.
8. The preparation method according to claim 1, It is characterized in that The high-activity catalytic slurry also includes other slurry components; The other slurry includes a binder, a dispersant, a leveling agent and a defoamer; Wherein, the binder accounts for 1% to 20% of the total mass of the high-activity catalytic slurry; The dispersant accounts for 1% to 10% of the total mass of the high-activity catalytic slurry; The leveling agent accounts for 1% to 10% of the total mass of the high-activity catalytic slurry; The defoamer accounts for 0.1% to 10% of the total mass of the high-activity catalytic slurry.
9. An ultralight metal honeycomb monolithic catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the ultralight metal honeycomb monolithic catalyst according to claim 9 in purifying hydrogen production products from methanol reforming.
